A binary deep eutectic solvent catalyst and its preparation method and application

By using a binary deep eutectic solvent catalyst composed of γ-valerolactone and formic acid, efficient desulfurization is achieved under mild conditions, solving the problems of catalyst toxicity and harsh preparation conditions in the existing technology, and achieving efficient and green fuel Desulfurization effect.

CN116139930BActive Publication Date: 2024-10-25WUHAN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310059542.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-10-25
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

The catalysts used in existing oxidative desulfurization technology have toxicity issues, and the conditions for preparing deep eutectic solvents are harsh, with high reaction temperatures and long reaction times, making it difficult to achieve efficient and green desulfurization effects.

Method used

A binary deep eutectic solvent composed of γ-valerolactone and formic acid is used as a catalyst to form a homogeneous liquid by mixing at room temperature and reacting with the oxidant under mild conditions of 25 to 70°C to achieve efficient desulfurization of fuel.

Benefits of technology

It achieves an efficient reduction in the removal of thiophene-based sulfur-containing compounds in fuel, requires less oxidant, has mild reaction conditions, and the catalyst is easy to prepare and degrade on a large scale, so it has great potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116139930B_ABST
    Figure CN116139930B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of oil oxidation desulfurization, and discloses a binary low eutectic solvent catalyst and its preparation method and application, wherein the catalyst includes γ-valerolactone and formic acid; the preparation method of the catalyst is: γ-valerolactone and formic acid are mixed in a molar ratio of 1:4-5, stirred at room temperature for 30 minutes, until the mixture becomes a homogeneous liquid; the application of the catalyst includes: adding a low eutectic solvent to the oil to be treated, mixing evenly, adding an oxidant at 25-70°C, reacting for 4-100 minutes, and separating the desulfurized oil. The catalyst prepared by the present invention uses naturally occurring γ-valerolactone and formic acid, is cheap and easy to obtain, and is green and degradable; during desulfurization, the oxidant demand is small, the reaction conditions are mild, desulfurization can be completed at room temperature or mild temperature, the desulfurization efficiency is high, and thiophene sulfur-containing compounds that are difficult to remove in fuel oil can be effectively removed, and it has the potential for large-scale use.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oil oxidation desulfurization, and specifically relates to a binary low eutectic solvent catalyst and a preparation method and application thereof. Background Art

[0002] Exhaust gas produced by fuel combustion is one of the main factors causing environmental pollution. Since January 2019, my country has begun to fully supply national VIA standard gasoline (sulfur content less than 10ppm), and gasoline will develop towards sulfur-free in the future. At present, the most widely used desulfurization method in industry is hydrodesulfurization (HDS), which has the characteristics of high processing efficiency and strong desulfurization ability, but the technology has high energy consumption and harsh reaction conditions (>300℃,>3MPa), and the removal efficiency of thiophene sulfides is limited, resulting in the loss of gasoline octane number. Therefore, non-hydrodesulfurization has attracted people's attention. Among non-hydrodesulfurization technologies, oxidative desulfurization (ODS) has good prospects due to its mild reaction conditions.

[0003] In the prior art, organic titanium compounds are used as catalysts in oxidative desulfurization, such as butyl titanate and ethyl titanate used in Chinese patent CN105038840A, but butyl titanate and ethyl titanate are toxic and harmful to the environment and humans; metal coordination type low eutectic solvents are also used as catalysts, such as metal-phosphoric acid coordination type low eutectic solvents used in Chinese patent CN 114887659A, but the conditions for preparing the low eutectic solvents are relatively harsh, and even at 100°C, 1 hour is required. Therefore, it is urgent to develop a green catalyst that can quickly desulfurize under low temperature reaction conditions. Summary of the invention

[0004] The invention discloses a method for catalytic oxidation desulfurization of fuel oil by using a binary low eutectic solvent, which solves the problems of high reaction temperature and long time required when using a low eutectic solvent for oxidation desulfurization in the prior art.

[0005] A binary low eutectic solvent catalyst consists of gamma-valerolactone and formic acid, wherein the molar ratio of gamma-valerolactone to formic acid is 1:4-5.

[0006] The present invention also provides a method for preparing the binary low eutectic solvent catalyst, comprising the following preparation steps: mixing γ-valerolactone and formic acid in a molar ratio of 1:4 to 5, and stirring at room temperature for 30 minutes until the mixture becomes a homogeneous liquid.

[0007] The present invention also provides the use of the binary low eutectic solvent catalyst in catalytic oxidation desulfurization of fuel oil.

[0008] Preferably, the application specifically comprises the following steps:

[0009] Add the low eutectic solvent to the oil to be treated, mix well, add an oxidant at 25-70° C., react for 4-100 minutes, and separate to obtain a desulfurized oil product;

[0010] Preferably, the volume ratio of the low eutectic solvent to the oil to be treated is 1:1-10.

[0011] Preferably, the oxidant is a H2O2 solution with a concentration of 30%.

[0012] Preferably, the ratio of the amount of the oxidant to the amount of the sulfur content in the oil to be treated is 2 to 6:1.

[0013] Preferably, the sulfur-containing compounds in the oil to be treated include benzothiophene, dibenzothiophene and 4,6-dimethyldibenzothiophene.

[0014] Preferably, the separation method is: after standing, the oil product and the low eutectic solvent are separated into layers, and the upper liquid is the desulfurized oil product.

[0015] Preferably, the sulfur content in the oil to be treated ranges from 500 to 2000 ppm.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. The low eutectic solvent oxidative desulfurization catalyst prepared by the present invention uses two naturally occurring substances, γ-valerolactone and formic acid, and has high desulfurization efficiency, and can effectively reduce the thiophene sulfur-containing compounds that are difficult to remove in fuel oil; γ-valerolactone and formic acid are cheap and easy to obtain, non-flammable, green and degradable, and can complete desulfurization at room temperature or mild temperature, and the amount of oxidant required for the reaction is small, and the reaction conditions are mild; it has the potential for large-scale use. The reaction mechanism of the oxidative desulfurization is: hydrogen peroxide first oxidizes the formic acid in the low eutectic solvent into peroxyformic acid, and at the same time, the low eutectic solvent also acts as an extractant, extracting the thiophene sulfur-containing compounds in the oil into the low eutectic solvent and then undergoing an oxidation reaction, the thiophene sulfur-containing compounds are oxidized into the corresponding sulfones, and the polarity is enhanced, thereby increasing the solubility in the low eutectic solvent, and achieving desulfurization.

[0018] 2. Low eutectic solvents can be easily prepared on a large scale because they only need to mix specific hydrogen bond donors and hydrogen bond donors in a certain proportion and heat them to a certain temperature to form a stable liquid solvent. In addition, low eutectic solvents and ionic liquids have similar properties such as low toxicity and low vapor pressure, and low eutectic solvents are easier to degrade than ionic liquids, and have great potential in oxidative desulfurization. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is the desulfurization rate of the deep eutectic solvent when the amount of oxidant used is different (temperature is 25°C);

[0020] Figure 2 is the desulfurization rate of the low eutectic solvent at different temperatures (the amount of oxidant is 22uL);

[0021] Figure 3 The desulfurization rate of three different sulfides at 70°C with a low eutectic solvent and an oxidant dosage of 55uL. DETAILED DESCRIPTION

[0022] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The methods described in the embodiments of the present invention are conventional methods unless otherwise specified. The materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified.

[0024] The present invention detects the sulfur content in the oil product by gas chromatography (GC-FID) and calculates the desulfurization rate:

[0025]

[0026] The sulfur content in the simulated oil used in the embodiments of the present invention ranges from 500 to 2000 ppm, with 500 ppm simulated oil being taken as an example.

[0027] Example 1

[0028] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0029] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0030] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0031] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 25 °C, then add 22 μL of 30% H2O2 solution, react for 100 min, let stand and separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0032] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0033] Example 2

[0034] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0035] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0036] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0037] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 25 °C, then add 33 μL of 30% H2O2 solution, react for 80 min, let stand to separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0038] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0039] Example 3

[0040] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0041] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0042] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0043] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 25°C, then add 44 μL of 30% H2O2 solution, react for 80 min, let stand to separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0044] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0045] Example 4

[0046] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0047] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0048] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0049] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 25°C, then add 55 μL of 30% H2O2 solution, react for 50 min, let stand to separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0050] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0051] Example 5

[0052] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0053] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0054] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0055] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 25°C, then add 66 μL of 30% H2O2 solution, react for 40 minutes, let stand to separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0056] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0057] Example 6

[0058] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0059] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0060] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0061] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 30°C, then add 22 μL of 30% H2O2 solution, react for 100 min, let stand and separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate as 100%;

[0062] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0063] Example 7

[0064] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0065] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0066] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0067] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 40°C, then add 22 μL of 30% H2O2 solution, react for 40 minutes, let stand to separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0068] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0069] Example 8

[0070] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0071] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0072] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0073] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 50 ° C, then add 22 μL of 30% H2O2 solution, react for 20 minutes, let stand and separate, pour out the upper liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0074] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0075] Example 9

[0076] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0077] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0078] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0079] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 60°C, then add 22 μL of 30% H2O2 solution, react for 14 min, let stand to separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0080] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0081] Example 10

[0082] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0083] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0084] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0085] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 70 ° C, then add 22 μL of 30% H2O2 solution, react for 9 minutes, let stand and separate, pour out the upper liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0086] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0087] Embodiment 11

[0088] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0089] S1. Preparation of simulated oil: 1 g of dibenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0090] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0091] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 70°C, then add 55 μL of 30% H2O2 solution, react for 4 min, let stand to separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0092] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0093] Example 12

[0094] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0095] S1. Preparation of simulated oil: 0.0184 g of benzothiophene (BT) and 0.0367 mL of tetradecane were added to 20 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm of simulated oil;

[0096] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0097] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 70°C, then add 55 μL of 30% H2O2 solution, react for 6 minutes, let stand to separate, pour out the upper layer of liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0098] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0099] Example 13

[0100] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0101] S1. Preparation of simulated oil: 0.046 g 4,6-dimethyldiphenylbenzothiophene (4,6-DMDBT) and 0.0367 mL tetradecane were added to 20 mL of n-octane, and ultrasonic cleaning was performed at a power of 100 W for 30 min to prepare 500 ppm simulated oil;

[0102] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0103] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 70 ° C, then add 55 μL of 30% H2O2 solution, let stand for stratification after the reaction, pour out the upper liquid, obtain the desulfurized oil, measure the sulfur content and calculate the desulfurization rate to be 100%;

[0104] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0105] Embodiment 14

[0106] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0107] S1. Preparation of simulated oil: 1 g of diphenylbenzothiophene (DBT) and 0.7 g of tetradecane were added to 500 mL of n-octane and ultrasonically cleaned with an ultrasonic power of 100 W for 30 min; a simulated oil of 500 ppm was prepared;

[0108] S2. 0.6 mL of γ-valerolactone and 2.4 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0109] S3. Add 6 mL of γ-valerolactone / formic acid eutectic solvent to 6 mL of simulated oil, heat to 25 ° C, then add 22 μL of 30% H2O2 solution, let stand for stratification after the reaction, pour out the upper liquid, and obtain the desulfurized oil;

[0110] The molar ratio of γ-valerolactone to formic acid is 1:4.

[0111] Embodiment 15

[0112] A method for desulfurizing fuel oil by catalytic oxidation using a binary deep eutectic solvent, specifically comprising the following steps:

[0113] S1. Preparation of simulated oil: 0.046 g of diphenylbenzothiophene (DBT) and 0.0367 mL of tetradecane were added to 20 mL of n-octane and ultrasonically cleaned with an ultrasonic cleaner having a power of 100 W for 30 min; a simulated oil of 500 ppm was prepared;

[0114] S2. 0.6 mL of γ-valerolactone and 3.0 mL of formic acid were mixed and stirred at room temperature for 30 min until the mixture became a homogeneous liquid to obtain a γ-valerolactone / formic acid low eutectic solvent;

[0115] S3. Add 2 mL of γ-valerolactone / formic acid eutectic solvent to 10 mL of simulated oil, heat to 70 ° C, then add 55 μL of 30% H2O2 solution, let stand for stratification after the reaction, pour out the upper liquid, and obtain the desulfurized oil;

[0116] The molar ratio of γ-valerolactone to formic acid is 1:5.

[0117] Table 1 Test results of the embodiments provided by the present invention

[0118]

[0119] It can be seen from Table 1 that in Examples 1, 2, 3, 4, and 5, the higher the temperature, the shorter the desulfurization time. Figure 2As shown; in combination with application examples 5, 6, 7, 8, and 9, the more the amount of oxidant, the shorter the desulfurization time. In combination with application examples 11, 12, and 13, after selecting 70°C as the reaction temperature and adding 55 μL of hydrogen peroxide, the γ-valerolactone / formic acid low eutectic solvent can completely remove BT, DBT, and 4,6-DMDBT within 10 minutes, especially removing DBT, which only takes 4 minutes. Figure 3 shown.

[0120] Table 2 Desulfurization rate at different times at 25℃ and different H2O2 dosages (%)

[0121]

[0122] It can be seen from Table 2 that under different H2O2 dosages, the low eutectic solvent can achieve desulfurization at room temperature in a relatively short time, such as Figure 1 However, when the amount of oxidant is too much, the water in the oxidant will increase the mass transfer resistance, resulting in a lower desulfurization rate at the beginning of the reaction. Therefore, it is better to choose an oxidant dosage of less than 66uL.

[0123] Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0124] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a binary deep eutectic solvent catalyst, characterized in that: The method comprises the following preparation steps: mixing gamma-valerolactone and formic acid at a substance amount ratio of 1:4-5, and stirring at room temperature until the mixture becomes a homogeneous liquid.

2. Use of the binary deep eutectic solvent catalyst prepared by the preparation method according to claim 1 in catalytic oxidation desulfurization of fuel oil.

3. The use according to claim 2, characterized in that: The specific steps include: The low eutectic solvent is added to the oil to be treated, and after uniform mixing, an oxidant is added at 25 to 70° C., and after reacting for 4 to 100 minutes, the desulfurized oil product is separated.

4. The use according to claim 3, characterized in that: The volume ratio of the low eutectic solvent to the oil to be treated is 1:1-10.

5. The use according to claim 3, characterized in that: The oxidant is a 30% H2O2 solution.

6. The use according to claim 3, characterized in that: The ratio of the amount of the oxidant to the amount of the sulfur content in the oil to be treated is 2 to 6:

1.

7. The use according to claim 3, characterized in that: The sulfur-containing compounds in the oil to be treated include benzothiophene, dibenzothiophene and 4,6-dimethyldibenzothiophene.

8. The use according to claim 3, characterized in that: The separation method is as follows: after standing, the oil product and the low eutectic solvent are separated into layers, and the upper liquid is the desulfurized oil product.

9. The use according to claim 3, characterized in that: The sulfur content in the oil to be treated ranges from 500 to 2000 ppm.