A method for preparing bimodal polyethylene resin for pipe material and bimodal polyethylene resin thereof
By using Ziegler-Natta catalysts containing aromatic ester compounds for series reactions in the production of polyethylene pipes, the problem of high amounts of fine powder and oligomers in the slurry process in the existing technology is solved, and a highly resistant product is prepared. Bimodal polyethylene resin with environmental stress cracking and good tensile properties achieves extended device operation cycles and improved material properties.
Patent Information
- Application Number
- CN202111352412.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-11-16
AI Technical Summary
Existing polyethylene pipe catalysts have problems such as a large amount of fine powder and oligomers in the slurry process, and a short operating cycle of the device, resulting in high costs and backward technology. It is also difficult to prepare double catalysts with high environmental stress cracking resistance and good tensile properties. Peak polyethylene resin.
Ziegler-Natta catalysts containing aromatic ester compounds are used to perform ethylene homopolymerization and copolymerization in multiple reactors in series. By controlling the amount of hydrogen and the addition of comonomers, bis-catalysts with specific melt index and molecular weight distribution are prepared. Peak polyethylene resin.
Significantly improves the environmental stress cracking resistance, tensile properties and processing properties of bimodal polyethylene resin, reduces the precipitation of low molecular wax and the generation of oligomers, extends the device operation cycle, reduces production costs, and improves the mechanics of the material performance.
Smart Images

Figure BDA0003356273960000141 
Figure BDA0003356273960000151 
Figure BDA0003356273960000152
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyethylene, in particular to a method for preparing a bimodal polyethylene resin for pipe materials by using a Ziegler-Natta catalyst containing aromatic ester compounds and the bimodal polyethylene resin. Background Art
[0002] Polyethylene plastic pipes are mainly divided into two categories: high-density polyethylene HDPE (low-pressure polyethylene) and low-density polyethylene LDPE (high-pressure polyethylene). The application of polyethylene materials is very broad, and the pipe field is only an important aspect of polyethylene application. Due to the differences in the physical properties of HDPE and LDPE, the two materials have different applications in pipes: low-density polyethylene (LDPE) has good flexibility. However, the compressive strength is low, so it can only be used for low-pressure and small-diameter pipes. It is often made into coils and used for rural water improvement and some non-long-term use occasions. High-density polyethylene material (HDPE) is widely used in the field of pressure pipes (such as PE80, PE100) because of its good compressive resistance. The popular explanation of PE80 is: the pipe of this material is at 20°C, and it will not be damaged under continuous pressure for 50 years. The minimum required strength of the pipe wall is: 80MPa, and so on. In the early stage of the development of plastic pipes, the use of polyethylene pressure pipes was far less than that of polyvinyl chloride pipes. With the emergence of new HDPE materials and technologies, this difference in cost (weight) has changed greatly. With the emergence of the second-generation polyethylene pipe material (equivalent to PE80) and the third-generation polyethylene pipe material (equivalent to PE100), the weight of polyethylene pipes of the same length under the same diameter of 200, the same pressure level and conditions is only 93% of the weight of UPVC pipes. Therefore, the second-generation and third-generation polyethylene pipe materials not only significantly improve the minimum required strength of PE, but also improve the material's resistance to environmental stress cracking, and have significant resistance to rapid crack growth. More importantly, the wall thickness can be reduced and the transmission cross-section can be increased under the same use pressure. Increasing the pressure used under the same wall thickness can improve the transmission capacity (for example: when transporting natural gas under the same wall thickness, the transmission pressure of PE100 polyethylene pipes can reach 10 bars, while the transmission pressure of PE80 polyethylene pipes can only reach 8 bars). With the improvement of polyethylene technology, the economic benefits are significant. Recently, it has been reported that the fourth-generation polyethylene pipe material PE125 has been successfully developed. From this, it can be predicted that polyethylene pressure pipes with larger diameters and more economical properties have a broad application field.
[0003] At present, the more mature bimodal pipe material products on the market use imported catalysts to produce PE100 pipe materials. This type of catalyst improves the fine powder content of the polymer and extends the operation cycle of the device, but it does not fundamentally solve the long-standing problems of fine powder, oligomers, and short device operation cycle in the slurry process. Imported catalysts are expensive and have the problem of many oligomers. The operation cycle of the device is generally about one month, and it needs to be stopped for steaming after 5 months of operation. Therefore, the development of excellent domestic slurry polyethylene catalysts with low fine powder content and low oligomer content will have huge economic and social benefits, and will also enable my country's technology in this field to reach international levels. At the same time, strengthening my country's research on high-performance slurry catalysts is urgent and necessary, and directly affects my country's technological advancement and huge economic benefits, especially in this field. Summary of the invention
[0004] Therefore, in view of the problems existing in the prior art, the present invention provides a Ziegler-Natta catalyst containing aromatic ester compounds, which directly catalyzes polymerization in multiple reactors connected in series, and further combines different chain transfer agents, hydrogen dosages, and comonomer dosages in the reaction to prepare a bimodal polyethylene resin with a specific melt index, a specific molecular weight, and a molecular weight distribution. The bimodal polyethylene resin of the present invention does not have the problem of low molecular weight component analysis, and has high environmental stress cracking resistance, good tensile properties, and good thermal degradation resistance, and is very suitable for the production of high-performance bimodal polyethylene pipe material resins.
[0005] One of the objects of the present invention is to provide a method for preparing a bimodal polyethylene resin for pipe material comprising the following steps:
[0006] The first stage ethylene homopolymerization reaction comprises carrying out ethylene homopolymerization reaction in the presence of a Ziegler-Natta catalyst system containing aromatic ester compounds in the presence or absence of hydrogen to obtain a stream containing ethylene homopolymer;
[0007] The second stage ethylene copolymerization reaction: in the presence or absence of hydrogen, ethylene monomer and the logistics containing ethylene homopolymer obtained in the previous stage are added to the comonomer to carry out copolymerization reaction to obtain the bimodal polyethylene resin.
[0008] In the preparation method of the bimodal polyethylene resin of the present invention, the first stage ethylene homopolymerization reaction and the second stage ethylene copolymerization reaction use the same catalyst system. Specifically, the reactor of the two-stage reaction only needs to inject the catalyst during the first stage homopolymerization reaction, and the catalyst does not need to be re-injected during the second stage copolymerization reaction.
[0009] The Ziegler-Natta catalyst system containing aromatic ester compounds described in the preparation method of the bimodal polyethylene resin of the present invention can adopt the existing Ziegler-Natta catalyst system containing aromatic ester compounds in the prior art. Specific examples of the Ziegler-Natta catalyst system containing aromatic ester compounds described in the present invention can be found in patent documents CN1958620A, CN1958622A, CN102344514A, CN102344515A, CN102875708A, CN103772536A, CN102875709A, CN102993344A, CN102875707A, etc. The entire contents of these patent documents are incorporated into the present invention by reference.
[0010] Preferably, in the method for preparing a bimodal polyethylene resin of the present invention, the Ziegler-Natta catalyst system containing an aromatic ester compound comprises the following components: (1) a magnesium-containing compound; (2) an organic phosphorus compound; (3) an organic alcohol compound; (4) an organic epoxy compound; (5) an aromatic ester compound; and (6) a titanium-containing compound; the catalyst system is formed by reacting the magnesium-containing compound in a solvent system containing an organic phosphorus compound, an organic epoxy compound and an organic alcohol compound to form a magnesium complex; and the magnesium complex is reacted with an aromatic ester compound and a titanium-containing compound.
[0011] The Ziegler-Natta catalyst system containing aromatic ester compounds of the present invention is to form a magnesium complex by reacting a magnesium-containing compound in a solvent system containing an organic phosphorus compound, an organic epoxy compound and an organic alcohol compound. Usually, the magnesium complex is a uniform and transparent solution. The magnesium complex is then reacted with an aromatic ester compound and a titanium-containing compound to form a catalyst system.
[0012] Among the components of the Ziegler-Natta catalyst system containing aromatic ester compounds:
[0013] The magnesium-containing compound is selected from at least one of magnesium dihalide, a water complex or alcohol complex of magnesium dihalide, and a derivative of magnesium dihalide in which one halogen atom is replaced by a hydrocarbon oxide or a halohydrocarbon oxide. The magnesium dihalide is preferably magnesium dichloride, magnesium dibromide, or magnesium diiodide. Magnesium dichloride is the best.
[0014] The organophosphorus compound is at least one of a hydrocarbon ester of orthophosphoric acid, a hydrocarbon ester of phosphorous acid, a halogenated hydrocarbon ester of orthophosphoric acid, and a halogenated hydrocarbon ester of phosphorous acid. Specifically, trimethyl orthophosphate, triethyl orthophosphate, tributyl orthophosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, triphenyl phosphite, benzyl phosphite, etc. Among them, trimethyl orthophosphate, triethyl orthophosphate and tributyl orthophosphate are preferred, and tributyl orthophosphate is the best.
[0015] The organic epoxy compound is preferably selected from at least one of the oxides, glycidyl ethers and internal ethers of C2-C8 aliphatic olefins, C2-C8 aliphatic dienes, C2-C8 halogenated aliphatic olefins or C2-C8 halogenated aliphatic dienes; preferably selected from at least one of ethylene oxide, propylene oxide, butylene oxide, butadiene oxide, butadiene dioxide, epichlorohydrin, tetrahydrofuran, methyl glycidyl ether and diglycidyl ether; among them, ethylene oxide, propylene oxide, epichlorohydrin and tetrahydrofuran are preferred, with tetrahydrofuran and epichlorohydrin being the best.
[0016] The organic alcohol compound is C1-C 10 A straight chain, branched chain or cycloalkyl alcohol, or a C6-C 20 At least one of the alcohols containing an aromatic group. Examples of alcohols include aliphatic alcohols: methanol, ethanol, propanol, isopropanol, butanol, isobutanol, glycerol, hexanol, 2-methylpentanol, 2-ethylbutanol, n-heptanol, n-octanol, decanol, etc.; cycloalkanols such as cyclohexanol, methylcyclohexanol, etc.; aromatic alcohols such as benzyl alcohol, methylbenzyl alcohol, α-methylbenzyl alcohol, α, α-dimethylbenzyl alcohol, etc. Preferred are ethanol, butanol, 2-ethylhexanol, and glycerol. There is no particular restriction on the proportion of each alcohol in the alcohol composition.
[0017] The solvent system of the magnesium complex may optionally contain an inert diluent, which generally includes aromatic compounds or alkane compounds, wherein aromatic compounds include benzene, toluene, xylene, monochlorobenzene, dichlorobenzene, trichlorobenzene, monochlorotoluene and their derivatives; and alkanes include straight-chain alkanes, branched-chain alkanes or cycloalkanes of 3 to 20 carbon atoms or a mixture thereof, such as butane, pentane, hexane, cyclohexane, heptane, etc., whichever can be used as long as it helps dissolve the magnesium halide. The above-mentioned inert diluents may be used alone or in combination.
[0018] The general formula of the aromatic ester compound is R 1 n R 2 m C6H 5-n-m-x [(CH2) y COOR 3 ] x , where R 1 , R 2 Each is independent of C1-C 20 Alkyl, aryl, alicyclic, alkoxy, R 3 C1-C 20Alkyl, aryl, alicyclic group, 0 ≤ n < 5, 0 ≤ m < 5, 0 < x < 5, 0 ≤ y ≤ 9, where n, m, x, and y are all integers, and n + m + x < 5. The aromatic ester compounds described in the present invention include: methyl benzoate, ethyl benzoate, propyl benzoate, isopropyl benzoate, butyl benzoate, tert-butyl benzoate, hexyl benzoate, octyl benzoate, cyclohexyl benzoate, 2-methylcyclohexyl benzoate, ethyl o-methylbenzoate, ethyl p-methylbenzoate, ethyl 2,4-dimethylbenzoate, ethyl 2,6-dimethylbenzoate, ethyl 3,5-dimethylbenzoate, ethyl 2,4,6-triisopropylbenzoate, methoxyethyl benzoate, methoxypropyl benzoate, methoxybutyl benzoate, methoxyhexyl benzoate, methoxyoctyl benzoate, ethoxyethyl benzoate, ethoxypropyl benzoate, ethoxybutyl benzoate, ethoxyhexyl benzoate, ethoxyoctyl benzoate, butoxyethyl benzoate, butoxybutyl benzoate, butoxyhexyl benzoate, ethyl 5-acetyl-2-ethoxybenzoate, ethyl 3,4,5-trimethoxybenzoate, methyl phenylacetate, ethyl phenylacetate, propyl phenylacetate, isopropyl phenylacetate, butyl phenylacetate, tert-butyl phenylacetate, hexyl phenylacetate, octyl phenylacetate, cyclohexyl phenylacetate, 2-methylcyclohexyl phenylacetate, ethyl o-methylphenylacetate, ethyl p-methylphenylacetate, ethyl 2,4-dimethylphenylacetate, ethyl 2,6-dimethylphenylacetate, ethyl 3,5-dimethylphenylacetate, ethyl 2,4,6-triisopropylphenylacetate, methoxymethyl phenylacetate, methoxypropyl phenylacetate, methoxybutyl phenylacetate, methoxyhexyl phenylacetate, methoxyoctyl phenylacetate, ethoxyethyl phenylacetate, ethoxypropyl phenylacetate, ethoxybutyl phenylacetate, ethoxyhexyl phenylacetate, ethoxyoctyl phenylacetate, butoxyethyl phenylacetate, butoxybutyl phenylacetate, butoxyhexyl phenylacetate, ethyl 5-acetyl-2-ethoxyphenylacetate, ethyl 3,4,5-trimethoxyphenylacetate, methyl phenylpropionate, ethyl phenylpropionate, etc. Preferred are ethyl benzoate, propyl benzoate, ethoxyethyl benzoate, ethyl phenylacetate, and propyl phenylacetate.
[0019] The general formula of the titanium-containing compound is Ti(OR 5 ) a X 2 b where R 5 is a C1-C 14 aliphatic hydrocarbon group or aromatic hydrocarbon group, X 2 is a halogen, a is an integer from 1 to 4, b is an integer from 1 to 4, and a + b = 3 or 4.
[0020] The titanium-containing compounds include: TiCl4, TiBr4, TiCl4, Ti(OC2H5)Cl3, Ti(OCH3)Cl3, Ti(OC4H9)Cl3, Ti(OC2H5)Br3, Ti(OC2H5)2Cl2, Ti(OCH3)2Cl2, Ti(OCH3)2I2, Ti(OC2H5)3Cl, Ti(OCH3)3Cl, Ti(OC2H5)3I, Ti(OC2H5)4, Ti(OC3H7)4, Ti(OC4H9)4, etc. Preferred are TiCl4, Ti(OC2H5)Cl3, Ti(OCH3)Cl3, Ti(OC4H9)Cl3, and Ti(OC4H9)4. TiCl4 is the best.
[0021] The components of the Ziegler-Natta catalyst system containing aromatic ester compounds of the present invention are calculated based on each mole of magnesium-containing compound in the magnesium complex. The aromatic ester compound is 0.1 to 1 mole, preferably 0.1 to 0.5 mole, for example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 mole; the titanium-containing compound is 1 to 20 moles, preferably 1 to 15 moles, for example, it can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 moles.
[0022] In the solvent system for forming a magnesium complex in the Ziegler-Natta catalyst system containing aromatic ester compounds of the present invention, the organic epoxy compound is 0.2-10 moles, preferably 0.2-4 moles, for example, specifically 0.2, 0.3, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 moles per mole of the magnesium-containing compound; the organic phosphorus compound is 0.1-10 moles, preferably 0.2-4 moles, for example, specifically 0.1, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 moles; and the organic alcohol compound is 0-6 moles, preferably 0-2 moles, for example, specifically 0, 1, 2, 3, 4, 5, 6 moles.
[0023] Preferably, the Ziegler-Natta catalyst system containing aromatic ester compounds of the present invention is prepared by a method comprising the following steps:
[0024] (1) Under the protection of inert gas, the magnesium-containing compound is dissolved in a solvent system containing the organic epoxy compound and the organic phosphorus compound to form a uniform solution of the magnesium complex, and the dissolution temperature is 50 to 90° C.; the organic alcohol compound is added during or after the solution is formed to obtain a magnesium complex reaction solution. The reaction is sufficient, and the general reaction time is 0.5 to 6 hours, preferably 1 to 6 hours.
[0025] (2) The reaction solution is contacted with the titanium-containing compound at a temperature of -30°C to 0°C, and the aromatic ester compound is introduced before, after or during the reaction; the mixture is slowly heated to 50 to 120°C, and the solid matter gradually precipitates and forms particles. The reaction is sufficient, and the reaction time is generally 0.5 to 10 hours, preferably 0.5 to 6 hours.
[0026] The method may then include: (3) removing unreacted substances and solvent from the mixture (ie, the product after the reaction in step (2)) to obtain the Ziegler-Natta catalyst system containing aromatic ester compounds.
[0027] The unreacted products and solvent can be removed by a common method in the prior art, such as by suction filtration. In addition, it is also preferred to wash the reaction product with the inert diluent, such as hexane, to obtain the Ziegler-Natta catalyst system containing ester compounds.
[0028] The bimodal polyethylene resin of the present invention uses a Ziegler-Natta catalyst system containing aromatic ester compounds. During the polymerization reaction, a common cocatalyst for ethylene polymerization reaction, such as an organic aluminum cocatalyst, can be added in a common amount.
[0029] The method of the present invention comprises preparing the product by serially connecting ethylene homopolymerization and ethylene copolymerization in the presence of a Ziegler-Natta catalyst system containing aromatic ester compounds. The method of the present invention is preferably carried out in two or more reactors operated in series.
[0030] The series-connected ethylene homopolymerization and ethylene copolymerization may include two or more reaction stages; wherein both the ethylene homopolymerization and ethylene copolymerization may be carried out in one or more stages; preferably, the ethylene homopolymerization is carried out in one stage, and the ethylene copolymerization is carried out in one or two stages; more preferably, the series-connected ethylene homopolymerization and ethylene copolymerization include an ethylene homopolymerization stage and a subsequent ethylene copolymerization stage.
[0031] According to the method of the present invention, the first stage ethylene homopolymerization reaction comprises carrying out ethylene homopolymerization reaction in the presence of a Ziegler-Natta catalyst system comprising an ester compound in the presence or absence of hydrogen to obtain a logistics comprising ethylene homopolymer. The melt index of the ethylene homopolymer obtained by the first stage ethylene homopolymerization reaction is greater than or equal to 60 g / 10 min under a load of 1.2 kg, preferably greater than or equal to 65 g / 10 min. The density range is ≥0.963 g / cm 3 , preferably 0.963 to 0.980 g / cm 3 , more preferably 0.965 to 0.975 g / cm 3 .
[0032] In the second stage, ethylene copolymerization reaction is carried out by adding ethylene monomer and the stream containing ethylene homopolymer obtained in the above stage and the comonomer to carry out copolymerization reaction in the presence or absence of hydrogen, thereby producing a homopolymer and copolymer mixed bimodal polyethylene resin.
[0033] The method described in the present invention comprises a series of ethylene homopolymerization reaction and ethylene copolymerization reaction, and by controlling the hydrogen-ethylene ratio and the ethylene copolymerization conditions, two molecular weight distribution structures including a low molecular weight part (homopolymerization part) and a high molecular weight part (copolymerization part) are obtained, thereby obtaining the bimodal polyethylene resin.
[0034] More specifically, in the method of the present invention:
[0035] The reaction temperature of the first stage ethylene homopolymerization reaction is 60-100°C, preferably 70-90°C; the reaction pressure is 0.1-3.0 MPa, preferably 0.5-2 MPa.
[0036] The reaction temperature of the second stage ethylene copolymerization reaction is 60-100°C, preferably 70-90°C; the reaction pressure is 0.01-3.0 MPa, preferably 0.05-2 MPa.
[0037] Preferably, the first stage ethylene homopolymerization reaction is carried out in the presence of hydrogen, and the molar ratio of hydrogen to ethylene in the ethylene homopolymerization reaction stage (% / %) is 4.0-7.0, preferably 5.0-6.0, for example, specifically 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0. The hydrogen to ethylene molar ratio (% / %) of the present invention is the ratio of the molar percentage concentration (mol%) of hydrogen to the molar percentage concentration (mol%) of ethylene in actual production.
[0038] Preferably, the second stage ethylene copolymerization reaction is carried out in the presence of hydrogen, and the ratio of hydrogen to ethylene (% / %) in the ethylene copolymerization reaction stage is 0.01 to 0.2, preferably 0.05 to 0.1, for example, specifically 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2. The hydrogen to ethylene molar ratio (% / %) described in the present invention is the ratio of the molar percentage concentration (mol%) of hydrogen to the molar percentage concentration (mol%) of ethylene in actual production.
[0039] Preferably, the molar ratio (% / %) of the comonomer to ethylene in the second stage ethylene copolymerization reaction is 0.01 to 0.20, preferably 0.03 to 0.08, for example, specifically 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2. The molar ratio (% / %) of the comonomer to ethylene described in the present invention is the ratio of the molar percentage concentration (mol%) of the comonomer to the molar percentage concentration (mol%) of ethylene in actual production.
[0040] Preferably, the comonomer structural formula is: CH2=CHR, wherein R is a linear or branched alkane having 1 to 10 carbon atoms; the comonomer is preferably at least one of propylene, butene-1, pentene-1, hexene-1, octene-1, and decene-1.
[0041] The catalyst packing, the logistics rate of each stage or the range of reaction time are conventionally adjusted and selected according to the actual load of the reactor.
[0042] The preparation method of the bimodal polyethylene resin of the present invention can adopt slurry polymerization during polymerization, and the method carries out ethylene polymerization in at least two slurry reactors connected in series. The reactors connected in series obtain high molecular weight polyethylene (i.e., ethylene copolymerization part) and low molecular weight polyethylene (i.e., ethylene homopolymerization part) with different molecular weights, and the polyethylenes with different molecular weights can be well reacted and mixed in the reactors.
[0043] The slurry polymerization medium may be a common slurry polymerization medium, including at least one of an inert solvent such as isobutane, hexane, heptane, cyclohexane, naphtha, raffinate, hydrogenated gasoline, kerosene, benzene, toluene, xylene or the like saturated aliphatic hydrocarbons or aromatic hydrocarbons.
[0044] In order to adjust the molecular weight of the final polymer, hydrogen is usually used as a molecular weight regulator.
[0045] A second object of the present invention is to provide a bimodal polyethylene resin obtained by the method.
[0046] The bimodal polyethylene resin for pipe materials of the present invention comprises a low molecular weight portion (homopolymer unit) and a high molecular weight portion (copolymer unit), that is, has a bimodal molecular weight distribution.
[0047] Further,
[0048] The melt index of the bimodal polyethylene resin of the present invention is 0.10 to 0.40 g / 10 min, preferably 0.15 to 0.35 g / 10 min, under a load of 5 kg.
[0049] The density range of the bimodal polyethylene resin of the present invention is 0.943-0.963 g / cm 3 , preferably 0.945 to 0.955 g / cm 3 .
[0050] According to one aspect of the technical solution of the present invention, the homopolymer unit part of the bimodal polyethylene resin has a density range of ≥0.963g / cm 3 , preferably 0.963~0.980g / cm 3 , and the more preferred range is 0.965 to 0.975 g / cm 3 ; The melt index is greater than or equal to 60 g / min, preferably greater than or equal to 65 g / 10 min, under a load of 1.2 kg.
[0051] According to one aspect of the technical solution of the present invention, the bimodal polyethylene resin contains copolymerized units, wherein the copolymerized units are derived from comonomers copolymerized with ethylene, and the comonomers of the copolymerized units include α-olefin monomers.
[0052] Furthermore, the comonomer structural formula is preferably CH2=CHR; wherein R is preferably a linear or branched alkane having 1 to 10 carbon atoms; the comonomer is more preferably at least one of propylene, butene-1, pentene-1, hexene-1, octene-1, and decene-1, and the most preferred comonomer is at least one of hexene-1, butene-1, and octene-1.
[0053] The content of the comonomer of the copolymer unit in the bimodal polyethylene resin is greater than 0 and less than or equal to 1.0wt%, preferably 0.001-0.8wt%, for example 0.001, 0.005, 0.01, 0.05, 0.1, 0.15, 0.20, 0.25, 0.30, 0.35, 0.40, 0.45, 0.5, 0.55, 0.60, 0.65, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95, 1.0wt%.
[0054] According to one aspect of the technical solution of the present invention, the bimodal polyethylene resin of the present invention has better tensile properties, less low molecular weight wax precipitation and very good processing properties.
[0055] The tensile breaking nominal strain of the bimodal polyethylene resin of the present invention is greater than or equal to 500%.
[0056] The tensile yield stress of the bimodal polyethylene resin of the present invention is greater than or equal to 20 MPa.
[0057] The bimodal polyethylene resin of the present invention has a simple supported beam notched impact strength at 23°C greater than or equal to 20 kJ / m 2 .
[0058] The third object of the present invention is to provide a pipe material product prepared from the bimodal polyethylene resin. In specific applications, various extrusion processes and molding methods available in the art can be used to obtain bimodal pipe material polyethylene products, such as cable materials, natural gas pipelines, etc.
[0059] The bimodal polyethylene resin for pipe materials of the present invention adopts a Ziegler-Natta catalyst system containing aromatic ester compounds to prepare the bimodal polyethylene resin in multiple reactors connected in series. The catalyst system has the advantages of controllable particles, narrow particle size distribution, high catalytic activity, good hydrogen adjustment sensitivity, and high comonomer content. The bimodal polyethylene resin prepared by the catalyst containing aromatic ester compounds of the present invention has the characteristics of large particles and less fine powder content, less oligomer generation, outstanding mechanical properties, and excellent thermal degradation resistance. The use of the Ziegler-Natta catalyst system containing aromatic ester compounds of the present invention in multiple reactor processes connected in series solves the problems of long-standing problems such as large fine powder, large oligomers, and short device operation cycle in the slurry process, and the mechanical properties of the resin are significantly improved, with considerable economic benefits.
[0060] The bimodal polyethylene resin of the present invention prepared by the Ziegler-Natta catalyst system containing aromatic ester compounds of the present invention has good particle morphology, concentrated particle size distribution, less large particles and fine powder content, so it has good fluidity and is conducive to processing; at the same time, the bimodal polyethylene resin of the present invention has few oligomers, and its molecular weight and molecular weight distribution are controllable, and has good processing performance. Moreover, the bimodal polyethylene resin of the present invention does not have the problem of containing low molecular weight precipitates. The unique resin structure of the bimodal polyethylene resin of the present invention makes the polyethylene pipe material products prepared therefrom resistant to environmental stress cracking and excellent in mechanical properties. The bimodal polyethylene resin of the present invention has a melt index of 0.10 to 0.40 g / 10min (5kg), preferably 0.15 to 0.35 g / 10min, and a density of 0.943 to 0.963 g / cm 3 , preferably 0.945 to 0.955 g / cm 3 It is very suitable for pipe products. DETAILED DESCRIPTION
[0061] The present invention will be further described below by means of specific examples, but they do not constitute any limitation to the present invention.
[0062] The data related to the polymer in the examples were obtained by the following test methods:
[0063] (1) Resin tensile properties: measured according to the method described in GB / T 1040.2-2006, with a test speed of 50 mm / min.
[0064] (2) Melt mass flow rate (also known as melt index, MI): The melt index of the resin after ethylene homopolymerization was measured at 190°C under a load of 1.2 kg, and the melt index of the resin after ethylene copolymerization was measured under a load of 5 kg according to the method described in ASTM D1238-2038, using a CEAST 7026 melt indexer. The measurement was performed using a 1.00 mm die.
[0065] (3) Simply supported beam notched impact strength: measured in accordance with the method described in GB / T 1043.1.
[0066] (4) Resin density: Determined according to the method described in GB / T 1033.2-2010. The extruded specimens used in the melt flow rate test are used as the specimens for density determination. The surface of the specimens is smooth, free of voids and burrs. After the specimens are cut, they are placed on a cold metal plate, and then immersed in a beaker filled with distilled water, covered with a lid, and boiled in 200 ml of boiling distilled water for 30 minutes for annealing. The beaker is then placed in a laboratory environment and cooled to room temperature, and the test is performed within 24 hours.
[0067] (5) The content of comonomer in bimodal polyethylene resin: determined by nuclear magnetic resonance method. A 400MHz nuclear magnetic resonance spectrometer (NMR) of Bruker Company of Switzerland was used, with a 10mm probe. The solvent was deuterated o-dichlorobenzene, and about 250mg of the sample was placed in 2.5ml of the deuterated solvent. The sample was dissolved in an oil bath at 140℃ to form a uniform solution. 13C-NMR was collected, the probe temperature was 125℃, a 90° pulse was used, the sampling time AQ was 5 seconds, the delay time D1 was 10 seconds, and the number of scans was more than 5000 times.
[0068] (6) Particle size distribution of resin powder: The particle size distribution of resin powder was investigated by sieving using a German Retsch sieving instrument.
[0069] (7) Oxidation induction time: Determined according to the method described in GB / T19466.6-2009. Place the plastic sample and an inert reference substance (such as aluminum oxide) in a differential thermal analyzer, and rapidly replace the inert gas (such as nitrogen) in the sample chamber with oxygen at a certain temperature. Test the changes in the DTA curve (differential thermal spectrum) caused by the oxidation of the sample, and obtain the oxidation induction period (time) OIT (min) to evaluate the heat aging resistance of the plastic.
[0070] (8) Flexural modulus: measured according to the method described in GB / T9341-2008.
[0071] The raw materials used in the examples and comparative examples of the present invention are all commercially available.
[0072] Example 1
[0073] (1) Preparation of the Ziegler-Natta catalyst system containing ester compounds:
[0074] The preparation method of the solid catalyst is the same as that of patent CN201210397456.7 (CN103772536A). In a reactor fully replaced with high-purity nitrogen, 4.0g of magnesium dichloride, 50ml of toluene, 3.0ml of epichlorohydrin, 9.0ml of tributyl phosphate, and 4.4ml of ethanol are added in sequence, and the temperature is raised to 70°C under stirring. When the solid is completely dissolved to form a uniform solution, the reaction is carried out for 2 hours. The system is cooled to -10°C, 4.0ml of ethyl benzoate is slowly added dropwise, and 60ml of titanium tetrachloride is added dropwise after 10 minutes of constant temperature. The temperature is slowly raised to 85°C and reacted for 2 hours. Stop stirring, let it stand, the suspension is quickly layered, the supernatant is removed, the hexane is washed four times, and the high-purity nitrogen is blown dry to obtain a solid ester compound-containing Ziegler-Natta catalyst system with good circulation and narrow particle size distribution.
[0075] (2) Polymerization reaction:
[0076] The polymerization reaction was carried out in two slurry reactors connected in series.
[0077] The above-obtained Ziegler-Natta catalyst system containing ester compounds and the co-catalyst (triethylaluminum) are continuously introduced into the first reactor through the catalyst storage tank to complete the first stage of ethylene homopolymerization reaction; the polymerization reaction temperature of the first reactor is 84°C and the reaction pressure is 0.78MPa. Hydrogen is added to the feed of the first reactor, hydrogen is used as a molecular weight regulator, and hexane is used as a diluent. The amount of hydrogen added is 21kg / h, wherein the hydrogen / ethylene molar ratio (% / %) is 5.6, and an ethylene homopolymer is obtained. The ethylene homopolymer prepared in the first reactor has a melt index of 90g / 10min and a density of 0.9688g / cm 3 .
[0078] The ethylene homopolymer obtained in the first reactor enters the second reactor; the polymerization temperature of the second reactor is 78°C and the reaction pressure is 0.24MPa. In the feed of the second reactor, the amount of hydrogen added is 1.25kg / h, and the amount of comonomer butene added is 514kg / h; the hydrogen / ethylene molar ratio (% / %) is 0.105; the butene / ethylene molar ratio (% / %) is 0.041. The melt index of the bimodal polyethylene resin obtained by the reaction in the second reactor is 0.24g / 10min; the density is 0.950g / cm 3The melt index of the bimodal polyethylene resin pellets obtained after the reaction in the second reactor was completed was 0.22 g / 10 min; the density was 0.950 g / cm 3 The comonomer content of the bimodal polyethylene resin is 0.069%wt. Specific test data of basic properties and mechanical properties of the resin are shown in Tables 1-6.
[0079] The obtained bimodal polyethylene resin is used to prepare pipe materials using existing processes, and the resin has good processing performance and no problem of low molecular weight precipitates. The unique resin structure of the bimodal polyethylene resin of the present invention improves the tensile strength and rapid crack growth resistance of the prepared polyethylene pipe material.
[0080] Comparative Example 1
[0081] The TH series catalyst transferred by Lyondellbasell was used to prepare bimodal polyethylene pipe material resin.
[0082] After being activated, the solid catalyst component continuously enters the first reactor through the catalyst storage tank to complete the first stage of ethylene polymerization reaction. The polymerization reaction temperature of the first reactor is 85°C, the reaction pressure is 0.78MPa; the hydrogen addition amount is 25kg / h, wherein the hydrogen / ethylene molar ratio (% / %) is 6.5, and an ethylene homopolymer is obtained. The ethylene homopolymer prepared in the first reactor has a melt index of 102g / 10min and a density of 0.9694g / cm 3 .
[0083] The ethylene homopolymer stream obtained in the first reactor enters the second reactor; the polymerization temperature of the second reactor is 82°C, and the reaction pressure is 0.24MPa. The amount of butene added to the feed of the second reactor is 639kg / h, the butene / ethylene molar ratio (% / %) is 0.051; the hydrogen / ethylene molar ratio (% / %) is 0.290; the melt index of the bimodal polyethylene resin obtained by the reaction in the second reactor is 0.23g / 10min; the density is 0.949g / cm 3 After the reaction in the second reactor, the melt index of the bimodal polyethylene resin obtained was 0.22 g / 10 min; the density was 0.949 g / cm 3 The comonomer content of the bimodal polyethylene resin is 0.061%wt. The test data of the basic properties and mechanical properties of the specific resin are shown in Tables 1 to 6.
[0084] Comparative Example 2
[0085] Imported Z501 series catalysts are used to prepare bimodal polyethylene pipe material resins.
[0086] After being activated, the solid catalyst component continuously enters the first reactor through the catalyst storage tank to complete the first stage of ethylene polymerization reaction. The polymerization reaction temperature of the first reactor is 84°C, the reaction pressure is 0.78MPa; the amount of hydrogen added is 12.5kg / h, and the hydrogen / ethylene molar ratio (% / %) is 3.23 to obtain ethylene homopolymer. The ethylene homopolymer prepared in the first reactor has a melt index of 103g / 10min and a density of 0.9697g / cm 3 .
[0087] The ethylene homopolymer stream obtained in the first reactor enters the second reactor; the polymerization temperature of the second reactor is 78°C, and the reaction pressure is 0.24MPa. The amount of butene added to the feed of the second reactor is 645kg / h, the butene / ethylene molar ratio (% / %) is 0.052; the hydrogen / ethylene molar ratio (% / %) is 0.006; the melt index of the bimodal polyethylene resin obtained by the reaction in the second reactor is 0.28g / 10min; the density is 0.949g / cm 3 After the reaction in the second reactor, the melt index of the bimodal polyethylene resin obtained was 0.25 g / 10 min and the density was 0.949 g / cm 3 The comonomer content of the bimodal polyethylene resin is 0.060%wt. The specific test data of the basic properties and mechanical properties of the resin are shown in Tables 1 to 6.
[0088] Table 1 Resin powder particle size distribution and catalyst activity
[0089]
[0090] From the data in Table 1, it can be seen that the Ziegler-Natta catalyst containing aromatic ester compounds prepared by the method provided by the present invention is used for ethylene polymerization in two or more series-connected reactions to prepare a bimodal polyethylene resin having good particle morphology, fewer large and small particles, concentrated particle size distribution, wherein the 75 μm to 150 μm region accounts for about 95%, and good fluidity. This is conducive to the smooth operation of the device feeding system and increases the production load of the device.
[0091] Table 2. Hydrogen-to-ethylene ratio of polymerization kettle and polymer powder density
[0092]
[0093] Table 3. Melt index of polymer powder in polymerization kettle
[0094]
[0095] It can be seen from Tables 2 and 3 that when producing bimodal polyethylene resins with a specific density and a specific melt index, the ester compound-containing Ziegler-Natta catalyst prepared by the method provided by the present invention is used for ethylene polymerization in two or more reactions connected in series, and the hydrogen-ethylene ratio of the first reactor can meet the production requirements under a relatively low condition; the amount of hydrogen added to the second reactor is easy to control, the production is stable, and the indicators of the produced resin products are qualified.
[0096] Table 4. Butene-ethylene ratio of polymerization kettle and comonomer content of polymer powder
[0097]
[0098] As can be seen from Table 4, when the ester compound-containing Ziegler-Natta catalyst prepared by the method provided by the present invention is used for ethylene polymerization in two or more reactions connected in series, when the amount of the comonomer butene added is small, the comonomer content of the polymer is significantly improved, which is beneficial to improving the mechanical properties of the resin.
[0099] Table 5. Ethane content of gas phase components in polymerization reactor
[0100] Aggregation Unit 1PE 2PE Ethane %(V) %(V) Example 1 4.1 0.79 Comparative Example 1 13.24 2.17 Comparative Example 2 10.98 1.85
[0101] It can be seen from the data in Table 5 that when the Ziegler-Natta catalyst containing aromatic ester compounds prepared by the method provided by the present invention is used for ethylene polymerization in two or more reactions connected in series, the ethylene ethane in the two polymerization reactors is significantly reduced, which is beneficial to improving the conversion rate of ethylene and reducing the pressure of the post-processing unit.
[0102] Table 6. Mechanical properties of resins
[0103]
[0104] It can be seen from the data in Table 6 that the Ziegler-Natta catalyst containing aromatic ester compounds prepared by the method provided by the present invention is used to polymerize ethylene in two or more reactions connected in series. The bimodal polyethylene resin prepared by the method provided by the present invention has higher tensile strength, higher impact strength and better thermal degradation resistance than the polyethylene resin of the comparative example, and is suitable for preparing large-diameter bimodal polyethylene pipe material products.
Claims
1. A method for preparing a bimodal polyethylene resin for pipe material, comprising the following steps: The first stage ethylene homopolymerization reaction comprises carrying out ethylene homopolymerization reaction in the presence of a Ziegler-Natta catalyst system containing aromatic ester compounds and in the presence of hydrogen to obtain a stream containing ethylene homopolymer; The first-stage ethylene homopolymerization reaction is carried out in the presence of hydrogen, where the molar ratio of hydrogen to ethylene is 4.0 to 7.0; the Ziegler-Natta catalyst system containing aromatic ester compounds comprises the following components: (1) a magnesium-containing compound; (2) an organic phosphorus compound; (3) an organic alcohol compound; (4) an organic epoxy compound; (5) an aromatic ester compound; (6) a titanium-containing compound; the general formula of the aromatic ester compound is R 1 n R 2 m C6H 5-n-m-x [(CH2) y COOR 3 x , where R 1 , R 2 are each independently C1-C 20 alkyl, aryl, cycloaliphatic, alkoxy, R 3 is C1-C 20 alkyl, aryl, cycloaliphatic, 0 ≤ n < 5, 0 ≤ m < 5, 0 < x < 5, 0 ≤ y ≤ 9, n, m, x, y are all integers, and n + m + x < 5; in the solvent system forming the magnesium complex in the Ziegler-Natta catalyst system containing aromatic ester compounds, based on each mole of the magnesium-containing compound, the organic alcohol compound is 0 to 6 moles; 0.2 to 10 moles of organic epoxy compound; The organic phosphorus compound is 0.1 to 10 moles; the components of the Ziegler-Natta catalyst system containing aromatic ester compounds are 0.1 to 1 mole of aromatic ester compounds per mole of magnesium-containing compound in the magnesium complex; and the titanium-containing compound is 1 to 20 moles; The second stage ethylene copolymerization reaction: in the presence of hydrogen, ethylene monomer and the logistics containing ethylene homopolymer obtained in the previous stage are added with comonomer to carry out copolymerization reaction to obtain the bimodal polyethylene resin, wherein the molar ratio of hydrogen to ethylene is 0.01 to 0.
2.
2. The method according to claim 1, characterized in that: The aromatic ester compound is prepared by reacting a magnesium-containing compound in a solvent system containing an organic phosphorus compound, an organic epoxy compound and an organic alcohol compound to form a magnesium complex; and reacting the magnesium complex with an aromatic ester compound and a titanium-containing compound to form the catalyst system.
3. The method according to claim 1, characterized in that: The magnesium-containing compound is selected from at least one of magnesium dihalide, a water complex or an alcohol complex of magnesium dihalide, and a derivative of magnesium dihalide in which one halogen atom is replaced by a hydrocarbonoxy group or a halohydrocarbonoxy group; and / or, The organic phosphorus compound is at least one of a hydrocarbon ester of orthophosphoric acid, a hydrocarbon ester of phosphorous acid, a halogenated hydrocarbon ester of orthophosphoric acid, and a halogenated hydrocarbon ester of phosphorous acid; and / or, The organic epoxy compound is at least one of an oxide, glycidyl ether, and internal ether of a C2-C8 aliphatic olefin, a C2-C8 aliphatic diene, a C2-C8 halogenated aliphatic olefin, and a C2-C8 halogenated aliphatic diene; and / or, The organic alcohol compound is C1-C 10 A straight chain, branched chain or cycloalkyl alcohol, or a C6-C 20 At least one of the alcohols containing an aromatic group; and / or, The general formula of the titanium-containing compound is Ti(OR 5 ) a X 2 b , where R 5 C1-C 14 Aliphatic or aromatic hydrocarbon group, X 2 is a halogen, a is an integer from 1 to 4, b is an integer from 1 to 4, and a+b=3 or 4.
4. The method according to claim 1, characterized in that: In the solvent system for forming a magnesium complex in the Ziegler-Natta catalyst system containing aromatic ester compounds, the organic alcohol compound is 0 to 2 moles per mole of the magnesium-containing compound; the organic epoxy compound is 0.2 to 4 moles; and the organic phosphorus compound is 0.2 to 4 moles per mole of the magnesium-containing compound; and / or The components of the Ziegler-Natta catalyst system containing aromatic ester compounds include 0.1 to 0.5 moles of aromatic ester compounds and 1 to 15 moles of titanium-containing compounds per mole of magnesium-containing compounds in the magnesium complex.
5. The method according to claim 1, characterized in that: The Ziegler-Natta catalyst system containing aromatic ester compounds is prepared by a method comprising the following steps: (1) under the protection of an inert gas, dissolving the magnesium-containing compound in a solvent system containing an organic epoxy compound and an organic phosphorus compound to form a uniform solution of a magnesium complex, wherein the dissolution temperature is 50 to 90° C.; adding an organic alcohol compound during or after the solution is formed to obtain a magnesium complex reaction solution; (2) contacting the reaction solution with the titanium-containing compound at a temperature of -30°C to 0°C, introducing the aromatic ester compound before, after or during the reaction; and slowly heating the mixture to 50 to 120°C to obtain the Ziegler-Natta catalyst system.
6. The method according to claim 1, characterized in that: The reaction temperature of the first stage ethylene homopolymerization reaction is 60-100°C; the reaction pressure is 0.1-3.0 MPa; and / or, The first stage ethylene homopolymerization reaction is carried out in the presence of hydrogen, wherein the molar ratio of hydrogen to ethylene is 5.0 to 6.
0.
7. The method according to claim 6, characterized in that: The reaction temperature of the first stage ethylene homopolymerization reaction is 70-90° C.; the reaction pressure is 0.5-2.0 MPa.
8. The method according to claim 1, characterized in that: The melt index of the ethylene homopolymer obtained by the first stage ethylene homopolymerization reaction is greater than or equal to 60 g / 10 min under a load of 1.2 kg; and / or, The density of the ethylene homopolymer obtained by the first stage ethylene homopolymerization reaction is greater than or equal to 0.963 g / cm 3 .
9. The method according to claim 8, characterized in that: The melt index of the ethylene homopolymer obtained by the first stage ethylene homopolymerization reaction is greater than or equal to 65 g / 10 min under a load of 1.2 kg; and / or, The density of the ethylene homopolymer obtained by the first stage ethylene homopolymerization reaction is 0.963-0.980 g / cm 3 .
10. The method according to claim 9, characterized in that: The density of the ethylene homopolymer obtained by the first stage ethylene homopolymerization reaction is 0.965-0.975 g / cm 3 .
11. The method according to claim 1, characterized in that: The reaction temperature of the second stage ethylene copolymerization reaction is 60-100°C; the reaction pressure is 0.01-3.0 MPa; and / or, The molar ratio of the comonomer to ethylene in the second stage ethylene copolymerization reaction is 0.01 to 0.
2.
12. The method according to claim 11, characterized in that: The reaction temperature of the second stage ethylene copolymerization reaction is 70-90°C; the reaction pressure is 0.05-2.0MPa; and / or, The second stage ethylene copolymerization reaction is carried out in the presence of hydrogen, wherein the molar ratio of hydrogen to ethylene is 0.05 to 0.1; and / or, The molar ratio of the comonomer to ethylene in the second stage ethylene copolymerization reaction is 0.03 to 0.
08.
13. The method according to claim 1, characterized in that: The comonomer structural formula is: CH2=CHR, wherein R is a linear or branched alkane having 1 to 10 carbon atoms.
14. The method according to claim 13, characterized in that: The comonomer is at least one of propylene, butene-1, pentene-1, hexene-1, octene-1, and decene-1.
15. A bimodal polyethylene resin obtained according to the method according to any one of claims 1 to 14; The melt index of the bimodal polyethylene resin is 0.10-0.40 g / 10 min under a load of 5 kg; the density of the bimodal polyethylene resin is 0.943-0.963 g / cm 3 ; The content of the comonomer in the bimodal polyethylene resin is greater than 0 and less than or equal to 1.0 wt %.
16. The bimodal polyethylene resin according to claim 15, characterized in that: The melt index of the bimodal polyethylene resin is 0.15-0.35 g / 10 min under a load of 5 kg; the density of the bimodal polyethylene resin is 0.945-0.955 g / cm 3 ; The content of the comonomer in the bimodal polyethylene resin is 0.001-0.8 wt%.
17. A pipe material product made from the bimodal polyethylene resin according to claim 15.