Method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis and preparing prebaked anodes using the same
Through the methods of low-temperature activation decyanization and high-pressure acid leaching, the purity and energy consumption problems of graphite recovery from aluminum electrolysis waste cathode carbon blocks are solved, efficient resource utilization is achieved, and used for prebaked anode preparation, reducing production costs and environmental pollution. .
Patent Information
- Application Number
- CN202310142387.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-21
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-02-21
AI Technical Summary
The existing methods for recycling waste cathode carbon blocks in aluminum electrolysis have problems such as low graphite purity, high energy consumption, and environmental pollution, making it difficult to realize resource utilization.
The method of low-temperature activation decyanization combined with high-pressure acid leaching is used to separate cyanide through mechanical activation and strong oxidizing agents. The acid-hydrofluoric acid system is used to dissolve and remove non-carbon impurities, and high-purity graphite is recovered and used for prebaked anodes. preparation.
It achieves efficient decomposition of graphite and directional conversion of fluoride in waste cathode carbon blocks, reduces the amount of carbon aggregate, improves resource utilization, simplifies the process, and reduces environmental pollution.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of comprehensive utilization of solid waste resources from aluminum electrolysis, and specifically to a method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis and preparing prebaked anodes using the same. Background Art
[0002] At present, there are mainly the following methods for harmless and resourceful treatment of waste cathode carbon blocks from aluminum electrolysis:
[0003] The first method is physical sorting, which mainly uses mechanical crushing to grind the waste cathode carbon blocks into fine powder, and then adds them to a flotation machine to fully mix with an aqueous solution, followed by adding collectors and frothers in turn, and utilizing the difference in hydrophobicity between graphite and electrolyte components in the waste cathode carbon blocks to achieve liquid phase separation and recovery of valuable components. Its disadvantage is that the separation of graphite and electrolyte components is not complete, and the purity of the recovered graphite is low, which limits the comprehensive utilization of the recycled products and there is a risk of secondary pollution.
[0004] The second method is high-temperature treatment, which mainly involves adding waste cathode carbon blocks of a certain particle size into high-temperature treatment equipment such as rotary kilns, vacuum furnaces, and graphitization furnaces for roasting, and utilizing the differences in saturated vapor pressure and boiling point of graphite and non-carbon components in the waste cathode carbon blocks to achieve gas phase separation and recovery of valuable components. The disadvantage is that the high-temperature treatment process is accompanied by huge energy consumption and carbon emissions, and the investment cost of high-temperature treatment equipment is extremely high. Flue-containing flue gas is extremely corrosive and poses an environmental pollution risk.
[0005] The third method is the alkaline-acid treatment method, which mainly involves refining the waste cathode carbon blocks, utilizing the differences in the chemical reaction characteristics of the non-carbon components, and performing alkaline leaching and acid leaching in turn, and then recovering the valuable components in the waste cathode carbon blocks through solid-liquid separation. The disadvantage is that the process is complicated, involving strong alkali and strong acid reagents, and the generated acid-base waste liquid has a serious risk of environmental pollution.
[0006] The fourth method is direct utilization, which mainly involves crushing untreated waste cathode carbon blocks to a certain particle size, and then dry-mixing them with calcined petroleum coke or electro-calcined anthracite in corresponding proportions, followed by wet mixing with modified asphalt, and preparing aluminum electrolysis prebaked anodes through molding and roasting in sequence to realize resource utilization of waste cathode carbon blocks. Its disadvantage is that it will introduce a large amount of catalytic impurities such as Na and Ca, resulting in increased reaction activity of the prebaked anode, increased carbon consumption and carbon emissions, and some fluorides will escape during the anode roasting process, corroding the equipment and reducing the performance of the prebaked anode. Summary of the invention
[0007] In order to solve the problems existing in the prior art, the main purpose of the present invention is to propose a method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis and using the same to prepare prebaked anodes, thereby achieving efficient decomposition of cyanide in waste cathode carbon blocks, directional conversion of fluoride and resource utilization of graphite, and having the characteristics of simple process, environmental protection and high resource utilization.
[0008] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0009] A method for recovering graphite from waste cathode carbon blocks in aluminum electrolysis, comprising the following steps:
[0010] S1. Low temperature activation decyanation
[0011] Mechanical activation combined with strong oxidizing agents are used to perform low-temperature activation and decyanation treatment on the waste cathode carbon blocks from aluminum electrolysis, and the slurry after low-temperature activation and decyanation is obtained after separation;
[0012] S2. High pressure acid leaching
[0013] An acid-hydrofluoric acid mixed acid system consisting of sodium fluoride and acid solution contained in waste cathode carbon blocks from aluminum electrolysis is used to dissolve and remove non-carbon impurity components of the slurry after low-temperature activation and decyanation during a high-pressure acid leaching process, and the solid residue after solid-liquid separation is dried to obtain recovered graphite.
[0014] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis described in the present invention, wherein: in the step S1, the waste cathode carbon blocks from aluminum electrolysis are added to an activation device, an aqueous solution is added and mixed according to a liquid-solid ratio of 3 to 15 mL / g, and then 0.01 to 0.08 mL / g of a strong oxidizing agent is added, and low-temperature activation and decyanation are performed under the conditions of a rotation speed of 100 to 300 r / min, a mass ratio of the activation medium of the activation device to the waste cathode carbon blocks from aluminum electrolysis of 10 to 20:1, and an activation time of 0.1 to 2 hours. After completion, the slurry after low-temperature activation and decyanation is separated from the activation medium by a vacuum filtration device;
[0015] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis described in the present invention, in which: in the step S2, the slurry after low-temperature activation and decyanation is added to a high-pressure reactor, and then an acid solution with a concentration of 2 to 10 mol / L in an amount of 0.5 to 5 times the volume of the slurry is added, and high-pressure acid leaching is carried out under the conditions of a reaction temperature of 120 to 220°C and a reaction time of 1 to 12 hours. After the reaction is completed, solid-liquid separation is carried out, the solid residue is dried to obtain recovered graphite, and the solution is recycled.
[0016] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks of aluminum electrolysis according to the present invention, the method further comprises:
[0017] S0. The waste cathode carbon blocks from aluminum electrolysis are coarsely crushed, medium crushed and finely crushed to obtain waste cathode carbon blocks with a particle size of ≤0.15mm.
[0018] As a preferred embodiment of the method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis described in the present invention, the strong oxidizing agents include hydrogen peroxide, sodium peroxide, potassium peroxide, calcium peroxide, potassium permanganate, and sodium hypochlorite; and the acids include hydrochloric acid, sulfuric acid, nitric acid, and perchloric acid.
[0019] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:
[0020] A method for preparing a prebaked anode comprises the following steps:
[0021] B1. The recycled graphite is added to the composite binder in a ratio of 1 to 10 wt% by mass to form a mixed material;
[0022] B2. The mixture and the carbon aggregate are added to a kneading machine and kneaded to obtain a kneaded paste;
[0023] B3. The kneaded paste is subjected to vibration molding and high-temperature calcination in sequence to obtain a prebaked anode.
[0024] As a preferred embodiment of the method for preparing a prebaked anode described in the present invention, wherein: in the step B1, the composite binder includes molten coal tar and epoxy resin, and the mass ratio of the molten coal tar to the epoxy resin is 10:90 to 90:10.
[0025] As a preferred embodiment of the method for preparing a prebaked anode described in the present invention, wherein: in the step B1, the mixing time is 0.1 to 0.5 h, and the mixing temperature is 80 to 160°C.
[0026] As a preferred embodiment of the method for preparing a prebaked anode described in the present invention, wherein: in the step B2, the mass ratio of the mixed material to the carbon aggregate is 10:90 to 20:80; the carbon aggregate includes calcined petroleum coke and residual anode.
[0027] As a preferred embodiment of the method for preparing a prebaked anode described in the present invention, wherein: in the step B2, the kneading temperature is 120-190° C. and the kneading time is 0.1-1 h.
[0028] The beneficial effects of the present invention are as follows:
[0029] The present invention proposes a method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis and preparing prebaked anodes using the same. Low-temperature activated decyanation-high-pressure acid leaching is used to recover graphite from waste cathode carbon blocks from aluminum electrolysis, thereby achieving efficient decomposition of cyanide in the waste cathode carbon blocks, directional conversion of fluoride and resource utilization of graphite. Using the recovered graphite for the preparation of prebaked anodes can effectively reduce the amount of carbon aggregate used and reduce the raw material cost of prebaked anode production. The method has the characteristics of simple process, environmental protection and high resource utilization. DETAILED DESCRIPTION
[0030] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] According to one aspect of the present invention, the present invention provides the following technical solution:
[0032] A method for recovering graphite from waste cathode carbon blocks in aluminum electrolysis, comprising the following steps:
[0033] S1. Low temperature activation decyanation
[0034] Mechanical activation combined with strong oxidizing agents are used to perform low-temperature activation and decyanation treatment on the waste cathode carbon blocks from aluminum electrolysis, and the slurry after low-temperature activation and decyanation is obtained after separation;
[0035] S2. High pressure acid leaching
[0036] An acid-hydrofluoric acid mixed acid system consisting of sodium fluoride and acid solution contained in waste cathode carbon blocks from aluminum electrolysis is used to dissolve and remove non-carbon impurity components of the slurry after low-temperature activation and decyanation during a high-pressure acid leaching process, and the solid residue after solid-liquid separation is dried to obtain recovered graphite.
[0037] Furthermore, before step S1, the method further includes: S0. coarsely crushing, medium crushing and fine crushing the waste cathode carbon blocks from aluminum electrolysis to obtain waste cathode carbon blocks with a particle size of ≤0.15 mm.
[0038] Furthermore, in the step S1, the waste cathode carbon block from aluminum electrolysis is added to the activation device, and the aqueous solution is added and mixed according to the liquid-solid ratio of 3 to 15 mL / g based on the amount of the waste cathode carbon block added, and then 0.01 to 0.08 mL / g of a strong oxidizing agent is added, and low-temperature activation and decyanation are performed under the conditions of a rotation speed of 100 to 300 r / min, a mass ratio of the activation medium of the activation device to the waste cathode carbon block from aluminum electrolysis of 10 to 20:1, and an activation time of 0.1 to 2 hours, and after completion, vacuum filtration is performed. The device separates the slurry after low-temperature activation and decyanation from the activation medium; specifically, the liquid-to-solid ratio of the amount of aqueous solution added to the mass of the aluminum electrolysis waste cathode carbon block can be, for example, but not limited to, any one of 3mL / g, 5mL / g, 7mL / g, 9mL / g, 11mL / g, 13mL / g, 15mL / g or a range between any two of them; strong oxidizing agents include hydrogen peroxide, sodium peroxide, potassium peroxide, calcium peroxide, potassium permanganate, and sodium hypochlorite, and the addition amount can be, for example, but not limited to, 0.01 The activation device is a planetary ball mill, and the activation medium is a pulverizer. The mass of the activating medium can be, for example but not limited to, any one of agate balls, stainless steel balls, and zirconia balls; the mass ratio of the activating medium to the aluminum electrolysis waste cathode carbon block can be, for example but not limited to, any one of 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, 16:1, 17:1, 18:1, 19:1, 20:1 or the range between any two of them; the activation time can be any one of 0.1h, 0.5h, 1.0h, 1.5h, 2.0h or the range between any two of them.
[0039] Furthermore, in step S2, the slurry after low-temperature activation and decyanation is added to a high-pressure reactor, and then an acid solution with a concentration of 2 to 10 mol / L is added in an amount of 0.5 to 5 times the volume of the slurry, and high-pressure acid leaching is carried out under the conditions of a reaction temperature of 120 to 220°C and a reaction time of 1 to 12 hours. After the reaction is completed, solid-liquid separation is carried out, and the solid residue is dried to obtain recovered graphite, and the solution is recycled. Specifically, the acid includes hydrochloric acid, sulfuric acid, nitric acid, and perchloric acid; the concentration of the acid solution can be, for example, but not limited to, any one of 2mol / L, 3mol / L, 4mol / L, 5mol / L, 6mol / L, 7mol / L, 8mol / L, 9mol / L, 10mol / L or a range between any two of them; the amount of acid solution added can be, for example, but not limited to, 0.5 times, 1 times, 1.5 times, 2 times, 2.5 times, 3 times, 3.5 times, 4 times, 4.5 times the volume of the slurry. The reaction temperature may be, for example, but not limited to, any one of 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, or any range between two thereof; the reaction time may be, for example, but not limited to, any one of 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, or any range between two thereof.
[0040] The present invention adopts mechanical activation combined with strong oxidizing agents such as hydrogen peroxide to perform low-temperature activation and decyanation treatment on waste cathode carbon blocks: on the one hand, the particle size can be reduced while the specific surface area of the waste cathode carbon blocks is significantly increased, the reaction contact area is increased, and the waste cathode carbon blocks and the strong oxidizing agents are fully mixed, thereby realizing low-temperature removal of highly toxic cyanide in the waste cathode carbon blocks. Under the condition of no external heat source, the cyanide removal rate is ≥95%; on the other hand, the reaction activity of the waste cathode carbon blocks can be increased by mechanical activation, and the strong oxidizing agents can effectively increase the interlamellar spacing of the graphite contained in the waste cathode carbon blocks. At the same time, the sodium fluoride contained in the waste cathode carbon blocks is innovatively used with acid solutions such as hydrochloric acid to form a more reactive acid-hydrofluoric acid mixed acid system, which is conducive to the dissolution and removal of non-carbon impurity components during high-pressure acid leaching. Only through acid leaching treatment, the purity of recovered graphite is ≥97.5%.
[0041] According to another aspect of the present invention, the present invention provides the following technical solution:
[0042] A method for preparing a prebaked anode comprises the following steps:
[0043] B1. The recycled graphite is added to the composite binder in a ratio of 1 to 10 wt% by mass to form a mixed material;
[0044] B2. The mixture and the carbon aggregate are added to a kneading machine and kneaded to obtain a kneaded paste;
[0045] B3. The kneaded paste is subjected to vibration molding and high-temperature calcination in sequence to obtain a prebaked anode.
[0046] Further, in step B1, the composite binder includes molten coal tar and epoxy resin, and the mass ratio of molten coal tar to epoxy resin is 10:90 to 90:10. Specifically, the mass ratio of molten coal tar to epoxy resin can be, for example but not limited to, any one of 10:90, 20:80, 30:70, 40:60, 50:50, 60:40, 70:30, 80:20, 90:10 or any two thereof; the amount of recycled graphite added to the binder mass can be, for example but not limited to, any one of 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% or any two thereof. In step B1, the mixing time is 0.1 to 0.5h, and the mixing temperature is 80 to 160°C. Specifically, the mixing time can be, for example, but not limited to, any one of 0.1 h, 0.2 h, 0.3 h, 0.4 h, 0.5 h, or a range between any two of them; the mixing temperature can be, for example, but not limited to, any one of 80° C., 90° C., 100° C., 110° C., 120° C., 130° C., 140° C., 150° C., 160° C., or a range between any two of them;
[0047] Furthermore, in step B2, the mass ratio of the mixed material to the carbon aggregate is 10:90 to 20:80; the carbon aggregate includes calcined petroleum coke and residual anode. Specifically, the mass ratio of the mixed material to the carbon aggregate can be, for example but not limited to, any one of 10:90, 11:89, 12:88, 13:87, 14:86, 15:85, 16:84, 17:83, 18:82, 19:81, 20:80 or a range between any two thereof; in step B2, the kneading temperature is 120 to 190°C and the kneading time is 0.1 to 1h. Specifically, the kneading temperature can be, for example, but not limited to, any one of 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, and 190°C, or a range between any two of them; the kneading time can be, for example, but not limited to, any one of 0.1h, 0.15h, 0.2h, 0.25h, 0.3h, 0.35h, 0.4h, 0.45h, 0.5h, 0.55h, 0.6h, 0.65h, 0.7h, 0.75h, 0.8h, 0.85h, 0.9h, 0.95h, and 1h, or a range between any two of them.
[0048] The use of coal tar-epoxy resin composite binder as a carrier of recycled graphite can, on the one hand, maximize the uniform dispersion of recycled graphite in prebaked anodes and effectively avoid raw material segregation; on the other hand, it can further reduce the softening point of the binder, achieve low-temperature kneading and molding of prebaked anodes, reduce the energy consumption of kneading and molding processes, and effectively enhance the wetting effect of the binder and carbon aggregate, thereby ensuring the performance of prebaked anode products prepared by blending recycled graphite. Based on the above advantages, the recycling of recycled graphite in the field of aluminum electrolysis carbon materials can be achieved, thereby effectively reducing the amount of carbon aggregate used and reducing the raw material cost of prebaked anode production; at the same time, the performance of the prepared prebaked anodes meets the standard technical requirements of "Prebaked Anodes for Aluminum Electrolysis" (YS / T 285-2012), where the apparent density is ≥1.52g / cm 3 , compressive strength ≥32MPa, resistivity ≤62μΩ·m, ash content ≤0.8%, CO 2 Reactivity ≥73%.
[0049] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0050] Example 1
[0051] This embodiment provides a method for recovering graphite from spent cathode carbon blocks in aluminum electrolysis, comprising the following steps:
[0052] S0. The aluminum electrolysis waste cathode carbon block is coarsely crushed, medium crushed and finely crushed to obtain a waste cathode carbon block with a particle size of ≤0.15mm;
[0053] S1. Add 10g of the waste cathode carbon block obtained in step S0 to the activation equipment, add an aqueous solution according to a liquid-solid ratio of 6mL / g to mix, then add 0.20mL of hydrogen peroxide, and perform low-temperature activation and decyanation at a speed of 250r / min, an activation medium of zirconium oxide balls, a mass ratio of zirconium oxide balls to aluminum electrolysis waste cathode carbon blocks of 10:1, and an activation time of 0.5h. After completion, the slurry after low-temperature activation and decyanation is separated from the activation medium by a vacuum filtration device, and the cyanide removal rate is 95.5%;
[0054] S2. The slurry after low-temperature activation and decyanation is added to a high-pressure reactor, and then a hydrochloric acid solution with a concentration of 6 mol / L, which is twice the volume of the slurry, is added, and high-pressure acid leaching is carried out at a reaction temperature of 180°C and a reaction time of 6 hours. After the reaction is completed, solid-liquid separation is carried out, and the solid residue is dried to obtain recovered graphite. The solution is recycled, and the purity of the recovered graphite is 97.8%.
[0055] This embodiment also provides a method for preparing a prebaked anode, comprising the following steps:
[0056] B1. The recycled graphite of step S2 is added to the composite binder at a ratio of 4wt% of the mass of the composite binder to form a mixed material; the mass ratio of molten coal tar and epoxy resin in the composite binder is 70:30, the mixing time is 0.2h, and the mixing temperature is 120°C;
[0057] B2. The mixed material and the carbon aggregate were added to a kneading machine in a mass ratio of 10:90 and kneaded to obtain a kneaded paste; the carbon aggregate included calcined petroleum coke and residual anode, the kneading temperature was 170 ° C, and the kneading time was 0.2h;
[0058] B3. The kneaded paste is subjected to vibration molding and high-temperature calcination in sequence to obtain a prebaked anode.
[0059] The apparent density of the prebaked anode prepared in this example is 1.53 g / cm 3 , compressive strength is 34MPa, resistivity is 60μΩ·m, ash content is 0.7%, CO 2 The reactivity is 75%.
[0060] Example 2
[0061] This embodiment provides a method for recovering graphite from spent cathode carbon blocks in aluminum electrolysis, comprising the following steps:
[0062] S0. The aluminum electrolysis waste cathode carbon block is coarsely crushed, medium crushed, and finely crushed to obtain a waste cathode carbon block with a particle size of 0.074 to 0.15 mm;
[0063] S1. Add 100g of the waste cathode carbon block obtained in step S0 to the activation device, add an aqueous solution according to a liquid-solid ratio of 12mL / g to mix, then add 4.0mL of hydrogen peroxide, and perform low-temperature activation and decyanation at a speed of 300r / min, an activation medium of zirconium oxide balls, a mass ratio of zirconium oxide balls to aluminum electrolysis waste cathode carbon blocks of 20:1, and an activation time of 1.5h. After completion, the slurry after low-temperature activation and decyanation is separated from the activation medium by a vacuum filtration device, and the cyanide removal rate is 97.8%;
[0064] S2. Add the slurry after low-temperature activation and decyanation into a high-pressure reactor, and then add a hydrochloric acid solution with a concentration of 10 mol / L that is 4 times the volume of the slurry, and carry out high-pressure acid leaching at a reaction temperature of 200°C and a reaction time of 10 hours. After the reaction is completed, solid-liquid separation is carried out, and the solid residue is dried to obtain recovered graphite. The solution is recycled, and the purity of the recovered graphite is 98.7%.
[0065] This embodiment also provides a method for preparing a prebaked anode, comprising the following steps:
[0066] B1. The recycled graphite of step S2 is added to the composite binder at a ratio of 6wt% of the mass of the composite binder to form a mixed material; the mass ratio of molten coal tar and epoxy resin in the composite binder is 50:50, the mixing time is 0.3h, and the mixing temperature is 100°C;
[0067] B2. The mixed material and the carbon aggregate were added to a kneading machine in a mass ratio of 13:87 and kneaded to obtain a kneaded paste; the carbon aggregate included calcined petroleum coke and residual anode, the kneading temperature was 150 ° C, and the kneading time was 0.25h;
[0068] B3. The kneaded paste is subjected to vibration molding and high-temperature calcination in sequence to obtain a prebaked anode.
[0069] The apparent density of the prebaked anode prepared in this example is 1.55 g / cm 3 , compressive strength is 38MPa, resistivity is 57μΩ·m, ash content is 0.4%, CO 2 The reactivity was 79%.
[0070] Example 3
[0071] This embodiment provides a method for recovering graphite from spent cathode carbon blocks in aluminum electrolysis, comprising the following steps:
[0072] S0. The aluminum electrolysis waste cathode carbon block is coarsely crushed, medium crushed, and finely crushed to obtain a waste cathode carbon block with a particle size of ≤0.074mm;
[0073] S1. Add 50g of the waste cathode carbon block obtained in step S0 to the activation equipment, add an aqueous solution according to a liquid-solid ratio of 9:1mL / g to mix, then add 3.0mL of hydrogen peroxide, and perform low-temperature activation and decyanation at a speed of 200r / min, an activation medium of zirconium oxide balls, a mass ratio of zirconium oxide balls to aluminum electrolysis waste cathode carbon blocks of 15:1, and an activation time of 1.0h. After the end, the slurry after low-temperature activation and decyanation is separated from the activation medium by a vacuum filtration device, and the cyanide removal rate is 96.7%;
[0074] S2. Add the slurry after low-temperature activation and decyanation into a high-pressure reactor, and then add a hydrochloric acid solution with a concentration of 8 mol / L, which is 3 times the volume of the slurry, and carry out high-pressure acid leaching at a reaction temperature of 210°C and a reaction time of 12 hours. After the reaction is completed, solid-liquid separation is carried out, and the solid residue is dried to obtain recovered graphite. The solution is recycled, and the purity of the recovered graphite is 98.5%.
[0075] This embodiment also provides a method for preparing a prebaked anode, comprising the following steps:
[0076] B1. The recycled graphite of step S2 is added to the composite binder at a ratio of 5wt% of the mass of the composite binder to form a mixed material; the mass ratio of molten coal tar and epoxy resin in the composite binder is 40:60, the mixing time is 0.5h, and the mixing temperature is 100°C;
[0077] B2. The mixed material and the carbon aggregate were added to a kneader in a mass ratio of 15:85 and kneaded to obtain a kneaded paste; the carbon aggregate included calcined petroleum coke and residual anode, the kneading temperature was 100 ° C, and the kneading time was 0.15h;
[0078] B3. The kneaded paste is subjected to vibration molding and high-temperature calcination in sequence to obtain a prebaked anode.
[0079] The apparent density of the prebaked anode prepared in this example is 1.54 g / cm 3 , compressive strength is 36MPa, resistivity is 58μΩ·m, ash content is 0.5%, CO 2 The reactivity was 78%.
[0080] The present invention adopts mechanical activation combined with strong oxidizing agents such as hydrogen peroxide to perform low-temperature activation and decyanation treatment on waste cathode carbon blocks: on the one hand, the particle size can be reduced while the specific surface area of the waste cathode carbon blocks is significantly increased, the reaction contact area is increased, and the waste cathode carbon blocks and the strong oxidizing agents are fully mixed, thereby realizing low-temperature removal of highly toxic cyanide in the waste cathode carbon blocks. Under the condition of no external heat source, the cyanide removal rate is ≥95%; on the other hand, the reaction activity of the waste cathode carbon blocks can be increased by mechanical activation, and the strong oxidizing agents can effectively increase the interlamellar spacing of the graphite contained in the waste cathode carbon blocks. At the same time, the sodium fluoride contained in the waste cathode carbon blocks is innovatively used with acid solutions such as hydrochloric acid to form a more reactive acid-hydrofluoric acid mixed acid system, which is conducive to the dissolution and removal of non-carbon impurity components during high-pressure acid leaching. Only through acid leaching treatment, the purity of recovered graphite is ≥97.5%.
[0081] The use of coal tar-epoxy resin composite binder as a carrier of recycled graphite can, on the one hand, maximize the uniform dispersion of recycled graphite in prebaked anodes and effectively avoid raw material segregation; on the other hand, it can further reduce the softening point of the binder, achieve low-temperature kneading and molding of prebaked anodes, reduce the energy consumption of kneading and molding processes, and effectively enhance the wetting effect of the binder and carbon aggregate, thereby ensuring the performance of prebaked anode products prepared by blending recycled graphite. Based on the above advantages, the recycling of recycled graphite in the field of aluminum electrolysis carbon materials can be achieved, thereby effectively reducing the amount of carbon aggregate used and reducing the raw material cost of prebaked anode production; at the same time, the performance of the prepared prebaked anodes meets the standard technical requirements of "Prebaked Anodes for Aluminum Electrolysis" (YS / T 285-2012), where the apparent density is ≥1.52g / cm3 , compressive strength ≥32MPa, resistivity ≤62μΩ·m, ash content ≤0.8%, CO 2 Reactivity ≥73%.
[0082] The method for recovering graphite from waste cathode carbon blocks from aluminum electrolysis and preparing prebaked anodes using the same provided by the present invention adopts low-temperature activated decyanation-high-pressure acid leaching to recover graphite from waste cathode carbon blocks from aluminum electrolysis, thereby achieving efficient decomposition of cyanide in the waste cathode carbon blocks, directional conversion of fluoride and efficient recovery of graphite. The use of the recovered graphite in the preparation of prebaked anodes can effectively reduce the amount of carbon aggregate used and the raw material cost of prebaked anode production, and has the characteristics of simple process, environmental protection and high resource utilization.
[0083] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for recovering graphite from waste cathode carbon blocks in aluminum electrolysis, characterized in that: The steps include: S1. Low temperature activation decyanation The waste cathode carbon block is subjected to low-temperature activation and decyanation treatment by mechanical activation combined with a strong oxidizing agent, wherein the strong oxidizing agent includes hydrogen peroxide, sodium peroxide, potassium peroxide, calcium peroxide, potassium permanganate, and sodium hypochlorite; the waste cathode carbon block is added to the activation device, and an aqueous solution is added and mixed according to a liquid-solid ratio of 3-15 mL / g, and then 0.01-0.08 mL / g of the strong oxidizing agent is added, and low-temperature activation and decyanation are carried out under the conditions of a rotation speed of 100-300 r / min, a mass ratio of the activation medium of the activation device to the waste cathode carbon block of 10-20:1, and an activation time of 0.1-2h. After the end, the slurry after low-temperature activation and decyanation is separated from the activation medium by a vacuum filtration device; after separation, a slurry after low-temperature activation and decyanation is obtained; the cyanide removal rate is ≥95%; S2. High pressure acid leaching The slurry after low-temperature activation and decyanation is added into a high-pressure reactor, and then an acid solution with a concentration of 2-10 mol / L is added in an amount of 0.5-5 times the volume of the slurry, and high-pressure acid leaching is carried out under the conditions of a reaction temperature of 120-220°C and a reaction time of 1-12 hours. The acid-hydrofluoric acid mixed acid system composed of sodium fluoride contained in the waste cathode carbon block and the acid solution is used to dissolve and remove the non-carbon impurity components of the slurry after low-temperature activation and decyanation during the high-pressure acid leaching process. The solid residue after solid-liquid separation is dried to obtain recovered graphite, and the purity of the recovered graphite is ≥97.5%, and the solution is recycled.
2. The method according to claim 1, characterized in that Before step S1, the following steps are also included: S0. The waste cathode carbon blocks are coarsely crushed, medium crushed and finely crushed to obtain waste cathode carbon blocks with a particle size of ≤0.15mm.
3. The method according to claim 1, characterized in that The acid includes hydrochloric acid, sulfuric acid, nitric acid, and perchloric acid.
4. A method for preparing a prebaked anode, characterized in that: The steps include: B1. The recovered graphite of any one of claims 1 to 3 is added to the composite binder in a ratio of 1 to 10 wt% of the mass of the composite binder to form a mixed material; B2. The mixture and the carbon aggregate are added to a kneading machine and kneaded to obtain a kneaded paste; B3. The kneaded paste is subjected to vibration molding and high-temperature calcination in sequence to obtain a prebaked anode.
5. The method for preparing a prebaked anode according to claim 4, characterized in that: In the step B1, the composite binder includes molten coal tar and epoxy resin, and the mass ratio of the molten coal tar to the epoxy resin is 10:90 to 90:
10.
6. The method for preparing a prebaked anode according to claim 4, characterized in that: In the step B1, the mixing time is 0.1-0.5 h, and the mixing temperature is 80-160° C.
7. The method for preparing a prebaked anode according to claim 4, characterized in that: In the step B2, the mass ratio of the mixed material to the carbon aggregate is 10:90-20:80; the carbon aggregate includes calcined petroleum coke and residual anode; the kneading temperature is 120-190° C. and the kneading time is 0.1-1 h.
Citation Information
Cited By
Method for recovering aluminum fluoride from waste cathode carbon block
CN120736548A