Perovskite cell passivation layer deposition method and perovskite cell
By forming a passivation layer on the filter paper and forming a double passivation layer structure in the perovskite solar cell, the problems of waste of raw materials and high costs in the prior art are solved, and the deposition of the high-efficiency passivation layer is achieved, and the pertitanium is improved Performance and stability of mine solar cells.
Patent Information
- Application Number
- CN202411212181.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-26
AI Technical Summary
The existing passivation layer preparation process has problems of raw material waste, high cost and equipment complexity, which limits the performance improvement and industrial development of perovskite solar cells.
The passivation layer material is dissolved by low temperature heating, forming a solution and drying it on the filter paper, and then the hole transport layer, perovskite active layer and passivation layer are deposited successively on the substrate, and a double passivation layer structure is formed by low temperature annealing and high temperature annealing. , simplify the process and reduce production costs.
Perovskite solar cells with low interface defect state and high energy conversion efficiency have been achieved, which improves the long-term stability and energy conversion efficiency of the battery, while reducing production costs and equipment requirements.
Smart Images

Figure CN119031801A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of perovskite solar cells, and in particular relates to a preparation process of a double passivation layer structure of a perovskite solar cell and a perovskite solar cell. Background Art
[0002] Perovskite solar cells have developed rapidly in the past decade, and their photoelectric conversion efficiency has exceeded 26%, approaching or even exceeding that of polycrystalline silicon solar cells under certain laboratory conditions. However, defects and interface problems in the perovskite material itself and the cell structure have become important factors limiting its further improvement in efficiency and long-term stability. In perovskite solar cells, defects and non-radiative recombination losses at the interface are one of the main reasons for reducing the open circuit voltage (Voc) and fill factor (FF). The introduction of passivation layers in perovskite solar cells aims to reduce these adverse effects and improve cell performance through the following mechanisms: 1. By coating a layer of passivation material on the surface of the perovskite layer, surface defects can be effectively reduced, carriers can be prevented from recombinating on the surface, thereby improving Voc and FF. 2. Inserting a passivation layer between the perovskite and the electron transport layer (ETL) or hole transport layer (HTL) can improve the energy level matching between the materials, reduce charge recombination at the interface, and enhance the charge extraction efficiency. 3. Ion migration in perovskite materials is an important factor leading to battery performance degradation. The passivation layer can help constrain the movement of ions inside the perovskite, thereby improving the long-term stability of the battery. 4. The passivation layer can also block moisture and oxygen, prevent environmental factors from corroding the perovskite material, and further improve the stability of the device. Therefore, the passivation layer plays an important role in optimizing the performance and improving the stability of perovskite solar cells. By developing new passivation materials and technologies, it is hoped that defects and interface recombination can be minimized to the greatest extent without affecting transparency and charge transfer, so as to achieve the commercial application of perovskite solar cells.
[0003] At present, the preparation process of the passivation layer can include the following typical methods: 1. In patent CN117440738A and document Sol. RRL 2024,8,2300814, the solution of the passivation material is coated on the surface or interface of the perovskite film by spin coating, dipping, spraying, etc., and then solidified by thermal annealing or solvent evaporation. However, in this method, most of the solution is not deposited on the substrate, but is thrown out or evaporated, resulting in a large amount of waste of raw materials, which significantly increases the manufacturing cost. 2. Atomic layer deposition (ALD) method, which is a precise thin film deposition technology that can control the thickness and uniformity of the film at the atomic scale, is often used to prepare films with high barrier properties and high passivation effects. However, the low deposition rate of ALD and the limited range of deposition material selection limit its further development. 3. Chemical vapor deposition (CVD) method: By transporting the gas precursor into the reaction chamber, a passivation layer is formed on the surface of the perovskite through a chemical reaction. However, CVD equipment usually requires a high vacuum environment, precise gas flow control, complex reaction chamber design, and strict temperature and pressure control. These factors lead to a high initial investment cost for CVD equipment. In addition, many precursor gases and reaction gases used in the CVD process are expensive, which increases operating costs. 4. Plasma-enhanced deposition (PE-CVD): By activating chemical reactions through plasma, the passivation layer can be deposited at a lower temperature. The quality of the film is greatly affected by the purity of the precursor. The precursor gas used in the PECVD process must have a very high purity. Any impurities may cause the quality of the film to deteriorate or form undesirable by-products. This not only increases the difficulty and cost of preparing the precursor gas, but also places higher requirements on the cleanliness and maintenance of PECVD equipment.
[0004] The passivation layer deposition method provided by the present invention can save production raw materials, does not require a high vacuum environment, precise gas flow control, complex reaction chamber design, and strict temperature and pressure control, and can prepare perovskite solar cells with high energy conversion efficiency through a simple process. Summary of the invention
[0005] In view of the deficiencies in the prior art, the object of the present invention is to provide a method for depositing a passivation layer of a perovskite cell and a perovskite cell, and to produce a perovskite solar cell with low interface defect states and high energy conversion efficiency through a simple and low-cost passivation layer preparation method.
[0006] The first aspect of the present invention provides a method for depositing a passivation layer of a perovskite cell, which specifically comprises the following steps:
[0007] (1) Dissolve the passivation layer material in an organic solvent, heat at low temperature for a period of time to help dissolve, and obtain a passivation layer solution after the passivation layer material is fully dissolved. Drop the passivation layer solution on a clean filter paper, and dry at low temperature for 24 hours to form a filter paper with the passivation layer solution attached;
[0008] (2) depositing a hole transport layer, a perovskite active layer and a first passivation layer on the substrate in a spatial order from bottom to top. After the first passivation layer is deposited, it is turned over and placed on the filter paper obtained in step (1) so that the first passivation layer is in direct contact with the filter paper. After low-temperature annealing, high-temperature annealing is performed and the filter paper is removed to obtain a double passivation layer structure.
[0009] Furthermore, the passivation layer material in step (1) includes at least one of the following materials: 4-fluorophenethylammonium chloride (4F-PEACl), phenethylammonium iodide (PEAI), butylammonium iodide (BAI), propylammonium iodide (PAI), 1,3-propylenediamine hydroiodide (PDADI), ethylenediamine hydroiodide (EDADI) or 1,8-octanediamine hydroiodide (ODADI).
[0010] In one embodiment, the organic solvent in step (1) is isopropanol.
[0011] In one embodiment, the low-temperature heating temperature in step (1) ranges from 30 to 80°C, the heating time ranges from 0 to 60 min; the volume range of the passivation layer solution ranges from 0 to 10 ml; and the low-temperature drying temperature ranges from 30 to 100°C.
[0012] Preferably, the low-temperature heating temperature in step (1) is 55°C, the heating time is 30 min, the volume of the passivation layer solution is 0.5 ml, and the low-temperature drying temperature is 40°C.
[0013] Furthermore, the first passivation layer in step (2) comprises at least one of the following materials: 4-fluorophenethylammonium chloride (4F-PEACl), phenethylammonium iodide (PEAI), butylammonium iodide (BAI), propylammonium iodide (PAI), 1,3-propylenediamine hydroiodide (PDADI), ethylenediamine hydroiodide (EDADI) or 1,8-octanediamine hydroiodide (ODADI).
[0014] In one embodiment, the low-temperature annealing in step (2) is performed at a temperature range of 30-100° C. for a time range of 0-10 min; the high-temperature annealing is performed at a temperature range of 60-200° C. for a time range of 0-30 min.
[0015] Preferably, the low-temperature annealing temperature in step (2) is 60° C. and the time is 2 min; the high-temperature annealing temperature is 100° C. and the time is 10 min.
[0016] Another aspect of the present invention provides a perovskite solar cell, which is obtained by the above-mentioned method for depositing a passivation layer of a perovskite cell, and its structure includes, from bottom to top, a substrate, a hole transport layer, a perovskite active layer, a first passivation layer, a second passivation layer, an electron transport layer, a hole blocking layer and a back electrode.
[0017] Furthermore, the first passivation layer and the second passivation layer are at least one of 4-fluorophenethylammonium chloride (4F-PEACl), phenethylammonium iodide (PEAI), butylammonium iodide (BAI), propylammonium iodide (PAI), 1,3-propylenediamine hydroiodide (PDADI), ethylenediamine hydroiodide (EDADI) or 1,8-octanediamine hydroiodide (ODADI); wherein the second passivation layer is prepared by the passivation layer deposition method described in the present invention.
[0018] In one embodiment, the substrate is a semiconductor transparent conductive film.
[0019] In one embodiment, the hole transport layer is poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly-3-hexylthiophene (P3HT), nickel oxide (NiO x ), molybdenum trioxide (MoO3), cuprous iodide (CuI), and cuprous thiocyanate (CuSCN).
[0020] In one embodiment, the perovskite active layer has an ABX3 structure, wherein the A position is an organic cation, including CH3NH3 + (MA + ), NH2CH=NH2 + (FA + )、CH3CH2NH3 + or Cs + At least one of the following, the B position is a metal cation, including Pb 2+ Sn 2+ At least one of the following, the X position is a halogen anion, including F - , Cl - Br - ,I - At least one of .
[0021] In one embodiment, the electron transport layer is zinc oxide (ZnO), tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C 61 Methyl butyrate (PC 61 BM), carbon 60 (C 60 ) at least one of.
[0022] In one embodiment, the hole blocking layer is at least one of tin dioxide (SnO2), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP), (3-[6-(diphenylphosphino)-2-naphthyl]-1,10-phenanthroline) (Phen-NaDPO) and other phenanthroline derivatives.
[0023] The back electrode is at least one of gold (Au), silver (Ag), copper (Cu), and aluminum (Al).
[0024] According to another aspect of the present invention, a method for preparing the perovskite battery as described above is also provided, which specifically comprises the following steps:
[0025] A substrate is provided, and a hole transport layer, a perovskite active layer and a first passivation layer are sequentially prepared on the substrate. The obtained thin film is turned over and attached to a filter paper containing a passivation layer solution, and low-temperature annealing and high-temperature annealing are sequentially performed to obtain a second passivation layer. An electron transport layer, a hole blocking layer and a back electrode are sequentially prepared on the second passivation layer.
[0026] Furthermore, the low-temperature annealing temperature ranges from 30 to 100° C., and the time is from 0 to 10 min; the high-temperature annealing temperature ranges from 60 to 200° C., and the time is from 0 to 30 min.
[0027] The preparation of the filter paper containing the passivation layer solution includes: dissolving the passivation layer material in an organic solvent, heating at low temperature for a period of time to help dissolution, obtaining a passivation layer solution after the passivation layer material is fully dissolved, dripping the passivation layer solution on clean filter paper, and drying at low temperature for 24 hours to form filter paper with the passivation layer solution attached.
[0028] Furthermore, the low-temperature heating temperature ranges from 30 to 80°C, the heating time ranges from 0 to 60 min; the volume range of the passivation layer solution is from 0 to 10 ml; and the low-temperature drying temperature ranges from 30 to 100°C.
[0029] Furthermore, the organic solvent is isopropanol.
[0030] Furthermore, the first passivation layer and the second passivation layer are both composed of at least one of the following materials: 4-fluorophenethylammonium chloride (4F-PEACl), phenethylammonium iodide (PEAI), butylammonium iodide (BAI), propylammonium iodide (PAI), 1,3-propylenediamine hydroiodide (PDADI), ethylenediamine hydroiodide (EDADI) or 1,8-octanediamine hydroiodide (ODADI).
[0031] The first passivation layer is prepared by coating, and the first passivation layer is obtained by coating a passivation layer solution on the surface of the perovskite active layer, spin coating and annealing.
[0032] In one embodiment, the substrate is ultrasonically cleaned in sequence using acetone, deionized water and isopropanol before preparation, with an ultrasonic power of 0-120 W and an ultrasonic cleaning time of 30 min;
[0033] Furthermore, the hole transport layer is poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), poly-3-hexylthiophene (P3HT), nickel oxide (NiO x ), molybdenum trioxide (MoO3), cuprous iodide (CuI), cuprous thiocyanate (CuSCN) or at least one of the following: the hole transport layer is spin-coated on the substrate by spin coating a hole transport layer solution at a rotation speed of 1000-6000 rpm, and then annealed at a temperature range of 60-200°C for a time of 0-30 min.
[0034] Furthermore, the preparation of the perovskite active layer includes: dissolving the perovskite material CsI:FAI:PbI2:PbBr2 in DMF:DMSO (the solvent ratio is between 0-3:10-7) at a molar ratio of x:(1-x):(y-1) / 2:(3-y) / 2 (wherein 0<x<1, 0<y<3), heating and stirring at 60°C for 12 h, and then filtering to obtain a perovskite solution; coating the perovskite solution on the hole transport layer, spin coating at a speed of 1000-6000 rpm for 30 s, and annealing at 100-150°C for 10-30 min at an air humidity of 40 RH% to obtain a perovskite active layer.
[0035] Furthermore, the electron transport layer is zinc oxide (ZnO), tin dioxide (SnO2), titanium dioxide (TiO2), [6,6]-phenyl C 61 Methyl butyrate (PC 61 BM), carbon 60 (C 60 );the hole blocking layer is at least one of tin dioxide (SnO2), 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP), (3-[6-(diphenylphosphino)-2-naphthyl]-1,10-phenanthroline) (Phen-NaDPO) and other phenanthroline derivatives. Both are prepared in sequence by evaporation, with an evaporation rate ranging from 0 to 2 Å / s and a thickness ranging from 0 to 20 nm.
[0036] Furthermore, the back electrode is prepared by vacuum evaporation at 5×10 -4 A 100 nm Ag electrode was thermally evaporated under a vacuum degree of 1.3 Pa.
[0037] Compared with the prior art, the perovskite cell based on the double passivation layer structure prepared by the above method has the following advantages: 1) Compared with the perovskite solar cell with a single passivation layer structure, the double passivation layer has a more optimized stepped energy level arrangement structure, which is beneficial to reduce non-radiative recombination losses and improve carrier transfer effects, thereby improving the energy conversion efficiency of the battery; 2) The double passivation layer has better oxygen isolation and moisture resistance, can effectively block moisture penetration, delay the degradation of perovskite, and improve the long-term stability of the device; 3) The passivation layer deposition method does not require a high vacuum environment, has low requirements for production equipment, reduces production costs and thresholds, and is conducive to the industrial development of perovskite solar cells; 4) The perovskite solar cell prepared by the passivation layer deposition method has higher open circuit voltage and energy conversion efficiency, which can achieve the effect of increasing efficiency and reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 A schematic diagram of a process for depositing a passivation layer of a perovskite solar cell provided by the present invention;
[0039] Figure 2 A schematic diagram of the structure of a perovskite solar cell based on a double passivation layer structure provided by the present invention;
[0040] Figure 3 A schematic diagram of the structure of a perovskite solar cell based on a single passivation layer structure provided by the present invention;
[0041] Figure 4 1 and 2 are IV curves of the perovskite solar cells in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention under AM 1.5G standard sunlight.
[0042] 100, substrate; 200, hole transport layer; 300, perovskite active layer; 410, first passivation layer; 420, second passivation layer; 500, electron transport layer; 600, hole blocking layer; 700, back electrode. DETAILED DESCRIPTION
[0043] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0044] In the description of the present invention, unless otherwise specified, "multiple" means two or more; the terms "center", "longitudinal", "lateral", "up", "down", "left", "right", "inside", "outside", "front end", "rear end", "head", "tail", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate the orientation or position relationship based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", "third" and the like are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0045] See also Figure 1~2 The embodiment of the present invention provides a deposition method of a perovskite battery passivation layer, in which the substrate on which the first passivation layer 410 is prepared is turned over, covered on a filter paper coated with a passivation layer material for low-temperature annealing, and then subjected to high-temperature annealing, which effectively solves the problem of solution throwing out and evaporation during high-temperature annealing in the traditional preparation method, simplifies the preparation process and reduces production costs. The deposition method specifically includes the steps of:
[0046] (1) Dissolve the passivation layer material in an organic solvent and heat it at low temperature for a period of time to help dissolve it. After the passivation layer material is fully dissolved, drop a certain amount of passivation layer solution on a surface with a size of about 30*30 mm. 2 On a clean filter paper, dry at low temperature for 24 hours to form a filter paper with a passivation layer solution attached;
[0047] (2) A hole transport layer 200, a perovskite active layer 300 and a first passivation layer 410 are sequentially deposited on a substrate 100 in a spatial order from bottom to top. After the first passivation layer 410 is deposited, it is turned over and placed on the filter paper in step (1) so that the first passivation layer 410 is in direct contact with the filter paper. After low-temperature annealing, the filter paper and the thin film on the substrate 100 are subjected to high-temperature annealing, and the filter paper is removed to obtain a first passivation layer 410 / second passivation layer 420 double passivation structure.
[0048] Furthermore, the passivation layer material in step (1) includes at least one of the following materials: 4-fluorophenethylammonium chloride (4F-PEACl), phenethylammonium iodide (PEAI), butylammonium iodide (BAI), propylammonium iodide (PAI), 1,3-propylenediamine hydroiodide (PDADI), ethylenediamine hydroiodide (EDADI) or 1,8-octanediamine hydroiodide (ODADI).
[0049] In one embodiment, the organic solvent in step (1) is isopropanol.
[0050] In one embodiment, the low-temperature heating temperature in step (1) ranges from 30 to 80°C, the heating time ranges from 0 to 60 min; the volume range of the passivation layer solution ranges from 0 to 10 ml; and the low-temperature drying temperature ranges from 30 to 100°C.
[0051] Furthermore, the first passivation layer in step (2) comprises at least one of the following material films: 4-fluorophenethylammonium chloride (4F-PEACl), phenethylammonium iodide (PEAI), butylammonium iodide (BAI), propylammonium iodide (PAI), 1,3-propylenediamine hydroiodide (PDADI), ethylenediamine hydroiodide (EDADI) or 1,8-octanediamine hydroiodide (ODADI).
[0052] In one embodiment, the low-temperature annealing in step (2) is performed at a temperature range of 30-100° C. for a time range of 0-10 min; the high-temperature annealing is performed at a temperature range of 60-200° C. for a time range of 0-30 min.
[0053] Specific embodiments and comparative examples are provided below to clearly and completely describe the technical solution of the present invention, and to conduct effective tests and corresponding comparisons on the devices obtained by the methods.
[0054] Embodiment 1:
[0055] This embodiment is a perovskite solar cell prepared by the method of the present invention, and its structure includes from bottom to top: a substrate 100, a hole transport layer 200, a perovskite active layer 300, a first passivation layer 410, a second passivation layer 420, an electron transport layer 500, a hole blocking layer 600 and a back electrode 700. The preparation method specifically includes the following steps:
[0056] (1) providing a substrate 100, ultrasonically cleaning the substrate 100 with acetone, deionized water and isopropanol for 15 min each, drying the substrate with N2, and treating the substrate with an oxygen plasma at a power of 150 W for 120 s;
[0057] (2) 100 ul of 2 mg / ml PTAA solution (solvent: toluene) was coated on the surface of the plasma-cleaned substrate 100, spin-coated at 4000 rpm for 30 s, and then the film was heated at 100 °C for 10 min to obtain a hole transport layer 200.
[0058] (3) The hole transport layer 200 prepared in the above step is treated in oxygen plasma at a power of 60 W for 60 s to remove dangling bonds on the surface of the hole transport layer 200 and improve the hydrophilicity of the hole transport layer 200.
[0059] (4) CsI:FAI:PbI2:PbBr2 was dissolved in 1 ml of DMF:DMSO (4:1 v / v) mixed solvent at a molar ratio of 0.22:0.78:0.775:0.225, where Pb 2+ The ion concentration was 1.7 M. After heating and stirring at 60 °C for 12 h, Cs was filtered using a 0.45 μm filter head. 0.22 FA 0.78 Pb(I 0.85 Br 0.15 )3 precursor solution; 120 ul of the precursor solution was coated on the surface of the hole transport layer 200, and the film was immediately placed in a flash evaporator at 2.0×10 -1 The perovskite active layer was obtained by flash evaporation at 100 ℃ for 60 s and then annealing at 100 ℃ for 10 min.
[0060] (5) 150 ul of a 2.5 mg / ml PDADI solution (solvent is isopropanol) is coated on the surface of the perovskite active layer 410, spin coated at 5000 rpm for 30 s, and then annealed at 100°C for 5 min to obtain the first passivation layer 410.
[0061] (6) Dissolve 0.8 mg 4F-PEACl in 1 ml isopropanol and heat at 55 °C for 30 min to dissolve it. After the material is fully dissolved, a passivation layer solution is obtained. Drop 500 ul of the passivation layer solution on a 30*30 mm 2 The film obtained in step (5) is turned over and placed on a clean filter paper, and dried at 60°C for 24 hours to form a filter paper with a passivation layer attached thereto; the film obtained in step (5) is turned over and placed on the filter paper so that the first passivation layer 410 is in direct contact with the filter paper, and then annealed at 65°C for 2 minutes, and then the filter paper and the film are transferred to 100°C for annealing for 10 minutes, and the filter paper is removed to obtain a first passivation layer 410 / second passivation layer 420 structure.
[0062] (7) Place the film obtained in the above steps on a mask plate and place it in the chamber of the vapor deposition machine at 1×10 -4 Pa vacuum was used to evaporate 20 nm C at an evaporation rate of 0.1-0.15 Å / s. 60 An electron transport layer 500 is obtained; after evaporation is completed and the layer is completely cooled, 5 nm BCP is evaporated at an evaporation rate of 0.1-0.15Å / s to obtain a hole blocking layer 600.
[0063] (8) Finally, in 1×10 -4 Pa vacuum, 100 nm Cu was evaporated at a rate of 1 Å / s to obtain a back electrode 700, and finally a perovskite cell was obtained.
[0064] Comparative Example 1:
[0065] Comparative Example 1 provides a perovskite solar cell having the same structural features as Example 1, except that in step (6), the second passivation layer is prepared by coating 100 ul of a 1 mg / ml 4F-PEACl solution (solvent is isopropanol) on the surface of the first passivation layer, spin coating at a speed of 5000 rpm for 30 s, and then annealing at 100°C for 5 min.
[0066] Comparative Example 2:
[0067] See also Figure 3 Comparative Example 2 provides a perovskite solar cell based on a single passivation layer structure. The structure is different from that of Example 1 in that a single passivation layer structure is adopted in Comparative Example 2, which includes, from bottom to top, a substrate 100, a hole transport layer 200, a perovskite active layer 300, a first passivation layer 410, an electron transport layer 500, a hole blocking layer 600, and a back electrode. The difference from Example 1 is that the electron transport layer 500 is directly evaporated on the first passivation layer 410 without performing step (6) to form a perovskite solar cell with a single passivation layer structure. The other conditions are the same as those of Example 1.
[0068] The JV curves of Example 1, Comparative Example 1 and Comparative Example 2 were measured under AM 1.5 G standard sunlight. Figure 4 As shown. The energy conversion efficiency of the perovskite solar cell based on a single passivation layer structure is 19.39%, while the energy conversion efficiency of the perovskite solar cell based on a double passivation layer structure prepared by spin coating is 20.09%. The energy conversion efficiency of the perovskite solar cell based on a double passivation layer structure prepared by the method of the present invention is 20.44%, wherein the open circuit voltage (Voc) and fill factor (FF) are greatly improved compared with the device prepared by the spin coating method, proving the feasibility and effectiveness of the deposition method of the present invention. As shown in the following table:
[0069] Solar cell performance parameters of Example 1, Comparative Example 1 and Comparative Example 2
[0070] sample Open circuit voltage (mV) <![CDATA[Short-circuit current density (mA / cm 2 )]]> Fill factor (%) Energy conversion efficiency (%) Example 1 1264.97 18.74 86.21 20.44 Comparative Example 1 1257.03 18.61 85.91 20.09 Comparative Example 2 1247.48 18.66 83.29 19.39
[0071] The above embodiments are only preferred implementation modes of the present invention. It should be pointed out that for ordinary technicians in this technical field, various changes, modifications, substitutions and deformations can be made to these embodiments without departing from the principles of the present invention. These technical solutions that are equivalent to the claims of the present invention all fall within the protection scope of the present invention, and the protection scope of the present invention is limited by the attached claims and their equivalents.
Claims
1. A method for depositing a passivation layer of a perovskite battery, characterized in that: The steps include: (1) Dissolve the passivation layer material in an organic solvent, heat at low temperature for a period of time to help dissolve, and obtain a passivation layer solution after the passivation layer material is fully dissolved. Drop the passivation layer solution on a clean filter paper, and dry at low temperature for 24 hours to form a filter paper with the passivation layer solution attached; (2) depositing a hole transport layer, a perovskite active layer and a first passivation layer on the substrate in a spatial order from bottom to top. After the first passivation layer is deposited, it is turned over and placed on the filter paper obtained in step (1) so that the first passivation layer is in direct contact with the filter paper. After low-temperature annealing, high-temperature annealing is performed and the filter paper is removed to obtain a double passivation layer structure.
2. The method for depositing a passivation layer of a perovskite cell according to claim 1, characterized in that: The passivation layer material in step (1) includes at least one of the following materials: 4-fluorophenethylammonium chloride, phenethylammonium iodide, butylammonium iodide, propylammonium iodide, 1,3-propylenediamine hydroiodide, ethylenediamine hydroiodide or 1,8-octanediamine hydroiodide.
3. The method for depositing a passivation layer of a perovskite cell according to claim 1, characterized in that: The organic solvent in step (1) is isopropanol.
4. The method for depositing a passivation layer of a perovskite cell according to claim 1, characterized in that: The low-temperature heating temperature in step (1) is in the range of 30-80°C, the heating time is in the range of 0-60 min; the volume of the passivation layer solution is in the range of 0-10 ml; and the low-temperature drying temperature is in the range of 30-100°C.
5. The method for depositing a passivation layer of a perovskite cell according to claim 1, characterized in that: The low-temperature annealing temperature in step (2) is in the range of 30-100°C, and the time is in the range of 0-10 min; the high-temperature annealing temperature is in the range of 60-200°C, and the time is in the range of 0-30 min.
6. A perovskite solar cell, characterized in that: The structure comprises: a substrate, a hole transport layer, a perovskite active layer, a first passivation layer, a second passivation layer, an electron transport layer, a hole blocking layer and a back electrode; the second passivation layer is obtained by the deposition method of the perovskite battery passivation layer according to any one of claims 1 to 5.
7. The perovskite solar cell according to claim 6, characterized in that: The first passivation layer and the second passivation layer are both composed of at least one of 4-fluorophenethylammonium chloride, phenethylammonium iodide, butylammonium iodide, propylammonium iodide, 1,3-propylenediamine hydroiodide, ethylenediamine hydroiodide or 1,8-octanediamine hydroiodide.
8. The perovskite solar cell according to claim 6, characterized in that: The substrate is a semiconductor transparent conductive film.
9. The perovskite solar cell according to claim 6, characterized in that: The hole transport layer is at least one of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], poly-3-hexylthiophene, nickel oxide, molybdenum trioxide, cuprous iodide, and cuprous thiocyanate.
10. The perovskite solar cell according to claim 6, characterized in that: The perovskite active layer has an ABX3 structure, wherein the A position is an organic cation, including CH3NH3 + (MA + ), NH2CH=NH2 + (FA + )、CH3CH2NH3 + or Cs + At least one of the following, the B position is a metal cation, including Pb 2+ Sn 2+ At least one of the following, the X position is a halogen anion, including F-, Cl - Br - ,I - At least one of .
11. The perovskite solar cell according to claim 6, characterized in that: The electron transport layer is at least one of zinc oxide, tin dioxide, titanium dioxide, [6,6]-phenyl C61 butyric acid methyl ester, and carbon 60.
12. The perovskite solar cell according to claim 6, characterized in that: The hole blocking layer is at least one of tin dioxide, 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, (3-[6-(diphenylphosphino)-2-naphthyl]-1,10-phenanthroline) and other phenanthroline derivatives.
13. The perovskite solar cell according to claim 6, characterized in that: The back electrode is at least one of gold, silver, copper and aluminum.
14. The method for preparing a perovskite solar cell according to any one of claims 6 to 13, comprising the steps of: A substrate is provided, and a hole transport layer, a perovskite active layer and a first passivation layer are sequentially prepared on the substrate. The obtained thin film is turned over and attached to a filter paper containing a passivation layer solution, and low-temperature annealing and high-temperature annealing are sequentially performed to obtain a second passivation layer. An electron transport layer, a hole blocking layer and a back electrode are sequentially prepared on the second passivation layer.
Citation Information
Patent Citations
Perovskite solar cell based on double passivation layers and preparation method thereof
CN117440738A
Cited By
Perovskite solar cell comprising protective layer and preparation method thereof
CN122421552A
Perovskite and passivation method and application thereof using dipole molecules for surface passivation
CN122833722A
Perovskite solar cell, manufacturing method therefor and use thereof
WO2026114026A1
Solar cell and preparation method therefor, photovoltaic module, and power consumption apparatus and power generation apparatus