A method for preparing porous ceramic material based on BN precursor
The porous ceramic material with nano-microporous structure is formed through non-melting treatment and decarburization ceramic treatment, which solves the problem of pyrolysis control and waste waste in the preparation of existing boron nitride materials, and achieves high adsorption performance and low-cost nano-materials. Microporous structure, suitable for gas separation in complex chemical environments.
Patent Information
- Application Number
- CN202310027279.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-09
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-09
AI Technical Summary
In the existing preparation method of boron nitride porous materials, the pyrolysis process is difficult to control, resulting in micron or even millimeter-sized foam pores in the material, poor adsorption capacity, and the organic precursor conversion method is costly, has low conversion rate, and produces waste materials and waste wires. , causing waste.
The non-melting BN precursor is used for decarburization and ceramic treatment to form a porous structure dominated by nanopores. The BN precursor waste and waste wire are recycled and reused, and B-O-B is formed through oxygen in-situ cross-linking reaction. Structure, pore-forming agent uses water as initiator to reduce costs.
The prepared porous ceramic material has a high specific surface area and good N2 adsorption performance, is suitable for gas separation in complex chemical environments, reduces waste in the BN fiber preparation process, and achieves the formation of low-cost and non-toxic nano-microporous structures. .
Smart Images

Figure CN116143525B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of porous ceramic material preparation, and specifically relates to a method for preparing a porous ceramic material based on a BN precursor. Background Art
[0002] On the one hand, porous materials are widely used in the fields of gas separation, storage and catalyst carriers. Commonly used oxide porous materials and porous carbon-based materials have a high specific surface area, but the materials are highly hydrophilic, have high surface activity, and have poor thermal conductivity, making it difficult to cope with the requirements of long-term use in complex chemical environments.
[0003] Nitrides, especially boron nitride materials, are hydrophobic, electrically insulating, resistant to acid and alkali corrosion, have very stable chemical properties, high thermal conductivity, excellent oxidation resistance at high temperatures (>900℃), and outstanding temperature resistance in inert or alkaline atmospheres. They have broad application prospects in the fields of corrosive gas / liquid separation and purification, high-temperature reaction carriers, thermal battery separators, etc.
[0004] However, in the current preparation method of boron nitride porous materials, the precursors used in the organic precursor pyrolysis method are trichloroborazine and its polymers, borazine and its polymers. The precursors have high reaction activity and the pyrolysis process is difficult to control. The porous materials obtained are mainly micron or even millimeter-level foam pores, and have poor adsorption capacity for micro-nano small molecules.
[0005] On the other hand, in the process of preparing BN fibers by the organic precursor conversion method, the raw material cost is high, the conversion rate is low, and the production process inevitably produces waste materials and waste fibers, resulting in waste. Summary of the invention
[0006] In view of the above problems, the present invention provides a method for preparing a porous ceramic material based on a BN precursor. The porous ceramic material prepared by the method of the present invention exhibits a porous structure mainly composed of nano-micropores, has a high specific surface area and good N2 adsorption performance; the method of the present invention can recycle and reuse the BN precursor waste and waste silk generated in the process of preparing BN fibers, thereby reducing waste.
[0007] The present invention provides a method for preparing a porous ceramic material based on a BN precursor, comprising the following steps: subjecting the BN precursor to an infusible treatment so that the oxygen content in the BN precursor after the infusible treatment is 20-70wt%; subjecting the BN precursor after the infusible treatment to a decarburization treatment and a ceramic treatment in sequence to obtain a porous ceramic material.
[0008] Preferably, the BN precursor is polyborazine obtained by polymerization of aminoborane monomer; and / or, the BN precursor includes BN precursor waste and / or BN precursor waste silk generated in the process of preparing BN fibers.
[0009] Preferably, the infusibility treatment is carried out at 15-35° C. in an air atmosphere.
[0010] Preferably, during the infusibility treatment, the relative humidity of the air is 20-60%.
[0011] Preferably, the infusibility treatment is performed for 3-18 hours.
[0012] Preferably, the decarburization treatment conditions are: using ammonia as the reaction gas and heating at a rate of 1-10°C / min.
[0013] Preferably, during the decarburization treatment, the temperature is raised to 800-1200° C. and maintained for 0.5-2 h.
[0014] Preferably, the ceramic treatment is carried out under the following conditions: heating at a rate of 3-6°C / min.
[0015] Preferably, during the ceramic treatment, the temperature is raised to 1800-2000° C. and maintained for 0.5-1 h.
[0016] The invention also provides a porous ceramic material prepared by the method.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] (1) The porous ceramic material prepared by the method of the present invention has a structure dominated by nano-micropores, has a high specific surface area and good N2 adsorption performance, and the specific surface area can reach 543m 2 / g, can be used for gas separation in complex chemical environments.
[0019] (2) The present invention can recycle waste materials and waste fibers generated during the melt spinning process when the BN fibers are prepared by the organic precursor conversion method, thereby reducing the waste in the BN fiber preparation process while preparing porous ceramic materials mainly composed of nano-micropores.
[0020] (3) The present invention uses the BOB structure of the oxygen in-situ cross-linking reaction as a pore-forming agent and water as an initiator, which is low-cost and non-toxic, and the reaction temperature is easy to achieve; the BN precursor after the infusible treatment is partially melted and foamed during the subsequent treatment process that is not cross-linked and solidified to form micron-sized pores, and the oxygen cross-linked and solidified part is removed at high temperature to form nano-sized pores. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a surface morphology of the porous ceramic material prepared in Example 1 of the present invention;
[0022] Figure 2 This is a microscopic morphology of fiber pores of the porous ceramic material prepared in Example 1 of the present invention;
[0023] Figure 3 The nitrogen adsorption and desorption curves of the porous ceramic material prepared in Example 1 of the present invention;
[0024] Figure 4 This is the pore size distribution curve of the porous ceramic material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] The present invention provides a method for preparing a porous ceramic material based on a BN precursor, comprising the following steps:
[0027] (1) The BN precursor is subjected to an infusible treatment.
[0028] The BN precursor is polyborazine obtained by polymerization of aminoborane monomers, which has relatively mild activity and is conducive to the process control of subsequent thermal cracking and pore formation.
[0029] The BN precursor includes BN precursor waste and / or BN precursor waste yarn generated in the melt spinning process when the BN fiber is prepared by the organic precursor conversion method.
[0030] The infusibility treatment is carried out under the following conditions: 15-35° C., air atmosphere, relative humidity of air of 20-60%, and treatment time of 3-18 hours.
[0031] The oxygen content of the BN precursor after the infusible treatment is 20-70wt%. If the oxygen content after the infusible treatment is too low, the subsequent treatment will mostly melt and foam, and the pore size will be too large; if the oxygen content is too high, the BN precursor is easily hydrolyzed and powdered. When the BN precursor includes BN precursor waste silk, too high or too low oxygen content will also result in the inability to maintain the fiber morphology in the subsequent treatment.
[0032] (2) The BN precursor after the infusible treatment is subjected to decarburization treatment and ceramic treatment in sequence to obtain a porous ceramic material.
[0033] The decarburization treatment conditions are: using ammonia as the reaction gas, heating to 800-1200° C. at a rate of 1-10° C. / min and maintaining the temperature for 0.5-2 h.
[0034] The ceramic treatment conditions are: in an inert atmosphere, heating to 1800-2000° C. at a rate of 3-6° C. / min and keeping the temperature for 0.5-1 h.
[0035] The heating rate during the decarburization and ceramicization treatments needs to be controlled within the above range to avoid a reduction in yield due to a too low heating rate and a melt foaming and powdering due to a too high heating rate.
[0036] The present invention also provides a porous ceramic material prepared by the above method. The porous ceramic material has a structure mainly composed of nano-micropores and a specific surface area of up to 543 m 2 / g.
[0037] Example 1
[0038] This embodiment provides a method for preparing a porous ceramic material based on a BN precursor, comprising the following steps:
[0039] (1) The BN precursor is subjected to an infusible treatment.
[0040] The BN precursor is polyborazine obtained by polymerization of aminoborane monomers. In this embodiment, as a preferred solution, the BN precursor is waste BN precursor generated during the melt spinning process when the BN fiber is prepared by an organic precursor conversion method.
[0041] The infusibility treatment was carried out under the following conditions: 25° C., air atmosphere, relative humidity of air was 30%, and the treatment time was 15 h.
[0042] The oxygen content in the BN precursor after the infusibility treatment is 40-65wt%.
[0043] (2) The BN precursor after the infusible treatment is subjected to decarburization treatment and ceramic treatment in sequence to obtain a porous ceramic material.
[0044] The decarburization treatment conditions are: using ammonia as the reaction gas, heating to 1000° C. at a rate of 5° C. / min and keeping the temperature for 1 hour.
[0045] The ceramic treatment conditions are: in an inert atmosphere, heating to 1850° C. at a rate of 4° C. / min and maintaining the temperature for 1 hour.
[0046] This embodiment also provides a porous ceramic material produced by the above method.
[0047] Example 2
[0048] This embodiment provides a method for preparing a porous ceramic material based on a BN precursor, comprising the following steps:
[0049] (1) The BN precursor is subjected to an infusible treatment.
[0050] The BN precursor is polyborazine obtained by polymerization of aminoborane monomers. In this embodiment, as a preferred solution, the BN precursor is the BN precursor waste remaining in the melt spinning process when the BN fiber is prepared by the organic precursor conversion method.
[0051] The infusibility treatment was carried out under the following conditions: 20° C., air atmosphere, relative humidity of air was 45%, and the treatment time was 9 hours.
[0052] The oxygen content in the BN precursor after the infusibility treatment is 55-65wt%.
[0053] (2) The BN precursor after the infusible treatment is subjected to decarburization treatment and ceramic treatment in sequence to obtain a porous ceramic material.
[0054] The decarburization treatment conditions are: using ammonia as the reaction gas, heating to 1100° C. at a rate of 8° C. / min and maintaining the temperature for 1.5 h.
[0055] The ceramic treatment conditions are: in an inert atmosphere, heating to 1950° C. at a rate of 5° C. / min and maintaining the temperature for 0.8 h.
[0056] The invention also provides a porous ceramic material prepared by the method.
[0057] Example 3
[0058] This embodiment provides a method for preparing a porous ceramic material based on a BN precursor, comprising the following steps:
[0059] (1) The BN precursor is subjected to an infusible treatment.
[0060] The BN precursor is polyborazine obtained by polymerization of aminoborane monomer. In this embodiment, as a preferred solution, the BN precursor is BN precursor waste and BN precursor waste silk generated during the melt spinning process when the BN fiber is prepared by the organic precursor conversion method.
[0061] The infusibility treatment was carried out under the following conditions: 15° C., air atmosphere, relative humidity of air was 60%, and the treatment time was 18 hours.
[0062] The oxygen content in the BN precursor after the infusibility treatment is 50-70wt%.
[0063] (2) The BN precursor after the infusible treatment is subjected to decarburization treatment and ceramic treatment in sequence to obtain a porous ceramic material.
[0064] The decarburization treatment conditions are: using ammonia as the reaction gas, heating to 1200° C. at a rate of 10° C. / min and keeping the temperature for 2 hours.
[0065] The ceramic treatment conditions are: in an inert atmosphere, heating to 2000° C. at a rate of 3° C. / min and maintaining the temperature for 0.5 h.
[0066] The invention also provides a porous ceramic material prepared by the method.
[0067] Example 4
[0068] This embodiment provides a method for preparing a porous ceramic material based on a BN precursor, comprising the following steps:
[0069] (1) The BN precursor is subjected to an infusible treatment.
[0070] The BN precursor is polyborazine obtained by polymerization of aminoborane monomers. In this embodiment, as a preferred solution, the BN precursor is waste BN precursor generated during the melt spinning process when the BN fiber is prepared by an organic precursor conversion method.
[0071] The infusibility treatment was carried out under the following conditions: at 35° C., in an air atmosphere, with a relative humidity of 20%, and for 3 hours.
[0072] The oxygen content in the BN precursor after the infusibility treatment is 20-45wt%.
[0073] (2) The BN precursor after the infusible treatment is subjected to decarburization treatment and ceramic treatment in sequence to obtain a porous ceramic material.
[0074] The decarburization treatment conditions are: using ammonia as the reaction gas, heating to 800° C. at a rate of 1° C. / min and maintaining the temperature for 0.5 h.
[0075] The ceramic treatment conditions are: in an inert atmosphere, the temperature is raised to 1800° C. at a rate of 6° C. / min and kept at that temperature for 1 hour.
[0076] The invention also provides a porous ceramic material prepared by the method.
[0077] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still modify the technical solutions recorded in the above embodiments, or replace part or all of the technical features therein with equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A method for preparing porous ceramic materials based on BN precursors, It is characterized in that The following steps are involved: The BN precursor is subjected to an infusible treatment, so that the oxygen content in the BN precursor after the infusible treatment is 20-70wt%; The BN precursor after the infusible treatment is subjected to decarburization treatment and ceramic treatment in sequence to obtain a porous ceramic material; The BN precursor includes BN precursor waste and / or BN precursor waste silk generated in the process of preparing BN fibers; The infusibility treatment is carried out under the following conditions: at 15-35°C in an air atmosphere; During the infusibility treatment, the relative humidity of the air is 20-60%; The time of the infusibility treatment is 3-18 hours; The conditions of the decarburization treatment are: using ammonia as the reaction gas and heating at a rate of 1-10°C / min; During the decarburization treatment, the temperature is raised to 800-1200°C and kept for 0.5-2h; The conditions of the ceramic treatment are: heating at a rate of 3-6°C / min; During the ceramic treatment, the temperature is raised to 1800-2000° C. and maintained for 0.5-1 h.
2. A porous ceramic material prepared by the method according to claim 1.
Citation Information
Patent Citations
Near-stoichiometric continuous BN ceramic fiber and preparation method thereof
CN113336556A