A non-precious metal-based carbon nanofiber electrode and its preparation method and application
By using non-noble metal-based carbon nanofiber electrodes in the electrocatalytic hydrogenation reduction system, using multi-level pore structure and uniformly dispersed Cu atoms and MoP loading, the problem of low electrocatalytic hydrogenation reduction efficiency is solved and efficient indigo dyeing effect is achieved. and stability.
Patent Information
- Application Number
- CN202310065202.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-01-17
AI Technical Summary
The catalytic activity of the existing electrode materials for the electrocatalytic hydrogenation reduction of indigo dye is not high, resulting in poor dyeing effect and dyeing efficiency, and the single metal catalyst is easy to agglomerate, affecting the dyeing effect.
Using non-noble metal-based carbon nanofiber electrodes, by adding terephthalic acid, soluble copper salts, phosphomolybdate and polyacrylonitrile to the spinning solution, a multi-level pore structure and uniformly dispersed Cu atoms are formed, combined with MoP loading, Improve catalytic activity and reactivity, and enhance the specific surface area and stability of the electrode through specific heat treatment and activation processes.
It significantly improves the electrocatalytic hydrogenation reduction efficiency of indigo dye, enhances the dyeing effect and dyeing efficiency, avoids the agglomeration problem of single metal catalysts, and improves the stability and recycling performance of the electrode.
Smart Images

Figure CN116122039B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of textile chemistry, and in particular to a non-noble metal-based carbon nanofiber electrode and a preparation method and application thereof. Background Art
[0002] Indigo dye is insoluble in water, but indigo dye molecules usually contain two or more conjugated carbonyl groups. When dyeing, it can be reduced by a reducing agent under alkaline conditions to a soluble leuco sodium salt with affinity for cellulose fibers, thereby achieving dyeing of the fibers. After dyeing, it is oxidized and restored to the original insoluble dye lake and fixed on the fibers. The traditional process uses hydrosulfite as a reducing agent, but it releases toxic gases when it encounters acid. At the same time, high concentrations of sulfates and sulfites will be produced during the reduction process, increasing the burden of sewage treatment. Therefore, in recent years, a variety of new reduction methods have been developed for indigo dyeing, such as bacterial reduction, chemical reduction and electrochemical reduction. Among them, electrochemical dyeing has the advantages of high efficiency and cleaning, mild reaction conditions, and adjustable and controllable reaction, and has been widely used in the field of indigo dyeing. Electrochemical dyeing is divided into direct electrochemical reduction, indirect electrochemical reduction and electrocatalytic reduction. Electrocatalytic hydrogenation reduction uses active hydrogen generated in situ by electrolysis of water to reduce the indigo dye on the low hydrogen overpotential conductive catalytic metal to a soluble leuco. At present, the cathode materials used for electrocatalytic hydrogenation reduction include porous graphite electrodes, nickel-zinc alloys, etc., but they all have defects such as low catalytic activity, low indigo conversion rate and low electroreduction rate.
[0003] Previous studies have found that the carbonyl group in the indigo molecule forms a larger conjugated system with the benzene ring and the C=C in the center of the molecule. The easy-to-flow π electron cloud tends to be on the side of the oxygen atom with greater electronegativity. Therefore, the introduction of a metal catalyst will further interact with the oxygen atom with a larger electron cloud density, increase the polarity of C=O and the positive charge of the carbonyl carbon, and activate the indigo molecule. However, the electrocatalytic reaction needs to be carried out under alkaline conditions. The single metal catalyst has low conductivity, poor corrosion resistance and activity, and is easy to agglomerate, resulting in poor dyeing effect and dyeing efficiency of the indigo dye. Therefore, it is urgent to develop a new composite electrode material for electrochemical dyeing to increase the dispersibility of the metal catalyst, increase the adsorption sites and catalytic activity, so as to improve the dyeing efficiency and dyeing effect. Summary of the invention
[0004] In view of the problem that the dyeing effect and dyeing efficiency of electrode materials used for electrochemical dyeing with indigo dye are poor, the present invention provides a non-precious metal-based carbon nanofiber electrode and a preparation method and application thereof.
[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0006] A method for preparing a non-noble metal-based carbon nanofiber electrode comprises the following steps:
[0007] Step a, adding terephthalic acid, soluble copper salt, soluble iron salt, phosphomolybdate and polyacrylonitrile into N,N-dimethylformamide, and dispersing them evenly to obtain a spinning solution;
[0008] Step b, injecting the spinning solution into an electrospinning device for electrospinning, and spraying molybdenum phosphide droplets on the ejected nanofibers during the entire spinning process to obtain a nanofiber felt;
[0009] Step c, pre-oxidizing the nanofiber felt at 260° C.-280° C. in an air atmosphere, and then carbonizing the nanofiber felt at 800° C.-900° C. in an inert atmosphere to obtain carbon nanofibers;
[0010] Step d, immersing the carbon nanofibers into a strong alkaline solution, then activating them at 900°C-1000°C under an inert atmosphere, cooling them, immersing the activated carbon nanofibers into a strong acid solution, washing them, and drying them to obtain a non-precious metal-based carbon nanofiber electrode.
[0011] In the current electrocatalytic hydrogenation reduction system of indigo dye, indigo dye is a water-insoluble solid particle and is separated from water in two phases. Therefore, the contact time between indigo dye and the catalytic electrode is short and the contact area is small. If the electrode's reduction ability is weak and its ability to adsorb hydrogen intermediates is weak, its reduction effect will be poor, resulting in poor dyeing effect.
[0012] Compared with the prior art, the method for preparing the non-noble metal-based carbon nanofiber electrode provided by the present invention has the following advantages:
[0013] (1) As an electrode material, it must realize a self-supporting structure, that is, it can form an electrode without adding a binder, which requires the electrode to have great flexibility and integrity. The present invention adds terephthalic acid to the spinning solution, which directly sublimates during the high-temperature heat treatment process to form a multi-level pore structure in the carbon nanometer, especially a macroporous structure, which greatly improves the flexibility of the spinning membrane and achieves the purpose of forming a flexible electrode without a binder;
[0014] (2) Metal atoms easily aggregate at the nanoscale, affecting their chemical properties. The present invention adds phosphomolybdate to the spinning solution, and obtains a cubic complex through the chelation of phosphomolybdate with copper ions, thereby obtaining uniformly dispersed Cu atoms in the subsequent high-temperature heat treatment, and allowing the Cu atoms to enter the intermediate ring of the graphite phase carbon nitride, thereby achieving the anchoring of Cu atoms on the surface of the graphite phase carbon nitride carrier, avoiding the problem of isolated metal atoms being easily aggregated; in addition, the lone pair of electrons of the nitrogen atom and the large π bond in the carbon atom lattice directly participate in the conjugation, so that the graphite phase carbon nitride material exhibits excellent catalytic performance; furthermore, the specific high-temperature heat treatment forms uniform defects on the surface of the graphite phase carbon nitride material, which provide a basis for anchoring isolated Cu atoms and also provide high reactivity and selectivity for the hydrogenation reaction;
[0015] (3) In the catalytic reaction process, a single metal active site often has the problem of insufficient adsorption sites. Therefore, the present invention introduces Mo and Cu to form diatomic active sites; and the present invention creatively adopts the form of spraying MoP droplets on the fiber surface during the electrospinning process, which can realize the uniform loading of MoP particles on the surface of a single nanofiber and effectively increase the loading amount of MoP, which can be increased to 60wt% of the spinning matrix, achieving the purpose of introducing high-loaded dual catalytic sites in the fiber without affecting the strong coordination of the Cu atomic anchoring site and the carrier, and significantly improving the catalytic performance of the material;
[0016] (5) The P atoms in phosphomolybdate and MoP can serve as proton capture sites, affecting the electron cloud density around Cu and Mo atoms and increasing the electron transfer rate, thus facilitating a rapid catalytic reaction.
[0017] (4) Through specific heat treatment and activation processes, the morphology of the nanofiber electrode is effectively controlled. The carbon nanoarray at the branch of the nanofiber trunk effectively increases the specific surface area of the electrode material. The stability and catalytic activity of the electrode material are significantly improved through N and P heteroatom doping and MoP synergistic effect, breaking through the technical bottleneck of the inability to take into account the loading amount of electroactive substances, conductivity and capacitive activity.
[0018] Preferably, in step a, the soluble copper salt is copper chloride, copper nitrate or copper sulfate.
[0019] Preferably, in step a, the soluble iron salt is ferric chloride, ferric nitrate or ferric sulfate.
[0020] Preferably, in step a, the phosphomolybdate is ammonium phosphomolybdate.
[0021] Preferably, in step a, the mass concentration of terephthalic acid in the electrospinning dispersion is 4%-5%, the mass concentration of soluble copper salt is 3%-4%, the mass concentration of soluble iron salt is 4%-5%, the mass concentration of phosphomolybdate is 2%-4%, and the mass concentration of polyacrylonitrile is 10%-12%.
[0022] The preferred ratio of each raw material is conducive to obtaining a porous fiber membrane with a high Cu loading, and is conducive to subsequent high-temperature treatment to obtain uniformly dispersed Cu atoms, so that the Cu atoms are uniformly anchored on the carrier surface.
[0023] Preferably, in step b, the parameters of the electrospinning are: the distance between the nozzle and the aluminum foil is 12 cm-15 cm, the spinning voltage is 12 kV-14 kV, the spinning flow rate is 0.5 mL / h-1.0 mL / h, and the humidity is 35%-45%.
[0024] Exemplarily, the inner diameter of the spinning needle is 0.2 mm-0.4 mm.
[0025] The preferred electrospinning parameters are conducive to obtaining a continuous nanofiber membrane, making the nanofibers have a porous structure, and improving the specific surface area and flexibility of the nanofibers.
[0026] Preferably, in step b, the molybdenum phosphide solution is passed through an ultrasonic spray humidifier to form molybdenum phosphide droplets and sprayed onto the nanofibers; the molybdenum phosphide solution is a mixed aqueous solution of molybdenum phosphide and sodium dodecylbenzene sulfonate, wherein the concentration of molybdenum phosphide is 1g / L-2g / L, and the concentration of sodium dodecylbenzene sulfonate is 8g / L-10g / L.
[0027] Preferably, in step b, the speed of spraying molybdenum phosphide droplets is 40mL / h-50mL / h.
[0028] In order to ensure that the spinning solution does not block the spinneret hole and to ensure that a continuous fiber membrane is obtained, the electroactive substance is generally added to the prepared fiber membrane with a low loading amount of the electroactive substance, and it is difficult to effectively improve the catalytic activity of the material. The present invention adopts an ultrasonic spray humidifier to spray MoP droplets on the fiber surface, which does not affect the anchoring point of Cu atoms, is conducive to the uniform loading of Cu atoms on the carrier surface, and can achieve a high content of MoP loading, which is conducive to a significant improvement in catalytic activity.
[0029] Preferably, in step c, the pre-oxidation time is 1 h-2 h.
[0030] Preferably, in step c, the temperature is raised to 260°C-280°C in a programmed temperature raising manner, with a heating rate of 0.5°C / min-1.0°C / min.
[0031] Preferably, in step c, the carbonization time is 1.5h-2h.
[0032] Preferably, in step c, the temperature is raised to 800°C-900°C in a programmed temperature raising manner, with a heating rate of 2°C / min-5°C / min.
[0033] Preferably, in step d, the activation time is 2.5h-3h.
[0034] Preferably, in step d, the strong alkaline solution is a 0.8 mol / L-1.2 mol / L sodium hydroxide solution, and the volume-to-mass ratio of the strong alkaline solution to the carbon nanofibers is 20-30:1, wherein the unit of mass is gram and the unit of volume is milliliter.
[0035] Preferably, the immersion time in the strong alkaline solution is 2.5 h to 3.5 h.
[0036] Preferably, in step d, the strong acid solution is a 0.8 mol / L-1.2 mol / L hydrochloric acid solution, and the volume-to-mass ratio of the strong acid solution to the activated carbon nanofibers is 15-20:1, wherein the unit of mass is gram and the unit of volume is milliliter.
[0037] Preferably, the immersion time in the strong acid solution is 1.5 h to 2.5 h.
[0038] The preferred preparation process parameters are beneficial to controlling the morphology of the nanofibers, branching out carbon nanotube arrays on the nanofiber trunk, increasing the specific surface area of the nanofibers, and obtaining nanofibers with uniformly loaded Cu atoms. The synergistic effect of special morphology, uniformly dispersed atomic Cu and MoP effectively improves the electrocatalytic activity and stability of the nanofibers, thereby effectively increasing the catalytic performance, service life and recycling performance of the electrode.
[0039] The present invention also provides a non-noble metal-based carbon nanofiber electrode, which is prepared by any of the above-mentioned methods for preparing the non-noble metal-based carbon nanofiber electrode.
[0040] The present invention also provides the use of the non-noble metal-based carbon nanofiber electrode in electrochemical dyeing of reduced dyes.
[0041] It should be noted that the vat dye in the present invention is indigo dye.
[0042] Metal-based carbon nanofiber electrodes generally adsorb hydrogen atoms to discharge or couple to generate hydrogen, which reduces the electrolysis efficiency. The present invention utilizes the confinement effect of nanofibers and the chelation effect of phosphomolybdate to prepare a composite metal catalyst / multi-level array structure flexible electrode, which can integrate hydrogen production and hydrogenation catalysis through morphology control, doping N, P heteroatoms, and the synergistic effect of evenly dispersed Cu atoms and MoP. It can not only use the active hydrogen generated in situ by electrolysis of water to reduce indigo dye, but also adsorb hydrogen intermediates at the same time to reduce hydrogen evolution side reactions; and the multi-level structure and large specific surface area of the prepared nanofiber electrode are conducive to increasing the effective contact area and cyclic contact rate between indigo dye and catalyst / electrode, significantly improving the efficiency of electrocatalytic hydrogenation reduction, and thus effectively improving the indigo dyeing effect.
[0043] The present invention also provides an electrochemical dyeing process, using the above-mentioned non-noble metal-based carbon nanofiber electrode as a cathode to dye fiber fabrics through electrochemical dye reduction under alkaline conditions.
[0044] Compared with the prior art, the electrochemical dyeing process provided by the present invention can significantly improve the conduction current efficiency, shorten the dye reduction time, and effectively improve the dyeing effect.
[0045] Furthermore, the electrochemical dyeing process specifically comprises the following steps:
[0046] Step 1: Under the protection of an inert atmosphere, using the non-precious metal-based carbon nanofiber electrode as a cathode, adding a reduced dye to a cathode electrolyte, and reducing the reduced dye with a constant current at 20-30° C. under stirring conditions to obtain a reduced dye solution;
[0047] Step 2: placing the wetted fiber fabric into the reduction dyeing solution for dyeing, ventilating and oxidizing, soap boiling, washing and drying to obtain the reduction-dyed fiber fabric.
[0048] Preferably, the initial concentration of the vat dye is 0.5-1.0 g / L.
[0049] Preferably, an H-type electrolysis device is used for constant current reduction, the current density is 40mA-50mA, and the reduction time is 30min-40min.
[0050] Exemplarily, the diaphragm of the H-type electrolysis device is a Nafion membrane.
[0051] Exemplarily, when the non-precious metal-based carbon nanofiber electrode is used as a cathode, it is cut into 1 cm*2 cm.
[0052] Preferably, the cathode electrolyte is a 0.8 mol / L-1.2 mol / L sodium hydroxide solution.
[0053] Preferably, the anode electrode liquid is a 0.8 mol / L-1.2 mol / L sulfuric acid solution.
[0054] Preferably, the anode is a copper sheet or a foam copper electrode.
[0055] Exemplarily, the size of the copper sheet or foam copper electrode is 1 cm*2 cm.
[0056] Preferably, the electrolytic reduction temperature is 20°C-30°C.
[0057] If the temperature is too low, the redox ability of the dye is weak and the amount of reduced dye is small; if the temperature is too high, the properties of the dye will be destroyed and the reduction dyeing of the dye will be affected.
[0058] Exemplarily, soap boiling uses a solution of 4 g / L soap powder and 3 g / L sodium carbonate at 95° C. for 20 min.
[0059] The invention also provides a fiber fabric which is made by utilizing the electrochemical dyeing process.
[0060] The fiber fabric here refers to cotton cloth.
[0061] The composite non-precious metal-based carbon nanofibers prepared by the present invention have excellent catalytic activity, can integrate hydrogen production and hydrogenation catalysis, improve hydrogenation reduction efficiency, and reduce the occurrence of hydrogen evolution side reactions, thereby ensuring a high indigo dye reduction rate, a short dyeing reduction time, and a good indigo dyeing effect. The use of a medium in an indirect electrochemical reduction system and a dye intermediate in a direct electrochemical reduction system can also be avoided, which is conducive to realizing industrial production and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 This is a SEM image of the nanofiber mat prepared in step b of Example 1 of the present invention;
[0063] Figure 2 This is a SEM image of the non-noble metal-based carbon nanofiber electrode prepared in step d of Example 1 of the present invention;
[0064] Figure 3 The cyclic voltammetry curves of the non-noble metal-based carbon nanofiber electrode prepared in Example 1 of the present invention in indigo aqueous solutions of different concentrations are scanned;
[0065] Figure 4 These are photos of the non-precious metal-based carbon nanofiber electrodes prepared in step d in Example 1 and Comparative Example 7 of the present invention, wherein (a) is Example 1, and (b) is Comparative Example 7. DETAILED DESCRIPTION
[0066] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0067] The following examples and comparative examples were tested for performance:
[0068] (1) Absorbance:
[0069] In order to determine the reduction degree of indigo dye during the electrocatalytic hydrogenation process, the Cary 60 UV-visible spectrophotometer probe can be placed in the cathode chamber of the electrolytic cell. The absorption intensity at λmax=668nm is measured to determine the leuco form concentration of indigo dye at different reaction times in the cathode chamber of the electrolytic cell, and the indigo dye reduction rate is calculated based on the absorbance.
[0070] (2) K / S value test
[0071] Before the test, the dyed sample needs to be subjected to standard humidity and temperature control under constant temperature and humidity conditions, and then the K / S value is measured on a Datacolor 650 computer colorimeter for 5 times and the average value is taken.
[0072] (3) Dry and wet friction fastness test
[0073] According to the standard test method of GB / T3920-2008 "Textiles - Tests for Colour Fastness - Colour Fastness to Rubbing", a cotton fabric of 5cm×14cm in size was tested for dry and wet rubbing fastness. At the same time, the standard test of GB / T 251-2008 "Textiles - Tests for Colour Fastness - Grey Scale for Assessing Staining" was used to assess the colour fastness grade.
[0074] (4) Soap fastness test
[0075] According to the standard method of GB / T3921-2008D "Textiles - Colour Fastness - Colour Fastness to Washing with Soap", a cotton fabric of size 10cm×4cm was tested for soap fastness. At the same time, the standard test of GB / T250-2008 "Textiles - Colour Fastness - Grey Sample Scale for Assessing Discoloration" was used to assess the colour fastness to soap washing.
[0076] Example 1
[0077] This embodiment provides a method for preparing a non-noble metal-based carbon nanofiber electrode, comprising the following steps:
[0078] Step a, adding terephthalic acid, copper sulfate, ferric nitrate, ammonium phosphomolybdate and polyacrylonitrile into N,N-dimethylformamide, stirring with a magnetic force at 60° C. until the mixture is uniformly dispersed, to obtain a spinning solution;
[0079] The concentration of terephthalic acid in the spinning solution is 4wt%, the concentration of copper sulfate is 3wt%, the concentration of ferric nitrate is 4wt%, the concentration of ammonium phosphomolybdate is 3wt%, and the concentration of polyacrylonitrile is 10wt%;
[0080] Step b, injecting the spinning solution into a 5.0 mL syringe (the inner diameter of the needle is 0.4 mm) for electrostatic spinning, the distance between the nozzle and the aluminum foil is 15 cm, the spinning voltage is 14 kV, the spinning flow rate is 1.0 mL / h, the humidity is 35%, and the molybdenum phosphide solution is added to an ultrasonic sprayer, and molybdenum phosphide droplets are sprayed on the ejected nanofibers during the spinning process, and the spraying rate is 45 mL / h to obtain a nanofiber felt;
[0081] Wherein, the molybdenum phosphide solution is a mixed aqueous solution of 1.5 g / L molybdenum phosphide and 9 g / L sodium dodecylbenzene sulfonate;
[0082] Step c, heating the collected nanofiber felt in air at a rate of 1.0°C / min to 280°C, keeping the temperature for 1 hour, then introducing nitrogen, and heating the nanofiber felt at a rate of 3°C / min to 850°C, keeping the temperature for 2 hours, to obtain carbon nanofibers;
[0083] Step d, immersing the above-mentioned carbon nanofibers into 1.0M sodium hydroxide solution (solid-liquid ratio is 1g:25mL), immersing for 3h, and then activating at 950°C for 3h under an inert atmosphere, cooling to room temperature, immersing the activated carbon nanofibers into 1.0M hydrochloric acid solution (solid-liquid ratio is 1g:18mL), immersing for 2h, washing with deionized water until neutral, and drying in a vacuum drying oven at 120°C to obtain a non-precious metal-based carbon nanofiber electrode.
[0084] The SEM image of the nanofiber mat prepared in step b of this embodiment is as follows: Figure 1 As shown, the SEM image of the non-precious metal-based carbon nanofiber electrode prepared in step d is as follows Figure 2 As shown, after the heat treatment and activation treatment in step d, a carbon nanotube array branches out on the nanofiber trunk.
[0085] The non-precious metal-based carbon nanofiber electrode prepared in this example was used as the cathode, the copper electrode was used as the anode, and HgO was used as the reference electrode. Cyclic voltammetry curves were scanned in different concentrations of indigo aqueous solution (0.4 g / L, 0.6 g / L, 0.8 g / L, 1.0 g / L, and 1.2 g / L), with a scanning interval of 0 V to -1.5 V, a scanning direction from positive to negative, and a scanning speed of 0.01 V / s. The results are shown in Figure 2. Figure 3 shown.
[0086] As can be seen from the figure, during the forward scan, there is an oxidation peak at about -0.2V and -0.9V at different indigo concentrations. At -0.2V, the peak current reaches a peak value, forming an oxidation peak, and the oxidation peak current is 0.043A. During the negative scan, there is a reduction peak at -0.3V and -1.3V, and at -1.3V, the reduction peak current is 0.035A. This shows that the electrode system can reduce indigo to a leuco form, and shows higher oxidation peak current and reduction peak current as the dye concentration increases.
[0087] The non-precious metal-based carbon nanofiber electrode prepared above is used to construct an electrocatalytic hydrogenation reduction system for indigo dyeing:
[0088] An H-type electrolytic cell device was used, wherein the cathode was the non-precious metal-based carbon nanofiber electrode (1 cm*2 cm) prepared above, the anode was foam copper (1 cm*2 cm), the cathode electrolyte was 1.0 M NaOH solution and 0.5 g / L indigo dye (100 mL), the anolyte was 1.0 M H2SO4 solution (100 mL), and the diaphragm was a Nafion membrane. Nitrogen was first introduced for deoxygenation for 15 min, and then power was turned on for constant current reduction, the current density was 45 mA, and the reduction time was 35 min;
[0089] 5 g of cotton cloth was placed in cathode reducing solution for room temperature dyeing, and the dyeing was carried out for 1 min. The cloth was taken out and oxidized by ventilation for 5 min. The cloth was then washed with water at 50°C, and then washed with water in a soaping solution of 4 g / L soap powder and 3 g / L sodium carbonate at 95°C for 20 min. The cloth was then washed with water and dried to obtain dyed cotton cloth.
[0090] The cotton was dyed in exactly the same manner as above, except that the indigo dye concentration was replaced with 1.0 g / L.
[0091] Example 2
[0092] This embodiment provides a method for preparing a non-noble metal-based carbon nanofiber electrode, comprising the following steps:
[0093] Step a, adding terephthalic acid, copper sulfate, ferric nitrate, ammonium phosphomolybdate and polyacrylonitrile into N,N-dimethylformamide, stirring with a magnetic force at 60° C. until the mixture is uniformly dispersed, to obtain a spinning solution;
[0094] The concentration of terephthalic acid in the spinning solution is 5wt%, the concentration of copper sulfate is 3.5wt%, the concentration of iron nitrate is 5wt%, the concentration of ammonium phosphomolybdate is 4wt%, and the concentration of polyacrylonitrile is 12wt%;
[0095] Step b, injecting the spinning solution into a 5.0 mL syringe (the inner diameter of the needle is 0.4 mm) for electrostatic spinning, the distance between the nozzle and the aluminum foil is 13 cm, the spinning voltage is 12 kV, the spinning flow rate is 0.8 mL / h, the humidity is 45%, and the molybdenum phosphide solution is added to an ultrasonic sprayer, and molybdenum phosphide droplets are sprayed on the ejected nanofibers during the spinning process, and the spraying rate is 50 mL / h to obtain a nanofiber felt;
[0096] Wherein, the molybdenum phosphide solution is a mixed aqueous solution of 1.0 g / L molybdenum phosphide and 8 g / L sodium dodecylbenzene sulfonate;
[0097] Step c, heating the collected nanofiber felt in air at a rate of 0.8°C / min to 270°C, keeping the temperature for 1.5 hours, then introducing nitrogen, and heating the nanofiber felt at a rate of 2°C / min to 800°C, keeping the temperature for 2 hours, to obtain carbon nanofibers;
[0098] Step d, immersing the above-mentioned carbon nanofibers into 1.2M sodium hydroxide solution (solid-liquid ratio is 1g:20mL), immersing for 2.5h, and then activating at 900℃ for 3h under an inert atmosphere, cooling to room temperature, immersing the activated carbon nanofibers into 1.2M hydrochloric acid solution (solid-liquid ratio is 1g:15mL), immersing for 1.5h, washing with deionized water until neutral, and drying in a vacuum drying oven at 120℃ to obtain a non-precious metal-based carbon nanofiber electrode.
[0099] The non-precious metal-based carbon nanofiber electrode prepared above is used to construct an electrocatalytic hydrogenation reduction system for indigo dyeing:
[0100] An H-type electrolytic cell device was used, wherein the cathode was the non-precious metal-based carbon nanofiber electrode (1 cm*2 cm) prepared above, the anode was foam copper (1 cm*2 cm), the cathode electrolyte was 0.8 M NaOH solution and 1.0 g / L indigo dye (100 mL), the anolyte was 0.8 M H2SO4 solution (100 mL), and the diaphragm was a Nafion membrane. Nitrogen was first introduced for deoxygenation for 10 min, and then power was turned on for constant current reduction, the current density was 50 mA, and the reduction time was 30 min;
[0101] 5 g of cotton cloth was placed in cathode reducing solution for room temperature dyeing, immersed in dyeing for 1 min, taken out for ventilation oxidation for 5 min, then washed with water at 60°C, soaped in a soaping solution of 4 g / L soap powder and 3 g / L sodium carbonate at 95°C for 20 min, washed with water, and dried to obtain dyed cotton cloth.
[0102] Example 3
[0103] This embodiment provides a method for preparing a non-noble metal-based carbon nanofiber electrode, comprising the following steps:
[0104] Step a, adding terephthalic acid, copper sulfate, ferric nitrate, ammonium phosphomolybdate and polyacrylonitrile into N,N-dimethylformamide, stirring with a magnetic force at 60° C. until the mixture is uniformly dispersed, to obtain a spinning solution;
[0105] The concentration of terephthalic acid in the spinning solution is 4.5wt%, the concentration of copper sulfate is 4wt%, the concentration of iron nitrate is 4.5wt%, the concentration of ammonium phosphomolybdate is 2wt%, and the concentration of polyacrylonitrile is 11wt%;
[0106] Step b, injecting the spinning solution into a 5.0 mL syringe (the inner diameter of the needle is 0.4 mm) for electrostatic spinning, the distance between the nozzle and the aluminum foil is 12 cm, the spinning voltage is 13 kV, the spinning flow rate is 0.5 mL / h, the humidity is 40%, and the molybdenum phosphide solution is added to an ultrasonic sprayer, and molybdenum phosphide droplets are sprayed on the ejected nanofibers during the spinning process, and the spraying rate is 40 mL / h to obtain a nanofiber felt;
[0107] Wherein, the molybdenum phosphide solution is a mixed aqueous solution of 2g / L molybdenum phosphide and 10g / L sodium dodecylbenzene sulfonate;
[0108] Step c, heating the collected nanofiber felt in air at a rate of 0.5°C / min to 260°C, keeping the temperature for 2 hours, then introducing nitrogen, and heating the nanofiber felt at a rate of 5°C / min to 900°C, keeping the temperature for 1.5 hours, to obtain carbon nanofibers;
[0109] Step d, immersing the above-mentioned carbon nanofibers into 0.8M sodium hydroxide solution (solid-liquid ratio is 1g:30mL), immersing for 3.5h, and then activating at 1000℃ for 2.5h under an inert atmosphere, cooling to room temperature, immersing the activated carbon nanofibers into 0.8M hydrochloric acid solution (solid-liquid ratio is 1g:20mL), immersing for 2.5h, washing with deionized water until neutral, and drying in a vacuum drying oven at 120℃ to obtain a non-precious metal-based carbon nanofiber electrode.
[0110] The non-precious metal-based carbon nanofiber electrode prepared above is used to construct an electrocatalytic hydrogenation reduction system for indigo dyeing:
[0111] An H-type electrolytic cell device was used, wherein the cathode was the non-precious metal-based carbon nanofiber electrode (1 cm*2 cm) prepared above, the anode was foam copper (1 cm*2 cm), the cathode electrolyte was 1.2 M NaOH solution and 1.0 g / L indigo dye (100 mL), the anolyte was 1.2 M H2SO4 solution (100 mL), and the diaphragm was a Nafion membrane. Nitrogen was first introduced for deoxygenation for 13 min, and then power was turned on for constant current reduction, the current density was 40 mA, and the reduction time was 40 min;
[0112] 5 g of cotton cloth was placed in cathode reducing solution for room temperature dyeing, and the dyeing was carried out for 1 min. The cloth was taken out and oxidized by ventilation for 5 min. The cloth was then washed with water at 55°C, and then washed with water in a soaping solution of 4 g / L soap powder and 3 g / L sodium carbonate at 95°C for 20 min. The cloth was then washed with water and dried to obtain dyed cotton cloth.
[0113] Comparative Example 1
[0114] This comparative example provides a method for preparing a non-precious metal-based carbon nanofiber electrode. The preparation steps and parameters are exactly the same as those in Example 1, except that ammonium phosphomolybdate is not added to the spinning solution, and the rest are exactly the same.
[0115] In exactly the same manner as in Example 1, the prepared non-noble metal-based carbon nanofiber electrode was used to construct an electrocatalytic hydrogenation reduction system for indigo dyeing, and the concentration of the reduced indigo dye was 0.5 g / L.
[0116] Comparative Example 2
[0117] This comparative example provides a method for preparing a non-precious metal-based carbon nanofiber electrode. The preparation steps and parameters are exactly the same as those in Example 1, except that copper sulfate is not added to the spinning solution, and the rest are exactly the same.
[0118] In exactly the same manner as in Example 1, the prepared non-noble metal-based carbon nanofiber electrode was used to construct an electrocatalytic hydrogenation reduction system for indigo dyeing, and the concentration of the reduced indigo dye was 0.5 g / L.
[0119] Comparative Example 3
[0120] This comparative example provides a method for preparing a non-precious metal-based carbon nanofiber electrode. The preparation steps and parameters are exactly the same as those in Example 1, except that an ultrasonic spray humidifier is not used to spray MoP droplets throughout the spinning solution, and the rest are exactly the same.
[0121] In exactly the same manner as in Example 1, the prepared non-noble metal-based carbon nanofiber electrode was used to construct an electrocatalytic hydrogenation reduction system for indigo dyeing, and the concentration of the reduced indigo dye was 1.0 g / L.
[0122] Comparative Example 4
[0123] This comparative example provides a method for preparing a non-precious metal-based carbon nanofiber electrode. The preparation steps and parameters are exactly the same as those in Example 1, except that an ultrasonic spray humidifier is not used to spray MoP droplets throughout the spinning solution, but MoP is dispersed in the spinning solution of step a for electrostatic spinning.
[0124] By comparing the mass of the nanofiber felt prepared in step b of Example 1 and Comparative Example 3 after drying, it can be obtained that the mass of MoP sprayed during electrospinning for 5 hours accounts for 60% of the total mass of the spinning solution. When this mass content of MoP is dispersed in the spinning solution for spinning, it is found that the spinneret holes are blocked and cannot be drawn into fibers.
[0125] Comparative Example 5
[0126] After many attempts, it was found that if MoP is dispersed in the spinning solution for electrospinning, the maximum content can only reach 20wt%.
[0127] This comparative example provides a method for preparing a non-precious metal-based carbon nanofiber electrode. The preparation steps and parameters are exactly the same as those in Example 1, except that an ultrasonic spray humidifier is not used to spray MoP droplets throughout the spinning solution. Instead, 20 wt% of MoP is dispersed in the spinning solution of step a for electrospinning.
[0128] In exactly the same manner as in Example 1, the prepared non-noble metal-based carbon nanofiber electrode was used to construct an electrocatalytic hydrogenation reduction system for indigo dyeing, and the concentration of the reduced indigo dye was 1.0 g / L.
[0129] Comparative Example 6
[0130] This comparative example provides a method for preparing a non-precious metal-based carbon nanofiber electrode. The preparation steps and parameters are exactly the same as those in Example 1, except that ammonium phosphomolybdate is replaced by trimethylolmelamine, and the rest are exactly the same.
[0131] In exactly the same manner as in Example 1, the prepared non-noble metal-based carbon nanofiber electrode was used to construct an electrocatalytic hydrogenation reduction system for indigo dyeing, and the concentration of the reduced indigo dye was 1.0 g / L.
[0132] Comparative Example 7
[0133] This comparative example provides a method for preparing a non-precious metal-based carbon nanofiber electrode. The preparation steps and parameters are exactly the same as those in Example 1, except that terephthalic acid is not added to the spinning solution, and the rest are exactly the same.
[0134] The photos of the non-noble metal-based carbon nanofiber electrode prepared in step d of this comparative example and Example 1 are as follows Figure 4 As shown in the figure, it can be seen that if terephthalic acid is not added to the spinning solution, a self-supporting structure cannot be achieved, that is, the prepared carbon nanofibers cannot be used as electrodes in electrocatalytic hydrogenation reduction.
[0135] The cotton fabrics obtained by dyeing in Example 1 and Comparative Examples 1-6 were tested for dyeing performance, and the results are shown in Tables 1 and 2.
[0136] Table 1
[0137]
[0138] Table 2
[0139]
[0140]
[0141] As can be seen from the above table, the non-precious metal-based carbon nanofiber electrode prepared in the embodiment of the present invention can effectively improve the electrochemical reduction rate of indigo dye, increase the dyeing depth, and significantly improve the friction fastness after dyeing. In addition to being suitable for indigo dye, the non-precious metal-based carbon nanofiber electrode provided by the present invention is also suitable for other reducing dyes, and can achieve multiple cycles of dyeing, significantly improving the dyeing effect.
[0142] The cotton fabrics obtained by dyeing in Examples 2-3 of the present invention were subjected to dyeing performance tests, and the indigo reduction rate was more than 90%, the K / S value was 9.5-10.2, the dry rubbing fastness was 4-5, the wet rubbing fastness was 3-4, the washing staining / discoloration fastness was 4, and when the reduction dye solution was recycled for 10 times, the K / S value change rate of the dyed fabric sample was 3.0%-3.5%.
[0143] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a non-precious metal-based carbon nanofiber electrode, characterized in that: The steps include: Step a, adding terephthalic acid, soluble copper salt, soluble iron salt, phosphomolybdate and polyacrylonitrile into N,N-dimethylformamide and dispersing them evenly to obtain a spinning solution; Step b, injecting the spinning solution into an electrospinning device for electrospinning, and spraying molybdenum phosphide droplets on the ejected nanofibers during the entire spinning process to obtain a nanofiber felt; Step c, pre-oxidizing the nanofiber felt at 260° C.-280° C. in an air atmosphere, and then carbonizing the nanofiber felt at 800° C.-900° C. in an inert atmosphere to obtain carbon nanofibers; Step d, immersing the carbon nanofibers into a strong alkaline solution, then activating them at 900°C-1000°C under an inert atmosphere, cooling them, immersing the activated carbon nanofibers into a strong acid solution, washing them, and drying them to obtain a non-precious metal-based carbon nanofiber electrode.
2. The method for preparing a non-noble metal-based carbon nanofiber electrode according to claim 1, characterized in that: In step a, the soluble copper salt is copper chloride, copper nitrate or copper sulfate; and / or In step a, the soluble iron salt is ferric chloride, ferric nitrate or ferric sulfate; and / or In step a, the phosphomolybdate is ammonium phosphomolybdate; and / or In step a, the mass concentration of terephthalic acid in the electrospinning dispersion is 4%-5%, the mass concentration of soluble copper salt is 3%-4%, the mass concentration of soluble iron salt is 4%-5%, the mass concentration of phosphomolybdate is 2%-4%, and the mass concentration of polyacrylonitrile is 10%-12%.
3. The method for preparing the non-noble metal-based carbon nanofiber electrode according to claim 1, characterized in that: In step b, the electrospinning parameters are: the distance between the nozzle and the aluminum foil is 12 cm-15 cm, the spinning voltage is 12 kV-14 kV, the spinning flow rate is 0.5 mL / h-1.0 mL / h, and the humidity is 35%-45%; and / or In step b, the molybdenum phosphide solution is passed through an ultrasonic spray humidifier to form molybdenum phosphide droplets and sprayed onto the nanofibers; the molybdenum phosphide solution is a mixed aqueous solution of molybdenum phosphide and sodium dodecylbenzene sulfonate, wherein the concentration of molybdenum phosphide is 1g / L-2g / L, and the concentration of sodium dodecylbenzene sulfonate is 8g / L-10g / L; and / or In step b, the speed of spraying molybdenum phosphide droplets is 40mL / h-50mL / h.
4. The method for preparing a non-noble metal-based carbon nanofiber electrode according to claim 1, characterized in that: In step c, the pre-oxidation time is 1h-2h; and / or In step c, the temperature is raised to 260°C-280°C in a programmed temperature-raising manner at a heating rate of 0.5°C / min-1.0°C / min; In step c, the carbonization time is 1.5h-2h; and / or In step c, the temperature is raised to 800°C-900°C in a programmed temperature raising manner at a heating rate of 2°C / min-5°C / min.
5. The method for preparing a non-noble metal-based carbon nanofiber electrode according to claim 1, characterized in that: In step d, the activation time is 2.5h-3h; and / or In step d, the strong alkaline solution is a 0.8 mol / L-1.2 mol / L sodium hydroxide solution, and the volume mass ratio of the strong alkaline solution to the carbon nanofiber is 20-30:1, wherein the unit of mass is gram and the unit of volume is milliliter; and / or In step d, the immersion time in the strong alkaline solution is 2.5h-3.5h; and / or In step d, the strong acid solution is a 0.8 mol / L-1.2 mol / L hydrochloric acid solution, and the volume mass ratio of the strong acid solution to the activated carbon nanofibers is 15-20:1, wherein the unit of mass is gram and the unit of volume is milliliter; and / or In step d, the immersion time in the strong acid solution is 1.5h-2.5h.
6. A non-precious metal-based carbon nanofiber electrode, characterized in that: The non-precious metal-based carbon nanofiber electrode is prepared by the preparation method of any one of claims 1 to 5.
7. Use of the non-noble metal-based carbon nanofiber electrode according to claim 6 in electrochemical dyeing of reduced dyes.
8. An electrochemical dyeing process, characterized in that: The non-noble metal-based carbon nanofiber electrode according to claim 6 is used as a cathode to dye fiber fabrics by electrochemical dye reduction under alkaline conditions.
9. The electrochemical dyeing process according to claim 8, characterized in that: The initial concentration of the vat dye is 0.5 g / L-1.0 g / L; and / or The cathode electrolyte is a 0.8 mol / L-1.2 mol / L sodium hydroxide solution; and / or The anode electrode liquid is a 0.8 mol / L-1.2 mol / L sulfuric acid solution; and / or The anode is a copper sheet or a foam copper electrode.
10. A fiber fabric, characterized in that: The product is prepared by the electrochemical dyeing process described in claim 8 or 9.