Low-filled automotive polypropylene compositions containing recycled content

By blending polypropylene-polyethylene blends and inorganic fillers, the mechanical properties and odor problems of recycled materials in the motor vehicle industry are solved, and the large-scale replacement and performance improvement of polypropylene-polyethylene blends are achieved, which is suitable for Motor vehicle applications.

CN116113666BActive Publication Date: 2024-10-22北欧化工公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180055932.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-13
Filing Date
2021-08-11
Publication Date
2024-10-22
Estimated Expiration
2041-08-11

AI Technical Summary

Technical Problem

Polyolefin materials recycled from the automotive industry are difficult to use widely in applications due to limited mechanical properties, odor and emission issues, and complex heterophasic polypropylene copolymers are difficult to replace, limiting the reuse of recycled materials.

Method used

By blending polypropylene-polyethylene blends instead of complex heterophasic polypropylene copolymers, combined with inorganic fillers such as talc, the melt flow rate and intrinsic viscosity of the composition are optimized, tiger stripe performance and VOC characteristics are improved, and anisotropy is maintained .

Benefits of technology

It realizes the large-scale replacement of recycled polypropylene-polyethylene blends in motor vehicle applications, improves tiger stripe performance and VOC characteristics, maintains anisotropy, and improves the applicability of recyclates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004113297290000191
    Figure BDA0004113297290000191
  • Figure BDA0004113297290000201
    Figure BDA0004113297290000201
  • Figure BDA0004113297290000202
    Figure BDA0004113297290000202
Patent Text Reader

Abstract

A composition suitable for automotive applications, said composition being obtainable by blending at least components a) to f), or by blending at least components a), b), c), d) and f) in the absence of e): a) 12 to 40 wt%, preferably 14 to 38 wt%, more preferably 15 to 35 wt% of a first heterophasic polypropylene copolymer (HECO1); b) 12 to 40 wt%, preferably 14 to 38 wt%, more preferably 15 to 35 wt% of a second heterophasic polypropylene copolymer (HECO 2); c) 15 to 65 wt%, preferably 18 to 60 wt%, more preferably 20 to 55 wt% of a polypropylene-polyethylene blend (A); d) 3.0 to 20 wt%, preferably 5.0 to 15 wt%, more preferably 6.0 to 15 wt% of an inorganic filler; e) 0 to 15 wt% of HDPE; f) 0.01 to 4.0 wt% of an additive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to polypropylene-based compositions containing inorganic fillers and recyclates suitable for use in the automotive industry. Background Art

[0002] Compositions suitable for use in the automotive industry usually comprise one or more heterophasic polypropylene copolymers and / or random heterophasic copolymers and conventionally some inorganic fillers.

[0003] One of the fundamental problems in the polymer industry is recycling. Currently, the market for recyclates, especially those from household waste, usually denoted PCR ("post-consumer resin"), is somewhat limited. Starting from household waste, the sorting and separation processes employed do not allow the manufacture of pure polymers, i.e., there are always some contaminants, or the process may even result in a blend of different polymers. When it comes to polyolefins, which account for the vast majority of the polymer portion of the collected household waste, a perfect separation of polypropylene and polyethylene is almost impossible. Recycled polyolefin materials, especially post-consumer resins, are often cross-contaminated by non-polyolefin materials, such as polyethylene terephthalate, polyamide, polystyrene, or non-polymeric substances such as wood, paper, glass or aluminum. Worse, these post-consumer recycled polyolefin materials are easily available on a multi-ton scale, but unfortunately have limited mechanical properties and often have severe odor and / or emission problems.

[0004] In addition to the required mechanical properties, the automotive industry is also very critical with regard to odor and emissions, and there is a trend towards further increasing the requirements. This significantly limits the use of recyclates in automotive applications.

[0005] However, there is a deeply felt need to allow the dumping and reuse of post-consumer polyolefin recyclates in final products without causing harm to health and safety.

[0006] The present invention is based on the unexpected finding that complex heterophasic polypropylene copolymers can be at least partially replaced by polypropylene-polyethylene blends derived from post-consumer recycled polyolefin streams, even with benefits regarding VOC properties and tiger stripe performance (MSE). Unexpectedly, anisotropy is not degraded. Summary of the invention

[0007] The present invention provides a composition suitable for automotive applications, wherein the composition is obtainable by blending at least components a) to f), or by blending at least components a), b), c), d) and f) in the absence of e):

[0008] a) 12 to 40 wt%, preferably 14 to 38 wt%, more preferably 15 to 35 wt% of a first heterophasic polypropylene copolymer (HECO 1);

[0009] b) 12 to 40 wt%, preferably 14 to 38 wt%, more preferably 15 to 35 wt% of a second heterophasic polypropylene copolymer (HECO 2);

[0010] c) 15 to 65 wt%, preferably 18 to 60 wt%, more preferably 20 to 55 wt% of a polypropylene-polyethylene blend (A);

[0011] d) 3.0 to 20 wt%, preferably 5.0 to 15 wt%, more preferably 6.0 to 15 wt% of an inorganic filler;

[0012] e) 0 to 15 wt% HDPE;

[0013] f) 0.01 to 4.0 wt% of additives;

[0014] All percentages are with respect to the total composition;

[0015] The total polyethylene content is 5.0 to 15.0 wt% relative to the total amount of the composition, and the total polyethylene content is the sum of the HDPE and the polyethylene of the polypropylene-polyethylene blend (A);

[0016] (i) the first heterophasic polypropylene copolymer (HECO 1) comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, the first heterophasic polypropylene copolymer (HECO 1) having:

[0017] - a melt flow rate MFR2 (230°C, ISO 1133) of 8 to 25 g / 10 min, preferably 10 to 24 g / 10 min, more preferably 12 to 23 g / 10 min; and

[0018] - an intrinsic viscosity of the xylene cold soluble fraction (XCS) content of 3.1 to 4.5 dl / g, preferably 3.2 to 4.4 dl / g, more preferably 3.3 to 4.2 dl / g (measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1);

[0019] (ii) the second heterophasic polypropylene copolymer (HECO 2) comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, the second heterophasic polypropylene copolymer (HECO 2) having:

[0020] - a melt flow rate MFR2 (230°C, ISO 1133) of 25 to 75 g / 10 min, preferably 30 to 70 g / 10 min, more preferably 35 to 65 g / 10 min; and

[0021] - an intrinsic viscosity below the xylene cold soluble fraction (XCS) content observed for HECO 1 (measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1), preferably an intrinsic viscosity of a xylene cold soluble fraction (XCS) content of 2.0 to 3.2 dl / g, more preferably of 2.5 to 3.3 dl / g;

[0022] (iii) the polypropylene-polyethylene blend (A) comprises:

[0023] A-1) polypropylene; and

[0024] A-2) Polyethylene;

[0025] The weight ratio of polypropylene to polyethylene is 19:1 to 7:3, and the polypropylene-polyethylene blend (A) has:

[0026] - a melt flow rate MFR2 (230° C., ISO 1133) of 5.0 to 30 g / 10 min, preferably 7.0 to 26 g / 10 min, more preferably 9.0 to 23 g / 10 min;

[0027] - 2.0 to 15 wt%, preferably 2.5 to 13 wt%, more preferably 3.0 to 11 wt% of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25° C.); and

[0028] - Optionally, a residual ash content below 3.0 wt%, preferably between 0.5 and 2.7 wt%, more preferably between 0.7 and 2.5 wt%;

[0029] The polypropylene-polyethylene blend (A) has one or more of the following characteristics:

[0030] (aa) a limonene content of 0.1 ppm to 100 ppm, preferably 0.1 ppm to 50 ppm, more preferably 0.1 ppm to 20 ppm, most preferably 0.1 ppm to 5 ppm, as measured by solid phase microextraction (HS-SPME-GC-MS);

[0031] (bb) a fatty acid content of 0.1 to 100 ppm as measured by solid phase microextraction (HS-SPME-GC-MS);

[0032] (cc) a polyamide content of 0.05 to 1.5 wt % as measured by FTIR; and

[0033] (dd) a polystyrene content of 0.05 to 3.0 wt % as measured by FTIR; and

[0034] (iv) the inorganic filler, preferably talc:

[0035] - having a median particle size d before compounding of 0.3 to 3.0 μm, more preferably 0.5 to 2.5 μm 50 ;

[0036] - preferably, having a top cut particle size d before compounding of 1.0 to 8.0 μm 95 ;

[0037] Optionally, the HDPE has a melt flow rate (190° C., ISO 1133) of 1.0 to 20 g / 10 min, preferably 1.0 to 10 g / 10 min;

[0038] -945 to 965 kg / m 3 Density, preferably 950 to 960 kg / m 3 density; optionally and preferably

[0039] - Tensile modulus of 800 to 950 MPa (ISO 527-2);

[0040] Components a) to e) comprise at least 90 wt%, preferably at least 95 wt%, most preferably at least 96 wt% of the composition suitable for automotive applications.

[0041] The present invention also provides an article comprising, preferably consisting of, the composition described herein.

[0042] In another aspect, the present invention provides the use of a composition according to the invention for injection molding of an article.

[0043] Specifically, the present invention provides a composition suitable for automotive applications as described above, wherein the composition is obtainable by blending at least components a) to f), or by blending at least components a), b), c), d) and f) in the absence of e):

[0044] a) 12 to 40 wt%, preferably 14 to 38 wt%, more preferably 15 to 35 wt% of a first heterophasic polypropylene copolymer (HECO 1);

[0045] b) 12 to 40 wt%, preferably 14 to 38 wt%, more preferably 15 to 35 wt% of a second heterophasic polypropylene copolymer (HECO 2);

[0046] c) 15 to 65 wt%, preferably 18 to 60 wt%, more preferably 20 to 55 wt% of a polypropylene-polyethylene blend (A);

[0047] d) 3.0 to 20 wt%, preferably 5.0 to 15 wt%, more preferably 6.0 to 15 wt% of an inorganic filler;

[0048] e) 0 to 15 wt% HDPE;

[0049] f) 0.01 to 4.0 wt% of additives;

[0050] All percentages are with respect to the total composition;

[0051] The total polyethylene content is 5.0 to 15.0 wt% relative to the total amount of the composition, and the total polyethylene content is the sum of the HDPE and the polyethylene of the polypropylene-polyethylene blend (A);

[0052] (i) the first heterophasic polypropylene copolymer (HECO 1) comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, the first heterophasic polypropylene copolymer (HECO 1) having:

[0053] - a melt flow rate MFR2 (230°C, ISO 1133) of 8 to 25 g / 10 min, preferably 10 to 24 g / 10 min, more preferably 12 to 23 g / 10 min;

[0054] - an intrinsic viscosity of the xylene cold soluble fraction (XCS) content of 3.1 to 4.5 dl / g, preferably 3.2 to 4.4 dl / g, more preferably 3.3 to 4.2 dl / g (measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1);

[0055] - 19 to 40 wt%, preferably 20 to 37 wt%, more preferably 22 to 35 wt% of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25° C.);

[0056] - a melt flow rate MFR2 (230° C., ISO 1133) of the xylene insoluble fraction (XCI) (ISO 16152, 1st edition, 25° C.) of 20 to 50 g / 10 min, preferably 25 to 45 g / 10 min, more preferably 28 to 44 g / 10 min; and

[0057] - a content of units derived from ethylene in the xylene cold soluble fraction (XCS) of 40 to 60 wt %, preferably 41 to 55 wt %, more preferably 42 to 50 wt %;

[0058] (ii) the second heterophasic polypropylene copolymer (HECO 2) comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, the second heterophasic polypropylene copolymer (HECO 2) having:

[0059] - a melt flow rate MFR2 (230°C, ISO 1133) of 25 to 75 g / 10 min, preferably 30 to 70 g / 10 min, more preferably 35 to 65 g / 10 min; and

[0060] - an intrinsic viscosity below the xylene cold soluble fraction (XCS) content observed for HECO 1 (measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1), preferably an intrinsic viscosity of a xylene cold soluble fraction (XCS) content of 2.0 to 3.2 dl / g, more preferably of 2.5 to 3.3 dl / g;

[0061] - 8 to 18 wt%, preferably 10 to 17 wt%, more preferably 12 to 17 wt% of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25° C.);

[0062] - a melt flow rate MFR2 (230° C., ISO 1133) of the xylene insoluble fraction (XCI) (ISO 16152, 1st edition, 25° C.) of 50 to 200 g / 10 min, preferably 60 to 180 g / 10 min, more preferably 70 to 160 g / 10 min; and

[0063] - a content of units derived from ethylene in the xylene cold soluble fraction (XCS) of 25 to 44 wt %, preferably 30 to 42 wt %, more preferably 35 to 40 wt %;

[0064] (iii) the polypropylene-polyethylene blend (A) comprises:

[0065] A-1) polypropylene; and

[0066] A-2) Polyethylene;

[0067] The weight ratio of polypropylene to polyethylene is 19:1 to 7:3, and the polypropylene-polyethylene blend (A) has:

[0068] - a melt flow rate MFR2 (230° C., ISO 1133) of 5.0 to 30 g / 10 min, preferably 7.0 to 26 g / 10 min, more preferably 9.0 to 23 g / 10 min;

[0069] - 2.0 to 15 wt%, preferably 2.5 to 13 wt%, more preferably 3.0 to 11 wt% of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25° C.); and

[0070] - Optionally, a residual ash content below 3.0 wt%, preferably between 0.5 and 2.7 wt%, more preferably between 0.7 and 2.5 wt%;

[0071] The polypropylene-polyethylene blend (A) has one or more of the following characteristics:

[0072] (aa) a limonene content of 0.1 ppm to 100 ppm, preferably 0.1 ppm to 50 ppm, more preferably 0.1 ppm to 20 ppm, most preferably 0.1 ppm to 5 ppm, as measured by solid phase microextraction (HS-SPME-GC-MS);

[0073] (bb) a fatty acid content of 0.1 to 100 ppm as measured by solid phase microextraction (HS-SPME-GC-MS); (cc) a polyamide content of 0.05 to 1.5 wt% as measured by FTIR; and

[0074] (dd) a polystyrene content of 0.05 to 3.0 wt % as measured by FTIR; and

[0075] (iv) the inorganic filler, preferably talc:

[0076] - having a median particle size d before compounding of 0.3 to 3.0 μm, more preferably 0.5 to 2.5 μm 50 ;

[0077] - preferably, having a top cut particle size d before compounding of 1.0 to 8.0 μm 95 ;

[0078] Optionally, the HDPE has a melt flow rate (190° C., ISO 1133) of 1.0 to 20 g / 10 min, preferably 1.0 to 10 g / 10 min;

[0079] -945 to 965 kg / m 3 Density, preferably 950 to 960 kg / m 3 density; optionally but preferably

[0080] - Tensile modulus of 800 to 950 MPa (ISO 527-2);

[0081] Components a) to e) comprise at least 90 wt%, preferably at least 95 wt%, most preferably at least 96 wt% of the composition suitable for automotive applications.

[0082] The tensile modulus (ISO 527.2; 23° C.) of the composition of the present invention is preferably from 1650 to 1900 MPa.

[0083] Beneficial Effects

[0084] The present invention not only allows to replace complex heterophasic propylene copolymers with recycled polypropylene-polyethylene blends originating from household waste which can be obtained on a very large scale, but also enables to improve the tiger grain properties as reflected by the MSE values ​​and the VOC (VDA 278) properties. Furthermore, despite the common belief that shrinkage and anisotropy will be worse when introducing recycled polyolefin blends, in the present invention the anisotropy results remain the same. DETAILED DESCRIPTION

[0085] definition

[0086] Unless otherwise defined, all technical terms and scientific terms used herein have the same meanings as those generally understood by those of ordinary skill in the art to which the present invention belongs. Although any methods and materials similar or equivalent to those described herein can be used in practice for the test of the present invention, preferred materials and methods are as described herein. When describing and claiming the present invention, the following terms will be used according to the definitions listed below. Unless otherwise expressly stated, the use of the terms "a", "a kind" etc. refers to one (kind) or more (kinds).

[0087] For the purpose of this specification, the term "recycled waste" or "recycled material" is used to refer to materials recovered from both post-consumer waste and industrial waste, as opposed to virgin polymers. Post-consumer waste refers to items that have completed at least the first use cycle (or life cycle), i.e., items that have reached their first purpose. In contrast, industrial waste refers to manufacturing waste, conversion waste, respectively, which usually do not reach the hands of consumers. The term "virgin" refers to newly manufactured materials and / or items that have not been recycled before their first use. Virgin materials and post-consumer materials can be easily distinguished based on the presence or absence of contaminants (e.g., limonene and / or fatty acids and / or paper and / or wood). Polypropylene-polyethylene blends can also be distinguished from their sources by the presence of polystyrene and / or polyamide. The residual content represents the content above the detection limit. Many different types of polyethylene or polypropylene can be present in "recycled materials". The ratio of polypropylene (A-1) to polyethylene plus polyethylene copolymer (A-2) is experimentally determined by using isotactic polypropylene (iPP) and high-density polyethylene (HDPE) for calibration. Polymer blends are mixtures of more than 2 polymer components. Typically, blends can be made by mixing more than two polymeric components. Suitable mixing procedures known in the art are post-polymerization blending. Post-polymerization blending can be dry blending of polymeric components (e.g., polymer powders and / or compounded polymer pellets) or melt blending of polymeric components by melt mixing. Propylene random copolymers are copolymers of propylene monomer units and comonomer units, wherein the comonomer units are randomly distributed on the polypropylene chain. "Compatibilizers" are substances in polymer chemistry that are added to polymer blends with limited intermiscibility to increase their stability. "Polypropylene-polyethylene blends" refer to compositions comprising both polypropylene and polyethylene, and also include polypropylene copolymers and polyethylene copolymers. Since the polypropylene content and polyethylene content cannot be directly measured, the weight ratio of polypropylene (A-1) to polyethylene (A-2) of 19:1 to 7:3 represents an equivalent ratio determined by calibration with iPP and HDPE and by IR spectroscopy. The term "elastomer" refers to a natural polymer or synthetic polymer with elasticity. The term "XCS" refers to the xylene cold soluble fraction (XCS wt%) measured at 25°C according to ISO 16152. The term "XCI" refers to the xylene cold insoluble fraction (XCI wt%) measured at 25°C according to ISO 16152. If not otherwise specified, "%" refers to wt%. The presence of heterogeneous properties can be easily determined by the number of glass transition points. Reactor blends are blends derived from production in two or more reactors connected in series or in a reactor with two or more reaction compartments. Reactor blends can alternatively be produced by blending in solution. Reactor blends are contrasted with compounds produced by melt extrusion.The ethylene-based elastomer refers to an elastomer composed of units derived from ethylene in an amount of at least % by weight.

[0088] Compositions of the present invention

[0089] The compositions of the present invention suitable for automotive applications are particularly useful for injection molding of articles used in vehicle interiors and exteriors.

[0090] The composition suitable for automotive applications of the present invention has one or more of the following characteristics:

[0091] (aa) Residual amount of limonene;

[0092] (bb) Residual fatty acid content;

[0093] (cc) residual content of polyamide; and

[0094] (dd) Residual content of polystyrene.

[0095] These residual amounts are introduced by combining the polypropylene-polyethylene blend (A) with a polypropylene-polyethylene blend (A) derived from consumer waste. The presence of this residual material can be used as a way to distinguish between incorporation of polypropylene-polyethylene blends (A) derived from consumer waste and incorporation of polypropylene-polyethylene blends (A) derived from industrial waste. In other words, the above allows a distinction between post-consumer recyclate (PCR) and post-industrial recyclate (PIR). The measurement of the residual amounts of limonene / fatty acids, polyamide and / or polystyrene can be performed on the final composition as well as on the blend (A).

[0096] Preferably, the compositions of the invention suitable for automotive applications have a VOC measured on material directly obtained by extrusion (following the procedure as described in VDA 278) of less than 75 μg / g composition, preferably less than 70 μg / g composition. Without wishing to be bound by theory, the Applicant believes that, in a first aspect, the presence of fillers, in particular the presence of talc, is beneficial. In a second aspect, the incorporation of the polypropylene-polyethylene blend (A) may also contribute to the overall unexpectedly low VOC content, since the polymers may have lost some amount of VOC during their first use due to exposure to adverse weather, i.e. higher temperatures and wind.

[0097] In any case, lower VOC contents, i.e. below 70 μg / g composition (VDA 278), can be obtained by relatively large amounts of blend (A), in particular by 30 to 60 wt%, preferably 35 to 55 wt%, more preferably 45 to 55 wt% of polypropylene-polyethylene blend (A).

[0098] The composition of the present invention comprises a total content of polyethylene of 5.0 to 15.0 wt%, preferably 6.0 to 12.0 wt%, relative to the total composition, the total content of polyethylene being the sum of the HDPE and the polyethylene of the polypropylene-polyethylene blend (A).

[0099] Preferably, the tensile modulus (ISO 527.2; 23°C) of the composition of the present invention is from 1650 to 1900 MPa.

[0100] Preferably, the composition of the present invention has a melt flow rate (ISO 1133, 2.16 kg, 230° C.) of 13.0 to 25 g / 10 min.

[0101] Preferably, the composition of the present invention has an MSE surface quality below 4.5. Such excellent surface quality is obtained at a rather low amount of blend (A), preferably 15 to 30 wt%, more preferably 18 to 30 wt%, most preferably 20 to 30 wt%.

[0102] Preferably, compositions of the present invention suitable for automotive applications have a heat distortion temperature (ISO 75B) of at least 90°C.

[0103] HECO 1

[0104] The first heterophasic polypropylene copolymer (HECO 1) comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, wherein the first heterophasic polypropylene copolymer (HECO 1) has a melt flow rate MFR2 (230°C, ISO 1133) of 8 to 25 g / 10 min, preferably 10 to 24 g / 10 min, more preferably 12 to 23 g / 10 min; and an intrinsic viscosity of the xylene cold soluble fraction (XCS) of 3.1 to 4.5 dl / g, preferably 3.2 to 4.4 dl / g, more preferably 3.3 to 4.2 dl / g (measured in decalin at 135°C according to DIN ISO 1628 / 1).

[0105] Preferably, the first heterophasic polypropylene copolymer (HECO 1) comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, wherein the first heterophasic polypropylene copolymer (HECO 1) has:

[0106] - a melt flow rate MFR2 (230°C, ISO 1133) of 8 to 25 g / 10 min, preferably 10 to 24 g / 10 min, more preferably 12 to 23 g / 10 min;

[0107] - an intrinsic viscosity of the xylene cold soluble fraction (XCS) content of 3.1 to 4.5 dl / g, preferably 3.2 to 4.4 dl / g, more preferably 3.3 to 4.2 dl / g (measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1);

[0108] - 19 to 40 wt%, preferably 20 to 37 wt%, more preferably 22 to 35 wt% of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25° C.);

[0109] - a melt flow rate MFR2 (230° C., ISO 1133) of the xylene insoluble fraction (XCI) (ISO 16152, 1st edition, 25° C.) of 20 to 50 g / 10 min, preferably 25 to 45 g / 10 min, more preferably 28 to 44 g / 10 min; and

[0110] - a content of units derived from ethylene in the xylene cold soluble fraction (XCS) ranging from 40 to 60 wt%, preferably from 41 to 55 wt%, more preferably from 42 to 50 wt%.

[0111] The first heterophasic polypropylene copolymer (HECO 1) is preferably nucleated, more preferably nucleated by poly(vinylcyclohexane). Heterophasic polypropylene copolymers of this nature are commercially available.

[0112] HECO 2

[0113] The second heterophasic polypropylene copolymer (HECO 2) comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, wherein the second heterophasic polypropylene copolymer (HECO 2) has:

[0114] - a melt flow rate MFR2 (230°C, ISO 1133) of 25 to 75 g / 10 min, preferably 30 to 70 g / 10 min, more preferably 35 to 65 g / 10 min; and

[0115] an intrinsic viscosity below the xylene cold soluble fraction (XCS) content observed for HECO 1 (measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1), preferably an intrinsic viscosity of a xylene cold soluble fraction (XCS) content of 2.0 to 3.2 dl / g, more preferably of 2.5 to 3.3 dl / g.

[0116] Preferably, the second heterophasic polypropylene copolymer (HECO 2) comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, wherein the second heterophasic polypropylene copolymer (HECO 2) has:

[0117] - a melt flow rate MFR2 (230°C, ISO 1133) of 25 to 75 g / 10 min, preferably 30 to 70 g / 10 min, more preferably 35 to 65 g / 10 min;

[0118] - an intrinsic viscosity below the xylene cold soluble fraction (XCS) content observed for HECO 1 (measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1), preferably an intrinsic viscosity of a xylene cold soluble fraction (XCS) content of 2.0 to 3.2 dl / g, more preferably of 2.5 to 3.3 dl / g;

[0119] - 8 to 18 wt%, preferably 10 to 17 wt%, more preferably 12 to 17 wt% of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25° C.);

[0120] - a melt flow rate MFR2 (230° C., ISO 1133) of the xylene insoluble fraction (XCI) (ISO 16152, 1st edition, 25° C.) of 50 to 200 g / 10 min, preferably 60 to 180 g / 10 min, more preferably 70 to 160 g / 10 min; and

[0121] - a content of units derived from ethylene in the xylene cold soluble fraction (XCS) ranging from 25 to 44 wt%, preferably from 30 to 42 wt%, more preferably from 35 to 40 wt%.

[0122] Such heterophasic propylene copolymers are commercially available.

[0123] Polypropylene-polyethylene blends (A)

[0124] The polypropylene-polyethylene blend (A) of the present invention comprises:

[0125] A-1) polypropylene; and

[0126] A-2) Polyethylene;

[0127] The weight ratio of polypropylene to polyethylene is 19:1 to 7:3.

[0128] At the same time, the polypropylene-polyethylene blend (A) has:

[0129] - a melt flow rate MFR2 (230° C., ISO 1133) of 5.0 to 30 g / 10 min, preferably 7.0 to 26 g / 10 min, more preferably 9.0 to 23 g / 10 min;

[0130] - 2.0 to 15 wt%, preferably 2.5 to 13 wt%, more preferably 3.0 to 11 wt% of xylene cold soluble fraction (XCS) (ISO 16152, 1st edition, 25° C.); and

[0131] - Optionally, a residual ash content below 3.0 wt%, preferably between 0.5 and 2.7 wt%, more preferably between 0.7 and 2.5 wt%.

[0132] The inventive polypropylene-polyethylene blend (A) is a recycled material, preferably a recycled material originating from household waste. Particularly preferably, the inventive polypropylene-polyethylene blend (A) originates from post-consumer waste in an amount of at least 90 wt%.

[0133] The polypropylene-polyethylene blend (A) of the present invention may have one or more of the following properties:

[0134] aa) a limonene content of 0.1 ppm to 100 ppm, preferably 0.1 ppm to 50 ppm, more preferably 0.1 ppm to 20 ppm, most preferably 0.1 ppm to 5 ppm, as measured by solid phase microextraction (HS-SPME-GC-MS);

[0135] bb) a fatty acid content of 0.1 to 100 ppm as measured by solid phase microextraction (HS-SPME-GC-MS);

[0136] cc) a polyamide content of 0.05 to 1.5 wt % as measured by NMR;

[0137] dd) a polystyrene content of 0.05 to 3.0 wt % as measured by NMR;

[0138] ee) Residual ash content is as described above.

[0139] It should be understood that the composition of the polypropylene-polyethylene blend (A) can vary widely, i.e. can include polypropylene homopolymer, polypropylene copolymer, polyethylene and polyethylene copolymer. Since the polypropylene content and polyethylene content cannot be directly determined, the weight ratio of polypropylene (A-1) to polyethylene (A-2) of 19:1 to 7:3 is an equivalent ratio determined by calibration of iPP and HDPE.

[0140] Typically, the polypropylene-polyethylene blend (A) of the present invention may also have one or more of the following properties:

[0141] - the residual content of PET measured as described in the experimental part;

[0142] - residual talc and chalk content as described in the experimental part;

[0143] - Residual content of metals measured by X-ray fluorescence (XRF);

[0144] - the residual amount of paper as described in the experimental part;

[0145] - the amount of wood residue as described in the experimental section; and

[0146] - The total free fatty acid content measured by using headspace solid phase microextraction (HS-SPME-GC-MS) was 0.1 ppm to 100 ppm.

[0147] Preferably, the polypropylene-polyethylene blend (A) of the present invention is obtained by washing and / or aeration steps known in the art.

[0148] additive

[0149] Additives are generally used in the composition of the present invention. Preferably, the additives are selected from at least one of antioxidants, UV stabilizers, slip agents, nucleating agents, pigments, lubricants, masterbatch polymers and / or anti-fogging agents.

[0150] Inorganic fillers

[0151] The inorganic filler is preferably talc. The inorganic filler (preferably talc) has a median particle size d before compounding of 0.3 to 3.0 μm, more preferably 0.5 to 2.5 μm. 50 ; preferably, having a top cut particle size d before compounding of 1.0 to 8.0 μm 95 Such inorganic fillers are commercially available.

[0152] HDPE

[0153] HDPE, in particular virgin HDPE, can be added to the composition of the present invention in an amount of up to 15 wt%. HDPE contributes to the scratch resistance of the final composition. Due to the presence of HDPE in blend (A), the amount of HDPE used for the targeted scratch resistance can be reduced or can be omitted entirely.

[0154] Detailed Description

[0155] Several preferred embodiments will be described below.

[0156] In a first preferred embodiment, the composition of the invention suitable for automotive applications is obtainable by blending at least components a) to f), or by blending at least components a), b), c), d) and f) in the absence of e):

[0157] a) 20 to 40 wt%, preferably 20 to 38 wt%, more preferably 20 to 35 wt% of a first heterophasic polypropylene copolymer (HECO 1);

[0158] b) 20 to 40 wt%, preferably 20 to 38 wt%, more preferably 20 to 35 wt% of a second heterophasic polypropylene copolymer (HECO 2);

[0159] c) 15 to 30 wt%, preferably 18 to 30 wt%, more preferably 20 to 30 wt% of a polypropylene-polyethylene blend (A);

[0160] d) 3.0 to 20 wt%, preferably 5.0 to 15 wt%, more preferably 6.0 to 15 wt% of an inorganic filler;

[0161] e) 0 to 15 wt% HDPE;

[0162] f) 0.01 to 4.0 wt% of additives;

[0163] Therein, components a) to e) account for at least 90 wt%, preferably at least 95 wt%, most preferably at least 96 wt% of the composition suitable for automotive applications.

[0164] In this embodiment, the amount of blend (A) is quite low, i.e. the amount of recyclate that can be dumped in the final product is not that high. However, in this embodiment, the MSE surface quality is surprisingly excellent and the VOC is also good. All definitions and preferences as described above for the individual components, in particular for blend (A), also apply to this embodiment.

[0165] Therefore, preferably, the composition according to this embodiment has an MSE surface quality below 4.5.

[0166] In another embodiment, the composition of the present invention suitable for automotive applications can be obtained by blending at least components a) to f), or can be obtained by blending at least components a), b), c), d) and f) in the absence of e):

[0167] a) 10 to 20 wt%, preferably 11 to 20 wt%, more preferably 12 to 20 wt% of a first heterophasic polypropylene copolymer (HECO 1);

[0168] b) 10 to 20 wt%, preferably 11 to 20 wt%, more preferably 12 to 20 wt% of a second heterophasic polypropylene copolymer (HECO 2);

[0169] c) 30 to 60 wt%, preferably 35 to 55 wt%, more preferably 45 to 55 wt% of a polypropylene-polyethylene blend (A);

[0170] d) 3.0 to 20 wt%, preferably 5.0 to 15 wt%, more preferably 6.0 to 15 wt% of an inorganic filler;

[0171] e) 0 to 15 wt% HDPE;

[0172] f) 0.01 to 4.0 wt% of additives;

[0173] Therein, components a) to e) account for at least 90 wt%, preferably at least 95 wt%, most preferably at least 96 wt% of the composition suitable for automotive applications.

[0174] In this second embodiment, the amount of polypropylene-polyethylene blend (A) (i.e. the amount of recyclate) is maximized. This allows dumping a higher amount of recyclate in the final product.

[0175] All definitions and preferences described above for the individual components, in particular for blend (A), also apply to this embodiment.

[0176] Preferably, the composition according to the second embodiment has a VOC of less than 70 μg / g of composition, measured according to the procedure described in VDA 278 on material obtained directly by extrusion.

[0177] Experimental Section

[0178] The following examples are included to demonstrate certain aspects and embodiments of the present invention as described in the claims. However, it should be understood by those skilled in the art that the following description is exemplary only and should not be construed as limiting the present invention in any way.

[0179] Test methods

[0180] a) Amount of iPP, polystyrene, polyethylene (and copolymers containing ethylene), poly(ethylene terephthalate) and amount of polyamide-6

[0181] To establish different calibration curves, different standards, iPP and HDPE and iPP, PS and PA6 were blended. To quantify the content of foreign polymers, IR spectra were recorded in the solid state using a Bruker Vertex 70 FTIR spectrometer. Films were prepared using a compression molding device at 190 ° C with a clamping force of 4 to 6 MPa. The thickness of the film used for the calibration standards for iPP and HDPE was 300 μm, and for the quantification of iPP, PS and PA6, a film thickness of 50 to 100 μm was used. By using a 4000-400 cm -1 spectral range, 6mm aperture, 2cm -1 Standard transmission FTIR spectroscopy was used with a spectral resolution of 16 background scans, 16 spectral scans, an interferogram zero filling factor of 32, and Norton Beer strong apodization.

[0182] Measured iPP at 1167cm -1The iPP content was quantified based on the absorbance of the band at , and the calibration curve (absorption / thickness in cm vs. iPP content in wt%).

[0183] Measured at 1601cm -1 (PS) and 3300cm -1 The PS and PA6 contents are quantified according to the calibration curve (absorption / thickness in cm vs. PS and PA content in wt%) by measuring the absorption of the band at (iPP+PS+PA6). The content of polyethylene and ethylene-containing copolymers is obtained by subtracting (iPP+PS+PA6) from 100, taking into account the content of non-polymeric impurities measured in the following method. The analysis is carried out as a double determination.

[0184] b) Tensile modulus and tensile strain at break

[0185] The tensile modulus and tensile strain at break were measured according to ISO 527-2 (crosshead speed = 1 mm / min; test speed 50 mm / min at 23° C.) using injection molded test specimens 1B (dog bone shape, 4 mm thick) prepared according to EN ISO 1873-2. The measurements were performed after a conditioning time of 96 hours at 23° C. for the test specimens.

[0186] c) Impact strength

[0187] 80×10×4 mm prepared according to EN ISO 1873-2 3 The impact strength is measured as the Charpy notched impact strength at +23°C, 0°C and -20°C according to ISO 179-1eA on injection-molded specimens of 1000 mm / s. The measurement is carried out after the specimens have been conditioned for 96 hours at 23°C.

[0188] d) Instrument breakdown test

[0189] According to ISO6603-2:2000 at 23℃, 0℃ and 20℃ in 60×60×1mm 3 Instrumented puncture tests were performed on injection-molded panels of 1000 mm / s. The measurements were performed after the specimens had been conditioned for 96 hours at 23°C.

[0190] e) Comonomer content

[0191] Poly(propylene-co-ethylene)-ethylene content-IR spectrum

[0192] Quantitative infrared (IR) spectroscopy is used to quantify the ethylene content of poly(ethylene-co-propylene) copolymers by calibration as a primary method. 13The calibration was facilitated by using in-house non-commercial calibration standards (measured by C solution state nuclear magnetic resonance (NMR) spectroscopy). The calibration procedure was performed in a conventional manner well documented in the literature. The calibration set consisted of 38 calibration standards with ethylene contents ranging from 0.2 to 75.0 wt % produced under various conditions at pilot or full scale. The calibration set was selected to reflect typical copolymer species encountered by the final quantitative IR spectroscopy.

[0193] Quantitative IR spectra were recorded in the solid state using a Bruker Vertex 70 FTIR spectrometer. 2 The spectra were recorded on square films. For samples with very high ethylene content (>50 mol%), 100 μm thick films were used. -1 spectral range, 6mm aperture, 2cm -1 Standard transmission FTIR spectroscopy was used with a spectral resolution of 16 background scans, 16 spectral scans, an interferogram zero filling factor of 64, and the Blackmann-Harris 3-term apodization method. >2 The structural unit is between 730 and 720 cm -1 The total area of ​​CH2 rocking deformation at Q )(Integral method G, limits are 762 and 694 cm -1 ) for quantitative analysis. The quantitative band was normalized to the band at 4323 cm corresponding to the CH structural unit. -1 The CH band area (A R )(Integral method G, limits are 4650 and 4007 cm -1 Then, using the secondary calibration curve, the normalized absorbance (A Q / A R ) predicts the ethylene content in weight percent. The calibration curve has been previously constructed by ordinary least squares (OLS) regression of the normalized absorbance measured on the calibration set and the initial comonomer content.

[0194] Poly(propylene-co-ethylene)-ethylene content- 13 C NMR spectroscopy

[0195] against 1 H and 13 Quantitative measurements were recorded in solution using a Bruker Avance III 400 NMR spectrometer operating at 400.15 and 100.62 MHz, respectively. 13 C{ 1H} NMR spectrum. Nitrogen was used as the atmosphere for all the experiments and the temperature was 125°C. 13 All spectra were recorded using a temperature probe head with an optimal extension of 10 mm at 40 °C. About 200 mg of the material was dissolved in 3 mL of 1,2-tetrachloroethane-d2 (TCE-d2) along with chromium (III) acetylacetonate (Cr(acac)3) to give a 65 mM solution of the relaxation agent in the solvent (Singh, G., Kothari, A., Gupta, V., Polymer Testing 28 5 (2009), 475).

[0196] To ensure that the solution is uniform, the NMR tube is further heated in a rotary furnace for at least 1 hour after initial sample preparation in a heating block. After inserting the magnet, the tube is rotated at 10 Hz. This setting is selected mainly for the quantitative needs of high resolution and accurate quantification of ethylene content. Standard single pulse excitation without NOE is used, using the optimal top cone angle, 1s cycle delay and double-stage WALTZ16 decoupling scheme (Zhou, Z. et al., J. Mag. Reson. 187 (2007) 225; and Busico, V. et al., Macromol. Rapid Commun. 2007, 28, 1128). A total of 6144 (6k) transient signals were collected for each spectrum. The quantitative 13C{1H} NMR spectrum is processed and integrated, and the relevant quantitative characteristics are determined by the integration. Using the chemical shift of the solvent, all chemical shifts are indirectly referenced to the central methylene of the ethylene block (EEE) at 30.00 ppm. Even if this structural unit is not present, the method can be similarly referenced. A characteristic signal corresponding to ethylene incorporation was observed (Cheng, HN, Macromolecules 17 (1984), 1950), and the comonomer fraction was calculated as the fraction of ethylene in the polymer relative to all monomers in the polymer: fE = E / (P + E). Using the method of Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157), by 13 C{ 1The comonomer fraction is quantified by integrating multiple signals over the entire spectral region of the {H} spectrum. This method was chosen for its robustness and ability to account for the presence of regional defects when necessary. The integration region is slightly adjusted to increase applicability to the entire range of comonomer contents encountered. For systems with very low ethylene contents where only isolated ethylene in the PPEPP sequence is observed, the method of Wang et al. is modified to reduce the impact of integration of sites that are no longer present. This approach reduces the overestimation of ethylene content for such systems by reducing the number of sites used to determine the absolute ethylene content to E = 0.5(Sββ + Sβγ + Sβδ + 0.5(Sαβ + Sαγ)). By using this set of sites, the corresponding integration equation becomes E = 0.5(I H +I G +0.5(I C +I D )) using the same notation as used in the article by Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157). The equation for absolute propylene content was not modified. The mole percent of comonomer incorporation was calculated from the mole fraction: E [mol %] = 100 × fE. The weight percent of comonomer incorporation was calculated from the mole fraction: E [wt %] = 100 × (fE × 28.06) / ((fE × 28.06) + ((1-fE) × 42.08)).

[0197] f) Comonomer content

[0198] Using the film thickness method, the intensity of the quantitative strip I(q) and the thickness of the pressed film T are used to determine the content using the following relationship: [I(q) / T]m+c=C, where m and c are obtained from a calibration curve (using 13 The comonomer content was determined from the C-NMR spectrum.

[0199] Using a Nicolet Magna 550IR spectrometer with Nicolet Omnic FTIR software, the 13 The comonomer content was measured in a known manner by Fourier transform infrared spectroscopy (FTIR) calibrated with C-NMR. Films with a thickness of about 250 μm were compression molded from the samples. Similar films were made from calibration samples with known comonomer content. The comonomer content was determined by the wavelengths from 1430 to 1100 cm -1 The absorbance is measured as the peak height by selecting the so-called short baseline or long baseline or both. The minimum and the peak height are determined by the wavelength of about 1410-1220 cm -1 The long baseline is drawn at about 1410-1320cm -1The short baseline in the . A specific calibration is required for each baseline type. In addition, the comonomer content of the unknown samples is within the range of the comonomer content of the calibration samples.

[0200] g) Talc and chalk content

[0201] The TGA follows the following procedure:

[0202] Thermogravimetric analysis (TGA) experiments were performed using a Perkin Elmer TGA 8000. About 10 to 20 mg of material was placed in a platinum pan. The temperature was equilibrated at 50°C for 10 minutes and then raised to 950°C at a heating rate of 20°C / min under nitrogen. The calculated weight loss (WCO2) between 550°C and 700°C was assigned to the CO2 escaping from the CaCO3, so the chalk content was estimated as:

[0203] Chalk content = 100 / 44×WCO2

[0204] Then, the temperature was lowered to 300°C at a cooling rate of 20°C / min. The gas was then switched to oxygen and the temperature was raised again to 900°C. The weight loss in this step was assigned to carbon black (Wcb). Knowing the contents of carbon black and chalk, the ash content excluding chalk and carbon black was calculated as:

[0205] Ash content = (ash residue) – 56 / 44 × WCO2 – Wcb

[0206] Wherein the ash residue is the wt% measured at 900°C in the first step carried out under nitrogen. The ash content was estimated to be the same as the talc content for the recyclate studied.

[0207] h)MFR

[0208] Melt flow rate (MFR2) is measured at 230°C (polypropylene-based materials) or 190°C (polyethylene-based materials) under a load of 2.16 kg. The melt flow rate is the amount of polymer in g that is extruded within 10 minutes at a temperature of 230°C (or 190°C) using a test apparatus standardized according to ISO 1133 under a load of 2.16 kg.

[0209] i) Amount of metal

[0210] The amount of metal was determined by X-ray fluorescence (XRF).

[0211] j) Amount of paper and wood

[0212] Paper and wood were measured by conventional laboratory methods including grinding, flotation, microscopy and thermogravimetric analysis (TGA).

[0213] k) Limonene measurement

[0214] Limonene was quantified by standard addition using solid phase microextraction (HS-SPME-GC-MS).

[0215] After adding different concentrations of limonene and a glass-coated magnetic stirring bar, 50 mg of ground sample was weighed into a 20 mL headspace bottle. The bottle was closed with a magnetic cap lined with silica gel / PTFE. A known concentration of diluted limonene standard was added to the sample using a microcapillary (10 pL). 0, 2, 20 and 100 ng (equal to 0 mg / kg, 0.1 mg / kg, 1 mg / kg and 5 mg / kg) of limonene was added, and in addition, a standard amount of 6.6 mg / kg, 11 mg / kg and 16.5 mg / kg of limonene was used in combination with some samples tested in this application. For quantitative analysis, ions-93 collected in SIM mode were used. At 60 ° C, the enrichment of volatile fractions was performed by performing headspace solid phase microextraction (using 2 cm stable bending 50 / 30 pm DVB / Carboxen / PDMS fiber) for 20 minutes. Desorption was performed directly in the heated injection port of the GCMS system at 270 ° C.

[0216] GCMS parameters:

[0217] Chromatographic column: 30m HP 5MS 0.25*0.25

[0218] Injector: Splitless, with 0.75 mm SPME liner, 270 °C

[0219] Temperature program: -10℃(1min)

[0220] Carrier gas: Helium 5.0, 31cm / s linear velocity, constant flow

[0221] MS: Single quadrupole, direct interface, 280°C interface temperature

[0222] Acquisition: SIM scan mode

[0223] Scan parameters: 20 to 300amu

[0224] SIM parameters: m / Z 93, 100 ms dwell time

[0225] l) Total free fatty acid content

[0226] Fatty acid quantification was performed by standard addition using headspace solid phase microextraction (HS-SPME-GC-MS).

[0227] 50mg ground sample was weighed in 20mL headspace bottle, after adding different concentrations of limonene and glass-coated magnetic stirring bar, the magnetic cap of silicone / PTFE lining was used to close the bottle. Free fatty acid mixture (acetic acid, propionic acid, butyric acid, valeric acid, caproic acid and octanoic acid) standard after dilution of known concentration was added in three different levels of samples using 10 μL microcapillaries. Each independent acid of 0,50,100 and 500ng (equal to 0mg / kg, 1mg / kg, 2mg / kg and 10mg / kg) was added. For quantitative, for all acids except propionic acid (here, ion 74 was used), ion 60 obtained under SIM mode was used.

[0228] GCMS parameters:

[0229] Chromatographic column: 20m ZB Wax plus 0.25*0.25

[0230] Syringe: Split 5:1, split liner with glass lining, 250°C

[0231] Temperature program: 40℃(1min)@6℃ / min to 120℃, @15℃ / min to 245℃(5min)

[0232] Carrier: Helium 5.0, 40cm / s linear velocity, constant current

[0233] MS: Single quadrupole, direct interface, 220°C interface temperature

[0234] Acquisition: SIM scan mode

[0235] Scan parameters: 46 to 250 amu, 6.6 scans / second

[0236] SIM parameters: m / z 60, 74, 6.6 scans / s

[0237] m) Glass transition temperature

[0238] The glass transition temperature was determined by dynamic mechanical thermal analysis according to ISO 6721-7. The glass transition temperature was determined by dynamic mechanical thermal analysis using a TA Ares G2 test apparatus at a heating rate of 2°C / min and a frequency of 1 Hz at temperatures between -130 and 160°C on compression molded samples (40×10×1 mm 3 ) and measured in torsional deformation mode.

[0239] n) VOC content

[0240] The VOC content was determined in accordance with VDA 278 on compositions obtained directly by compounding, ie subjected only to the storage prescribed in VDA 278.

[0241] o) Particle size distribution of fillers (especially talc)

[0242] Median particle size d measured by gravity liquid sedimentation according to ISO 1-3 50 and top cut particle size d 95 .

[0243] p) Xylene cold soluble fraction (XCS, wt%)

[0244] According to ISO 16152 (1st edition; 2005-07-01), the xylene cold soluble fraction (XCS) is determined at 25° C. The part that remains insoluble is the xylene cold insoluble (XCI) fraction.

[0245] q) Intrinsic viscosity

[0246] The intrinsic viscosity is determined in accordance with DIN ISO 1628 / 1 (October 1999) (in decalin at 135° C.).

[0247] r) Ash content

[0248] Ash content was determined according to ISO 3451-1 (1997) standard.

[0249] s) Density

[0250] Density was determined according to ISO 1183-187. Sample preparation was performed by compression molding according to ISO 1872-2:2007.

[0251] t) Heat Deformation Temperature (HDT)

[0252] 80×10×4 mm prepared according to ISO 1873-2 and stored at +23°C for at least 96 hours before measurement 3 The HDT is determined on injection moulded test specimens. The test is carried out according to ISO 75, condition A, at a nominal surface stress of 1.80 MPa, on flat supported specimens.

[0253] u)DSC analysis, melting temperature (T m ) and heat of fusion (H f ), crystallization temperature (T c ) and melting enthalpy (H m )

[0254] The measurements were performed using a TA Instrument Q200 Differential Scanning Calorimeter (DSC) on 5 to 7 mg samples. The DSC was run in the temperature range of -30 to +225°C at a scan rate of 10°C / min with a heating / cooling / heating cycle according to ISO 11357 / Part 3 / Method C2. The crystallization temperature (T c) is determined from the cooling step, while the melting temperature (T m ) and melting enthalpy (H m ) is determined from the second heating step. For fully crystalline polypropylene, by assuming H m The value is 209 J / g, and the crystallinity is calculated based on the melting enthalpy (see Brandrup, J., Immergut, EH, eds., Polymer Handbook, 3rd edition, Wiley, New York, 1989; Chapter 3).

[0255] v) Shrinkage FD, Shrinkage CD, Anisotropy

[0256] Shrinkage was measured on center-gated, injection-molded discs (180 mm diameter, 3 mm thickness, with a flow angle of 355° and a notch of 5°). Two specimens were molded with 2 different holding times (10 s and 20 s, respectively). The melt temperature at the gate was 260°C, the average flow front speed in the mound was 100 mm / s. Tool temperature: 40°C, back pressure: 600 bar.

[0257] After conditioning the specimens at room temperature for 96 hours, the dimensional changes radially and tangentially to the flow direction were measured for both discs. The average of the respective values ​​from the two discs was reported as the final result.

[0258] Anisotropy is the ratio of the shrinkage factor FD to the shrinkage factor CD.

[0259] w) Tiger stripes (MSE) or flow marks

[0260] The tendency to show flow marks was tested using the method described below. The method is described in detail in WO 2010 / 149529, the entire contents of which are incorporated herein. The surface quality was characterized using an optical measurement system described by Sybille Frank et al. in PPS 25 Intern. Conf. Polym. Proc. Soc 2009 or Proceedings of the SPIE, Vol. 6831, pp. 68130T-68130T-8 (2008).

[0261] The approach consists of two aspects:

[0262] 1. Image recording:

[0263] The basic principle of the measuring system is to illuminate the plate with a defined light source (LED) in a closed environment and to record the image with a CCD-camera system.

[0264] 2. Image analysis:

[0265] The specimen is illuminated from one side and the upwardly reflected part of the light is deflected by two mirrors to a CCD sensor. The gray value image thus generated is analyzed line by line. The mean square error (MSE) is calculated from the deviations of the recorded gray values, which allows the surface quality to be quantified, i.e. the larger the MSE value, the more obvious the surface defects. In general, for an identical material, the tendency to flow marks increases when the injection speed increases.

[0266] For this evaluation, 440×148×2.8 mm plates with die VW K50 and 1.4 mm film gate were used and prepared with different filling times of 1.5, 3 and 6 seconds, respectively.

[0267] Other conditions:

[0268] Melting temperature: 240℃

[0269] Molding temperature: 30℃

[0270] Dynamic pressure: 10 bar hydraulic

[0271] At a certain filling time, the smaller the MSE value, the smaller the tendency of flow marks.

[0272] experiment

[0273] Catalyst system:

[0274] For the polymerization process of HECO 1, the Ziegler-Natta type catalyst used in the inventive examples of WO 2016 / 066446 A1 and described in detail therein was used. For the polymerization process of HECO 2, the same catalyst was used, but the catalyst was prepolymerized with vinylcyclohexane to achieve nucleation with poly(vinylcyclohexane).

[0275] Nucleation by prepolymerization with vinylcyclohexane is described in detail in EP 2960256 B1 and EP 2960279 B1. These documents are incorporated herein by reference. In both cases, triethylaluminum (TEAL) was used as a cocatalyst and dicyclopentadienyl-dimethoxysilane (donor D) was used as an external donor, with the respective feed ratios shown in Table 1 below.

[0276] HECO1 and HECO2 were produced in a prepolymerization / loop reactor / gas phase reactor 1 / gas phase reactor 2 / gas phase reactor 3 configuration followed by a pelletizing step.

[0277] Table 1: Preparation of HECO 1 and HECO 2

[0278]

[0279] The heterophasic copolymers HECO1 and HECO2 were compounded in a co-rotating twin-screw extruder Coperion ZSK 47 at 220°C with 0.15 wt% of an antioxidant (Irganox B215FF from BASF, Germany; a 1:2 mixture of pentaerythritol-tetrakis(3-(3',5'-di-tert-butyl-4-hydroxyphenyl)-propionate (CAS No.: 6683-19-8) and tris(2,4-di-tert-butylphenyl)phosphite (CAS No.: 31570-04-4)), 0.05 wt% of Ca stearate (CAS No.: 1592-23-0, purchased from Faci, Italy).

[0280] Table 2 shows the properties of the polypropylene / polyethylene blends (A) used for evaluation.

[0281] Table 2: Properties of polypropylene / polyethylene blends (blend A)

[0282]

[0283] Table 3: Comparison of basic properties of HECO 1 and HECO 2 with blends (A)

[0284]

[0285] As can be seen from Table 3, it is not foreseeable to replace HECO 1 and / or HECO 2 with blend (A). Blend (A) shows inferior properties for both stiffness and impact properties.

[0286] HDPE is commercial grade with a density of 954kg / m 3 (ISO 1183), MFR2 (ISO 1133) is 4 g / 10 min, and tensile modulus is 850 MPa (ISO 527-2).

[0287] Using the prepared polymer recycled as described above, the final composition was extruded with talc Jetfine 3CA (d 50 =1.2μm; d 95 =3.3μm), antioxidant, UV stabilizer, slip agent, nucleating agent, carbon black masterbatch, calcium stearate, and antifogging agent are mixed together.

[0288]

[0289] As can be seen, the impact strength unexpectedly remains at an acceptable level. The addition of recyclate further results in a slight loss of stiffness. For lower amounts of recyclate (IE1), the tiger grain properties (MSE) are significantly improved, while the VOC (VDA 278, measured on pellets) can be significantly improved (IE1 and IE2).

Claims

1. A composition suitable for automotive applications, wherein: The composition may be obtained by blending at least components a) to f), or may be obtained by blending at least components a), b), c), d) and f) in the absence of e): a) 12 to 40 wt% of a first heterophasic polypropylene copolymer HECO 1; b) 12 to 40 wt% of a second heterophasic polypropylene copolymer HECO 2; c) 15 to 65 wt% of polypropylene-polyethylene blend A; d) 3.0 to 20 wt% of an inorganic filler; e) 0 to 15 wt% HDPE; f) 0.01 to 4.0 wt% of additives; All percentages are with respect to the total composition; Relative to the total amount of the composition, the total polyethylene content is 5.0 to 15.0 wt %, and the total polyethylene content is the sum of the HDPE and the polyethylene in the polypropylene-polyethylene blend A; (i) the first heterophasic polypropylene copolymer HECO 1 comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, the first heterophasic polypropylene copolymer HECO 1 having: - a melt flow rate MFR2 of 8 to 25 g / 10 min, the melt flow rate MFR2 being measured at 230° C. according to ISO 1133; and - an intrinsic viscosity of the xylene cold soluble fraction of 3.1 to 4.5 dl / g, measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1; (ii) the second heterophasic polypropylene copolymer HECO 2 comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, the second heterophasic polypropylene copolymer HECO 2 having: - a melt flow rate MFR2 of 25 to 75 g / 10 min, the melt flow rate MFR2 being measured at 230° C. according to ISO 1133; and - lower than the intrinsic viscosity of the xylene cold soluble fraction observed for HECO 1, measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1; (iii) the polypropylene-polyethylene blend A comprises: A-1) polypropylene; and A-2) Polyethylene; The weight ratio of polypropylene to polyethylene is 19:1 to 7:3, and the polypropylene-polyethylene blend A has: - a melt flow rate MFR2 of 5.0 to 30 g / 10 min, the melt flow rate MFR2 being measured at 230° C. according to ISO 1133; - 2.0 to 15 wt% of xylene cold soluble fraction, measured at 25°C according to ISO 16152 1st edition; and - Optionally, a residual ash content below 3.0 wt%; The polypropylene-polyethylene blend A has one or more of the following characteristics: (aa) a limonene content of 0.1 ppm to 100 ppm as measured by headspace solid phase microextraction-gas chromatography tandem mass spectrometry (HS-SPME-GC-MS); (bb) a fatty acid content of 0.1 to 100 ppm as measured by headspace solid phase microextraction-gas chromatography tandem mass spectrometry (HS-SPME-GC-MS); (cc) a polyamide content of 0.05 to 1.5 wt % as measured by FTIR; and (dd) a polystyrene content of 0.05 to 3.0 wt % as measured by FTIR; and (iv) the inorganic filler: - having a median particle size d before compounding of 0.3 to 3.0 μm 50 ; The optional HDPE has a melt flow rate of 1.0 to 20 g / 10 min and a 3 A density of , the melt flow rate being measured at 190°C according to ISO 1133; Components a) to e) comprise at least 96 wt % of the composition suitable for automotive applications.

2. The composition suitable for automotive applications according to claim 1, wherein The composition may be obtained by blending at least components a) to f) in the following amounts, or may be obtained by blending at least components a), b), c), d) and f) in the following amounts in the absence of e): a) 12 to 40 wt% of a first heterophasic polypropylene copolymer HECO 1; b) 12 to 40 wt% of a second heterophasic polypropylene copolymer HECO 2; c) 15 to 65 wt% of polypropylene-polyethylene blend A; d) 3.0 to 20 wt% of an inorganic filler; e) 0 to 15 wt% HDPE; f) 0.01 to 4.0 wt% of additives; All percentages are with respect to the total composition; Relative to the total amount of the composition, the total polyethylene content is 5.0 to 15.0 wt %, and the total polyethylene content is the sum of the HDPE and the polyethylene of the polypropylene-polyethylene blend A; (i) the first heterophasic polypropylene copolymer HECO 1 comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, the first heterophasic polypropylene copolymer HECO 1 having: - a melt flow rate MFR2 of 8 to 25 g / 10 min, the melt flow rate MFR2 being measured at 230° C. according to ISO 1133; - an intrinsic viscosity of the xylene cold soluble fraction of 3.1 to 4.5 dl / g, measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1; - 19 to 40 wt% of xylene cold soluble fraction, the xylene cold soluble fraction being measured at 25°C according to ISO 16152 1st edition; - a melt flow rate MFR2 of the xylene insoluble fraction measured at 25°C according to ISO 16152 1st edition of 20 to 50 g / 10 min, the melt flow rate MFR2 being measured at 230°C according to ISO 1133; and - a content of units derived from ethylene in the xylene cold soluble fraction of 40 to 60% by weight; (ii) the second heterophasic polypropylene copolymer HECO 2 comprises a matrix phase and an elastomeric phase dispersed in the matrix phase, the second heterophasic polypropylene copolymer HECO 2 having: - a melt flow rate MFR2 of 25 to 75 g / 10 min, the melt flow rate MFR2 being measured at 230° C. according to ISO 1133; - lower than the intrinsic viscosity of the xylene cold soluble fraction observed for HECO 1, measured in decalin at 135° C. in accordance with DIN ISO 1628 / 1; - 8 to 18 wt% of xylene cold soluble fraction, measured at 25°C according to ISO 16152 1st edition; - a melt flow rate MFR2 of the xylene insoluble fraction of from 50 to 200 g / 10 min, the xylene insoluble fraction being measured at 25°C according to ISO 16152 1st edition, the melt flow rate MFR2 being measured at 230°C according to ISO 1133; and - a content of units derived from ethylene in the xylene cold soluble fraction of 25 to 44% by weight; (iii) the polypropylene-polyethylene blend A comprises: A-1) polypropylene; and A-2) Polyethylene; The weight ratio of polypropylene to polyethylene is 19:1 to 7:3, and the polypropylene-polyethylene blend A has: - a melt flow rate MFR2 of 5.0 to 30 g / 10 min, the melt flow rate MFR2 being measured at 230° C. according to ISO 1133; - 2.0 to 15 wt% of xylene cold soluble fraction, measured at 25°C according to ISO 16152 1st edition; and - Optionally, a residual ash content below 3.0 wt%; The polypropylene-polyethylene blend A has one or more of the following characteristics: (aa) a limonene content of 0.1 ppm to 100 ppm as measured by headspace solid phase microextraction-gas chromatography tandem mass spectrometry (HS-SPME-GC-MS); (bb) a fatty acid content of 0.1 to 100 ppm as measured by headspace solid phase microextraction-gas chromatography tandem mass spectrometry (HS-SPME-GC-MS); (cc) a polyamide content of 0.05 to 1.5 wt % as measured by FTIR; and (dd) a polystyrene content of 0.05 to 3.0 wt % as measured by FTIR; and (iv) the inorganic filler: - having a median particle size d before compounding of 0.3 to 3.0 μm 50 ;as well as The optional HDPE has a melt flow rate of 1.0 to 20 g / 10 min and a 3 A density of , the melt flow rate being measured at 190°C according to ISO 1133; Components a) to e) comprise at least 96 wt % of the composition suitable for automotive applications.

3. The composition suitable for automotive applications according to claim 1 or 2, wherein The composition has a tensile modulus of 1650 to 1900 MPa, measured at 23°C according to ISO 527.

2.

4. The composition suitable for automotive applications according to claim 1 or 2, wherein The composition may be obtained by blending at least components a) to f), or may be obtained by blending at least components a), b), c), d) and f) in the absence of e): a) 20 to 40 wt% of a first heterophasic polypropylene copolymer HECO 1; b) 20 to 40 wt% of a second heterophasic polypropylene copolymer HECO 2; c) 15 to 30 wt% of polypropylene-polyethylene blend A; d) 3.0 to 20 wt% of an inorganic filler; e) 0 to 15 wt% HDPE; f) 0.01 to 4.0 wt% of additives; Components a) to e) comprise at least 96 wt % of the composition suitable for automotive applications.

5. The composition suitable for automotive applications according to claim 4, wherein The composition has an MSE surface quality of less than 4.

5.

6. The composition suitable for automotive applications according to claim 1 or 2, wherein The composition may be obtained by blending at least components a) to f), or may be obtained by blending at least components a), b), c), d) and f) in the absence of e): a) 10 to 20 wt% of a first heterophasic polypropylene copolymer HECO 1; b) 10 to 20 wt% of a second heterophasic polypropylene copolymer HECO 2; c) 30 to 60 wt% of polypropylene-polyethylene blend A; d) 3.0 to 20 wt% of an inorganic filler; e) 0 to 15 wt% HDPE; f) 0.01 to 4.0 wt% of additives; Components a) to e) comprise at least 96 wt % of the composition suitable for automotive applications.

7. The composition suitable for automotive applications according to claim 1 or 2, wherein: The composition has a heat distortion temperature of at least 90°C, the heat distortion temperature being measured according to ISO 75B.

8. The composition suitable for automotive applications according to claim 1 or 2, wherein: The composition has a melt flow rate of 13.0 to 25 g / 10 min, the melt flow rate being measured according to ISO 1133 at 230° C. under a load of 2.16 kg.

9. The composition suitable for automotive applications according to claim 1 or 2, wherein: The composition has a VOC of less than 75 μg / g composition, measured according to the procedure as described in VDA 278 on material obtained directly by extrusion.

10. An article comprising the composition of any one of claims 1-9.

11. Use of the composition according to any one of claims 1 to 9 for injection molding of articles.