Preparation method and application of N-oxidized pyridylnaphthalimide coordination polymer

By preparing N-oxypyridylnaphthalimide coordination polymer, the problems of low solar energy utilization efficiency and poor catalyst stability of existing photocatalytic materials are solved, and the effect of efficient degradation of organic pollutants is achieved, with good Chemical stability and photothermal stability.

CN118580513BActive Publication Date: 2024-10-22QUJING NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410847862.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-22
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing photocatalytic materials, such as titanium dioxide and zinc oxide, cannot effectively utilize sunlight energy, and are prone to carbon deposition during the catalytic process, leading to deactivation. It is difficult to develop materials with good stability, stable chemical properties, low cost and easy availability, and a wider range of photoresponse. Broad photocatalyst.

Method used

A kind of N-oxypyridyl naphthalimide coordination polymer is prepared by using N,N'-bis(4-N″-oxypyridyl)-1,4,5,8-naphthalene diimide and tris-naphthalenedimide. Europium chloride and phosphomolybdic acid react in a solvent to form a one-dimensional organic framework material for photocatalytic degradation of organic pollutants methyl blue and rhodamine B.

Benefits of technology

This coordination polymer has high quantum efficiency, high conversion rate, high catalytic activity and high chemical stability under visible light irradiation, can quickly degrade methyl blue and rhodamine B, has a wide light response range and is reusable. The preparation method is simple and low-cost, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118580513B_ABST
    Figure CN118580513B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an N-oxidized pyridyl naphthalimide coordination polymer and its application, and belongs to the technical field of photocatalytic material preparation. The preparation method of the N-oxidized pyridyl naphthalimide coordination polymer of the invention comprises the following steps: dissolving N,N'-di(4-N"-oxidized pyridyl)-1,4,5,8-naphthalene diimide, europium trichloride and phosphomolybdic acid in a solvent, reacting to obtain the N-oxidized pyridyl naphthalimide coordination polymer. The invention provides a preparation method of an N-oxidized pyridyl naphthalimide coordination polymer and its application in the photocatalytic degradation of organic pollutants methyl blue and rhodamine B. The coordination polymer can be used for catalytic degradation of organic pollutants methyl blue and rhodamine B in the environment under the irradiation of visible light, and has the characteristics of short degradation time, high degradation efficiency, wider light response range, and reusability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photocatalytic material preparation, and in particular to a preparation method and application of an N-oxide pyridylnaphthalimide coordination polymer. Background Art

[0002] Photocatalytic redox technology has a wide range of applications in organic conversion, environmental protection and new material development. The key to photocatalytic technology lies in the development of photocatalytic materials. Most of the current research on photocatalytic technology is mainly carried out around titanium dioxide and zinc oxide. However, due to the band gap of titanium dioxide being 3.2eV, it can only absorb ultraviolet light below 387.5nm and has no response to visible light. Zinc oxide also has similar properties, which greatly limits the utilization of sunlight energy. Therefore, in order to improve the efficiency of photocatalysis, further improvements are urgently needed.

[0003] For example, carbon-rich materials with good conductivity, such as carbon nanotubes, activated carbon, and graphene, are combined with semiconductor photocatalytic materials such as titanium dioxide and zinc oxide. Carbon-rich materials can act as electron acceptors, and rely on the high carrier mobility of carbon-rich materials to quickly migrate excited electrons to carbon-rich materials to improve electron migration ability, rather than accumulating on the surface of semiconductor photocatalytic materials, thereby effectively suppressing the recombination probability of photogenerated electrons and holes, accelerating the separation of photogenerated electron-hole pairs, and improving the photon efficiency. Although these studies have improved the quantum efficiency and catalytic stability of specific photocatalytic reactions, the results still have room for further improvement. Moreover, during the catalytic process, carbon deposition on the surface of photocatalysts such as titanium dioxide and zinc oxide is prone to catalyst inactivation. Therefore, it is very necessary to develop photocatalysts with good stability, stable chemical properties, low cost and easy availability, and a wider light response range.

[0004] In recent years, more and more researchers have shifted the research focus of photocatalytic materials from pure inorganic semiconductor materials to coordination polymers, because coordination polymers have unique performance advantages such as a wide variety, rich structures, regular pore structures, and adjustable pore sizes. Coordination polymers based on dye molecules are a type of complex formed by the coordination of organic dye molecules with strong visible light absorption and metal ions. They have attracted attention due to their tunable photoelectric properties, active sites, and large specific surface area. In addition to applications in solar cells, chemical sensors, lithium-ion batteries, etc., their application potential in photocatalysis has also been explored. However, there are still many difficulties in obtaining coordination polymer photocatalytic materials that are chemically stable, cheap and easy to obtain, have a wider light response range, and have high catalytic activity. Summary of the invention

[0005] The purpose of the present invention is to provide a preparation method of N-oxidized pyridyl naphthalimide coordination polymer and its application to solve the above-mentioned problems in the background technology. The present invention provides a preparation method of N-oxidized pyridyl naphthalimide coordination polymer and its application in photocatalytic degradation of organic pollutants methyl blue and rhodamine B. The coordination polymer can be used for catalytic degradation of organic pollutants methyl blue and rhodamine B in the environment under the irradiation of visible light, and has the characteristics of short degradation time, high degradation efficiency, wider light response range, and reusability.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention is to provide an N-oxidized pyridyl naphthalimide coordination polymer, wherein the chemical formula of the N-oxidized pyridyl naphthalimide coordination polymer is C 80 H 62 N 14 O 102 P2Mo 22 Eu2; the N-oxypyridylnaphthalene diimide coordination polymer belongs to the monoclinic system, the space group is C2 / c, the unit cell parameter α=90°, β=106.351(9)°, γ=90°.

[0008] The second technical solution of the present invention is to provide a method for preparing the above-mentioned N-oxidized pyridylnaphthalimide coordination polymer, comprising the following steps:

[0009] N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide, europium trichloride and phosphomolybdic acid are dissolved in a solvent and reacted to obtain the N-oxypyridyl naphthalene diimide coordination polymer (N-oxypyridyl naphthalene diimide coordination polymer).

[0010] The N-oxypyridyl naphthalene diimide coordination polymer of the invention is a one-dimensional organic framework material formed by coordination of nitrogen oxide, phosphomolybdate ion and europium ion on N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide.

[0011] The structural formula of N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide in the N-oxypyridyl naphthalene diimide coordination polymer is as follows:

[0012]

[0013] Preferably, the molar ratio of the N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide, europium trichloride and phosphomolybdic acid is 1:5:2 to 1:5:4.

[0014] Preferably, the solvent comprises a mixed solution of N,N-dimethylacetamide and water.

[0015] More preferably, the volume ratio of N,N-dimethylacetamide to water is 1:3.

[0016] Preferably, the reaction temperature is 95-105° C. and the reaction time is 24-48 hours.

[0017] The third technical solution of the present invention is to provide an application of the above-mentioned N-oxide pyridylnaphthalimide coordination polymer in the photocatalytic degradation of organic pollutants in water.

[0018] Preferably, the organic pollutants include methyl blue and rhodamine B.

[0019] Preferably, the excitation light wavelength range of the photocatalytic step is 400-750 nm.

[0020] Preferably, the photocatalytic excitation light source includes natural light source and artificial light source.

[0021] The beneficial technical effects of the present invention are as follows:

[0022] The preparation method of the invention has low requirements on synthesis equipment, is simple and convenient to operate, has low cost, short preparation time, can be mass-produced, and the prepared N-oxidized pyridylnaphthalene diimide coordination polymer has high crystallinity and good appearance.

[0023] The N-oxidized pyridylnaphthalene diimide coordination polymer of the present invention has good photothermal stability of the main structure and can withstand a temperature of up to 250° C. The product prepared by the present invention has the characteristics of high quantum efficiency, high conversion rate, high catalytic activity and high chemical stability as a photocatalyst, has extremely high degradation efficiency for environmental pollutants methyl blue and rhodamine B, and has good practical value and application prospects.

[0024] The present invention provides a preparation method of an N-oxide pyridylnaphthalene diimide coordination polymer and its application in photocatalytic degradation of organic pollutants methyl blue and rhodamine B. The coordination polymer can be used for catalytic degradation of organic pollutants methyl blue and rhodamine B in the environment under the irradiation of visible light, and has the characteristics of short degradation time, high degradation efficiency, wider light response range, reusability, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 This is the X-ray single crystal structure of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0027] Figure 2 This is a three-dimensional structure diagram of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0028] Figure 3 This is a thermogravimetric curve of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0029] Figure 4 This is the XRD pattern of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0030] Figure 5 This is the UV-visible spectrum of the photocatalytic degradation of methyl blue by the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0031] Figure 6 This is the UV-visible spectrum of the photocatalytic degradation of Rhodamine B by the N-oxide pyridylnaphthalene diimide coordination polymer prepared in Example 1.

[0032] Figure 7 This is the XRD pattern of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2.

[0033] Figure 8 This is the UV-visible spectrum of the photocatalytic degradation of methyl blue by the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2.

[0034] Fig. 9 This is the UV-visible spectrum of the photocatalytic degradation of Rhodamine B by the N-oxide pyridylnaphthalene diimide coordination polymer prepared in Example 2.

[0035] Fig.10 This is a graph showing the cyclic degradation rate of methyl blue by photocatalytic degradation of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2.

[0036] Fig.11 This is a graph showing the cyclic degradation rate of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2 for photocatalytic degradation of rhodamine B.

[0037] Fig.12 This is the XRD spectrum of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2 before and after cycling.

[0038] Fig.13 This is the UV-visible spectrum of the photocatalytic degradation of Rhodamine B using N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide in Comparative Example 1.

[0039] Fig.14 This is the UV-visible spectrum of the photocatalytic degradation of Rhodamine B using phosphomolybdic acid in Comparative Example 2. DETAILED DESCRIPTION

[0040] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0041] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0042] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0043] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.

[0044] Unless otherwise specified, the "room temperature" in the present invention is 20-30°C.

[0045] The N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide, europium trichloride, phosphomolybdic acid and N,N-dimethylacetamide used in the present invention are commercially available analytical reagents without further purification.

[0046] Example 1

[0047] Preparation of N-Oxypyridylnaphthalene diimide coordination polymer:

[0048] 0.10mmol of N,N'-bis(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide, 0.50mmol of europium trichloride and 0.20mmol of phosphomolybdic acid were added to a mixed solution containing 1mL of N,N-dimethylacetamide and 3mL of water, stirred for 10min at room temperature and air atmosphere to make it evenly dispersed, then transferred to a 25mL Teflon autoclave, heated to 95°C and reacted at a constant temperature for 48h. After the reaction was completed, it was cooled to room temperature at a cooling rate of 10°C / h, and then the obtained precipitate was washed with water to obtain yellow-green crystals. After grinding to pass a 300-mesh sieve, N-oxypyridyl naphthalene diimide coordination polymer was obtained with a yield of about 63% (calculated based on N,N'-bis(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide).

[0049] The X-ray single crystal structure and three-dimensional structure of the N-oxypyridylnaphthalene diimide coordination polymer prepared in this example are shown in Figure 1 and Figure 2 .

[0050] Figure 1 This is the X-ray single crystal structure of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0051] Figure 2 This is a three-dimensional structure diagram of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0052] from Figure 1 It can be seen that the europium atom adopts an octagonal tetragonal anti-prism configuration, coordinated with two N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide ligands, two water molecules and a single vacant Keggin-type phosphomolybdic acid anion. Figure 2 It can be seen that the vacant phosphomolybdic acid anion and the europium ion are connected to each other through N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide to form a one-dimensional chain structure, and then the chain structure is further connected into a three-dimensional structure by the weak interaction force between the phosphomolybdic acid anion and the naphthalene diimide ligand (lone pair electron-π and anion-π interaction).

[0053] The thermal stability of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in this example was characterized by a thermogravimetric analysis experiment. Specifically, the temperature was raised at a heating rate of 10°C / min under a nitrogen purge to measure the thermal gravimetric curve of the N-oxide pyridyl naphthalene diimide coordination polymer. The results are shown in FIG. Figure 3 .

[0054] Figure 3 This is a thermogravimetric curve of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0055] from Figure 3 It can be seen that the product loses about 2.8% of its weight in the temperature range from room temperature to 100°C, indicating that the prepared coordination polymer product contains a small amount of solvent molecules. After the solvent molecules evaporate, the product has almost no weight loss at 100-250°C, indicating that the product can exist stably in this temperature range and has good thermal stability. In the range of 250-800°C, the product loses weight rapidly, indicating that the product begins to decompose.

[0056] The N-oxypyridylnaphthalene diimide coordination polymer prepared in this example was subjected to XRD analysis, and the results are shown in FIG. Figure 4 .

[0057] Figure 4 This is the XRD pattern of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0058] from Figure 4 It can be seen that the characteristic peaks of the XRD spectrum of the coordination polymer are consistent with the characteristic peaks of the theoretical simulation, indicating that the structure of the synthesized N-oxide pyridyl naphthalene diimide coordination polymer is consistent with the simulated structure, with high crystallinity and no obvious impurity phase.

[0059] The X-ray single crystal diffraction data of the N-oxide pyridylnaphthalene diimide coordination polymer prepared in Example 1 are shown in Table 1.

[0060] Table 1 X-ray single crystal diffraction data

[0061]

[0062]

[0063] Application Example 1

[0064] Example 1 Photocatalytic degradation of methyl blue test product

[0065] Weigh 50 mg of the N-oxypyridylnaphthalene diimide coordination polymer prepared in Example 1 and add it to a 100 mL quartz reaction container, then add 10 -550 mL of 1.5 mol / L methyl blue solution was stirred continuously for 2 hours in a dark environment to allow the catalyst (N-oxypyridyl naphthalene diimide coordination polymer) and methyl blue molecules to reach adsorption-desorption equilibrium. The reaction vessel was then placed under a 300W xenon lamp (wavelength range 400-750nm) with a filter and stirred continuously. During the experiment, 5 mL of solution was taken out from the reaction vessel every 5 minutes. After centrifugation to separate the photocatalyst, it was placed in a UV-visible spectrometer to test the concentration change of methyl blue, which was used to represent the degradation process of methyl blue. The change of its UV-visible spectrum with the illumination time is shown in Figure 2. Figure 5 shown.

[0066] Figure 5 This is the UV-visible spectrum of the photocatalytic degradation of methyl blue by the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 1.

[0067] from Figure 5 It can be seen that the absorbance of methylene blue decreases rapidly with the increase of illumination time, indicating that methylene blue is rapidly decomposed under the action of the catalyst. Within 30 minutes, its degradation rate can reach 88.6%; within 45 minutes, methylene blue can be basically completely degraded, with a degradation rate of 98.4%. In this case, the originally blue methylene blue solution becomes a colorless solution.

[0068] Application Example 2

[0069] Example 1 Photocatalytic degradation of Rhodamine B test product

[0070] Weigh 50 mg of the N-oxypyridylnaphthalene diimide coordination polymer prepared in Example 1 and add it to a 100 mL quartz reaction container, then add 10 -5 50 mL of 1.5 mol / L Rhodamine B solution was stirred continuously for 2 hours in a dark environment to allow the catalyst (N-oxypyridyl naphthalene diimide coordination polymer) and the Rhodamine B molecules to reach adsorption-desorption equilibrium. The reaction vessel was then placed under a 300W xenon lamp (wavelength range 400-750nm) with a filter and stirred continuously. During the experiment, 5 mL of solution was taken out from the reaction vessel every 3 minutes. After centrifugation to separate the photocatalyst, it was placed in a UV-visible spectrometer to test the concentration change of Rhodamine B, which was used to represent the degradation process of Rhodamine B. The changes in its UV-visible spectrum with illumination time are shown in Figure 2. Figure 6 shown.

[0071] Figure 6 This is the UV-visible spectrum of the photocatalytic degradation of Rhodamine B by the N-oxide pyridylnaphthalene diimide coordination polymer prepared in Example 1.

[0072] from Figure 6It can be seen that the absorbance of Rhodamine B decreases rapidly with the increase of illumination time, indicating that Rhodamine B is rapidly decomposed under the action of the catalyst. Within 12 minutes, its degradation rate can reach more than 94.2%, and within 27 minutes, Rhodamine B can be completely degraded with a degradation rate of 99.2%. In this case, the originally red methylrhodamine B solution becomes a colorless solution.

[0073] Example 2

[0074] Preparation of N-Oxypyridylnaphthalene diimide coordination polymer:

[0075] 0.20mmol of N,N'-bis(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide, 1.0mmol of europium trichloride and 0.80mmol of phosphomolybdic acid were added to a mixed solution containing 3mL of N,N-dimethylacetamide and 9mL of water, stirred for 10min at room temperature and air atmosphere to make it evenly dispersed, then transferred to a 25mL Teflon autoclave, heated to 105℃ and reacted at constant temperature for 48h. After the reaction was completed, it was cooled to room temperature at a cooling rate of 10℃ / h, and then the obtained precipitate was washed with water to obtain yellow-green crystals. After grinding to pass a 300-mesh sieve, N-oxypyridyl naphthalene diimide coordination polymer was obtained with a yield of about 59% (calculated based on N,N'-bis(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide).

[0076] Figure 7 This is the XRD pattern of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2.

[0077] from Figure 7 It can be seen that the characteristic peaks of the XRD spectrum of the coordination polymer are consistent with the characteristic peaks of the theoretical simulation, indicating that the structure of the synthesized N-oxide pyridyl naphthalene diimide coordination polymer is consistent with the simulated structure, with high crystallinity and no obvious impurity phase.

[0078] Application Example 3

[0079] Example 2 Photocatalytic degradation of methyl blue test product

[0080] Weigh 100 mg of the N-oxypyridylnaphthalene diimide coordination polymer prepared in Example 2 and add it to a 250 mL quartz reaction container, then add 10 -5100mL of 1 mol / L methyl blue solution was stirred continuously for 2 hours in a dark environment to allow the catalyst (N-oxypyridyl naphthalene diimide coordination polymer) and methyl blue molecules to reach adsorption-desorption equilibrium. The reaction vessel was then placed under a 300W xenon lamp (wavelength range 400-750nm) with a filter and stirred continuously. During the experiment, 5mL of solution was taken out from the reaction vessel every 5 minutes. After centrifugation to separate the photocatalyst, it was placed in a UV-visible spectrometer to test the concentration change of methyl blue, which was used to represent the degradation process of methyl blue. The change of its UV-visible spectrum with the illumination time is shown in Figure 8 shown.

[0081] Figure 8 This is the UV-visible spectrum of the photocatalytic degradation of methyl blue by the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2.

[0082] from Figure 8 It can be seen that the absorbance of methylene blue decreases rapidly with the increase of illumination time, indicating that methylene blue is rapidly decomposed under the action of the catalyst. Within 30 minutes, the degradation rate reaches 86.3%. Within 45 minutes, methylene blue can be basically completely decomposed, with a degradation rate of 97.9%. In this case, the originally blue methylene blue solution becomes a colorless solution.

[0083] Application Example 4

[0084] Example 2 Photocatalytic degradation of Rhodamine B test product

[0085] Weigh 100 mg of the N-oxypyridylnaphthalene diimide coordination polymer prepared in Example 2 and add it to a 250 mL quartz reaction container, then add 10 -5 100mL of 1 mol / L Rhodamine B solution was stirred continuously for 2 hours in a dark environment to allow the catalyst (N-oxypyridyl naphthalene diimide coordination polymer) and the Rhodamine B molecules to reach adsorption-desorption equilibrium. The reaction vessel was then placed under a 300W xenon lamp (wavelength range 400-750nm) with a filter and stirred continuously. During the experiment, 5mL of solution was taken out from the reaction vessel every 3 minutes. After centrifugation to separate the photocatalyst, it was placed in a UV-visible spectrometer to test the concentration change of Rhodamine B, which was used to represent the degradation process of Rhodamine B. The changes in its UV-visible spectrum with illumination time are shown in Figure 2. Fig. 9 shown.

[0086] Fig. 9 This is the UV-visible spectrum of the photocatalytic degradation of Rhodamine B by the N-oxide pyridylnaphthalene diimide coordination polymer prepared in Example 2.

[0087] from Fig. 9It can be seen that the absorbance of Rhodamine B decreases rapidly with the increase of illumination time, indicating that Rhodamine B is rapidly decomposed under the action of the catalyst. Within 12 minutes, the degradation rate can reach 93.5%, and within 27 minutes, Rhodamine B can be completely degraded to 99.2%. In this case, the originally red methyl Rhodamine B solution becomes a colorless solution.

[0088] Application Example 5

[0089] To further demonstrate the chemical stability and photocatalytic stability of the coordination polymer prepared by the present invention, the products after the photocatalytic experiments of Application Examples 3 and 4 were centrifuged and recovered. The recovered photocatalysts were washed with water and dried at room temperature, and then three rounds of photocatalytic experiments were carried out under the same experimental conditions as Application Examples 3 and 4. The degradation rates of methyl blue and rhodamine B after each cycle were calculated, and the results are shown in FIG. Fig.10 and 11 shown.

[0090] Fig.10 This is a graph showing the cyclic degradation rate of methyl blue by photocatalytic degradation of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2.

[0091] Fig.11 This is a graph showing the cyclic degradation rate of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2 for photocatalytic degradation of rhodamine B.

[0092] from Fig.10 and 11 It can be seen that the catalytic performance of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2 is not significantly weakened after three cycles of use, indicating that the N-oxide pyridyl naphthalene diimide coordination polymer has good photocatalytic stability.

[0093] The XRD characterization of the N-oxidized pyridylnaphthalene diimide coordination polymer after three cycles of photocatalytic degradation of rhodamine B was carried out. Fig.12 .

[0094] Fig.12 This is the XRD spectrum of the N-oxide pyridyl naphthalene diimide coordination polymer prepared in Example 2 before and after cycling.

[0095] from Fig.12 It can be seen that the XRD spectra after three photocatalytic cycles are similar to those of the simulated and unphotocatalytic experiments. Figure 1 This indicates that the structure of the polymer has not changed and has good photothermal stability.

[0096] Comparative Example 1

[0097] The only difference from Application Example 2 is that the N-oxypyridyl naphthalene diimide coordination polymer prepared in Example 2 is replaced with an equal mass of N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide, and then the photocatalytic performance test is continued.

[0098] The structural formula of N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide is as follows:

[0099]

[0100] Specifically:

[0101] Weigh 50 mg of N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide prepared in Example 1 and add it to a 100 mL quartz reaction container, then add 10 -5 50 mL of 1.5 mol / L Rhodamine B solution was stirred continuously for 2 hours in a dark environment to allow the catalyst (N-oxypyridyl naphthalene diimide coordination polymer) and the Rhodamine B molecules to reach adsorption-desorption equilibrium. The reaction vessel was then placed under a 300W xenon lamp (wavelength range 400-750nm) with a filter and stirred continuously. During the experiment, 5 mL of solution was taken out from the reaction vessel every 3 minutes. After centrifugation to separate the photocatalyst, it was placed in a UV-visible spectrometer to test the concentration change of Rhodamine B, which was used to represent the degradation process of Rhodamine B. The changes in its UV-visible spectrum with illumination time are shown in Figure 2. Fig.13 shown.

[0102] Fig.13 This is the UV-visible spectrum of the photocatalytic degradation of Rhodamine B using N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide in Comparative Example 1.

[0103] from Fig.13 It can be seen that the absorbance of Rhodamine B does not change significantly with the increase of illumination time, indicating that the efficiency of the catalyst used in this comparative example in catalyzing the degradation of Rhodamine B is significantly lower than that of the N-oxypyridylnaphthalene diimide coordination polymer prepared in Example 2, indicating that the coordination of N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide with europium ions and phosphomolybdic acid can significantly improve its catalytic activity.

[0104] Comparative Example 2

[0105] The only difference from Application Example 2 is that the N-oxypyridylnaphthalene diimide coordination polymer prepared in Example 2 is replaced with an equal mass of phosphomolybdic acid, and then the photocatalytic performance test is continued. Fig.14 shown.

[0106] Fig.14 This is the UV-visible spectrum of the photocatalytic degradation of Rhodamine B using phosphomolybdic acid in Comparative Example 2.

[0107] from Fig.14 It can be seen that the absorbance of Rhodamine B does not change significantly with the increase of illumination time, indicating that the efficiency of the catalyst (phosphomolybdic acid) used in this comparative example in catalyzing the degradation of Rhodamine B is significantly lower than that of the N-oxidized pyridylnaphthalene diimide coordination polymer prepared in Example 2.

[0108] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A N-oxide pyridylnaphthalimide coordination polymer, characterized in that: The chemical formula of the N-oxidized pyridylnaphthalimide coordination polymer is C 80 H 62 N 14 O 102 P2Mo 22 Eu2; the N-oxidized pyridylnaphthalimide coordination polymer belongs to the monoclinic system, the space group is C2 / c, the unit cell parameter α=90°, β=106.351(9)°, γ=90°.

2. A method for preparing the N-oxide pyridylnaphthalimide coordination polymer according to claim 1, characterized in that: The following steps are involved: N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide, europium trichloride and phosphomolybdic acid are dissolved in a solvent and reacted to obtain the N-oxypyridyl naphthalene diimide coordination polymer.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the N,N'-di(4-N"-oxypyridyl)-1,4,5,8-naphthalene diimide, europium trichloride and phosphomolybdic acid is 1:5:2 to 1:5:

4.

4. The preparation method according to claim 2, characterized in that: The solvent includes a mixed solution of N,N-dimethylacetamide and water.

5. The preparation method according to claim 4, characterized in that: The volume ratio of the N,N-dimethylacetamide to water is 1:

3.

6. The preparation method according to claim 2, characterized in that: The reaction temperature is 95-105° C. and the reaction time is 24-48 hours.

7. Use of the N-oxide pyridylnaphthalimide coordination polymer according to claim 1 in photocatalytic degradation of organic pollutants in water.

8. The use according to claim 7, characterized in that: The organic pollutants include methyl blue and rhodamine B.

9. The use according to claim 7, characterized in that: The excitation light wavelength range of the photocatalytic step is 400-750nm.