High-pressure gas cylinder and manufacturing method thereof
By using a composite structure of metal lining, composite material layer and metal cladding layer on the high-pressure gas cylinder, and using DW-3 low-temperature epoxy adhesive for bonding, the stress concentration and liquid oxygen of the composite gas cylinder in low-temperature environments are solved. compatibility issues, achieving higher impact resistance and anti-leakage effects, simplifying the manufacturing process and reducing costs.
Patent Information
- Application Number
- CN202310161645.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-24
AI Technical Summary
Composite material gas cylinders have problems with stress concentration, microcrack propagation and liquid oxygen compatibility caused by material property mismatch in low-temperature environments, which limits their wide application in the aerospace field.
It adopts a composite structure of metal lining + composite material layer + metal cladding layer, which is bonded by DW-3 low-temperature epoxy glue. The metal cladding layer is 0.3~1mm lightweight aluminum alloy to isolate the composite material layer from liquid oxygen or Contact with liquid hydrogen.
It improves the impact resistance and anti-leakage effect of gas cylinders, solves the defects of composite gas cylinders in liquid oxygen or liquid hydrogen environments, simplifies the manufacturing process, and reduces costs.
Smart Images

Figure CN116146880B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aerospace manufacturing, and in particular relates to a high-pressure gas cylinder and a manufacturing method thereof. Background Art
[0002] With the rapid development of aerospace technology, spacecraft need to perform heavy and complex space missions. At present, most of the spacecraft in the aerospace system, such as artificial satellites, space shuttles, launch vehicles and space stations, need a large number of pressure vessels to store various liquids or gases to maintain the normal operation of subsystems. The development of high-performance high-pressure gas cylinders is crucial for the long-term in-orbit flight of spacecraft.
[0003] Gas cylinders can be divided into two categories according to their application and structure: metal gas cylinders and composite gas cylinders. Traditional aerospace high-pressure gas cylinders are all-metal structures with large mass, low pressure bearing capacity, and low reliability, which gradually cannot meet the needs of aerospace missions. With the development of fiber-reinforced resin-based composite materials, high-pressure gas cylinders gradually adopt metal-lined composite structures to reduce weight and fuel consumption, improve pressure bearing capacity and reliability. Metal-lined composite gas cylinders mostly use titanium alloys and metal liners, which have the characteristics of good air tightness, light weight and high strength. Although composite gas cylinders have been widely used in the aerospace field, for example, the U.S. SCl Industries has developed a cylindrical metal-lined carbon fiber-wound composite gas cylinder for the HS2601 satellite platform propulsion system with a working pressure of 28.96MPa, but there are still many problems.
[0004] Specifically, the service environment of composite gas cylinder parts is relatively harsh. The working environment temperature in liquid hydrogen environment is lower than -253℃, and the working environment in liquid oxygen environment is lower than -183℃. Under low temperature conditions, the mismatch in thermal expansion coefficients between the resin and fiber system leads to obvious stress concentration inside the parts, which further produces microcracks. The cyclic thermal stress caused by high and low temperature cycles during the service of the gas cylinder will cause the microcracks to continue to expand, and then produce defects such as pores, cracks, and delamination. For liquid hydrogen cylinders, it is necessary to overcome ultra-low temperature mechanical properties and hydrogen molecule penetration; and liquid oxygen cylinders are affected by the ignition point and flash point of the material. The composite material itself is prone to high temperature under impact loads such as collisions, resulting in highly active free radicals initiating a chain reaction between the polymer in the material and liquid oxygen, which causes an explosion. The liquid oxygen compatibility problem of the material needs to be overcome.
[0005] Therefore, issues such as composite material performance, permeability, and liquid oxygen compatibility at low temperatures severely limit the wider application of composite gas cylinders in the aerospace field. Summary of the invention
[0006] The present invention aims to provide a high-pressure gas cylinder whose shell wall adopts a composite structure of metal lining + composite material layer + metal cladding layer to solve the problems raised in the background technology.
[0007] To achieve the above-mentioned purpose, the present invention provides a high-pressure gas cylinder, which is used in a liquid oxygen environment or a liquid hydrogen environment, and includes a high-pressure gas cylinder body and a metal cladding layer coated on the outer surface of the high-pressure gas cylinder body. The shell wall of the high-pressure gas cylinder body includes a metal lining and a composite material layer from the inside to the outside, and the metal cladding layer and the composite material layer are bonded to each other by DW-3 low-temperature epoxy adhesive. The metal cladding layer is a lightweight aluminum alloy with a thickness of 0.3 to 1 mm, which is used to isolate the composite material layer from contact with liquid oxygen or liquid hydrogen.
[0008] The present invention also provides a method for manufacturing a high-pressure gas cylinder, wherein the high-pressure gas cylinder is used in a liquid oxygen environment or a liquid hydrogen environment, and comprises a high-pressure gas cylinder body, and a metal coating layer coated on the outer surface of the high-pressure gas cylinder body, wherein the metal coating layer is used to isolate the high-pressure gas cylinder body from contact with liquid oxygen or liquid hydrogen, and the metal coating layer comprises a first metal coating layer and a second metal coating layer, and the method comprises the following steps:
[0009] (1) providing a high-pressure gas cylinder body, the high-pressure gas cylinder body comprising a cylinder body located in the middle, a bottom seal and a head seal respectively arranged at two ends of the cylinder body, and a bottle mouth connected to the head seal, the shell wall of the high-pressure gas cylinder body comprising a metal lining and a composite material layer in sequence from inside to outside;
[0010] (2) providing a first metal coating layer, and coating the DW-3 low-temperature epoxy adhesive on the inner side of the first metal coating layer to form a first adhesive layer, wherein the first metal coating layer includes a bottom cover coating layer matching the shape of the bottom cover, a head cover coating layer matching the shape of the head cover, and a bottle mouth coating layer matching the shape of the bottle mouth;
[0011] (3) sleeve the parts of the first metal coating layer coated with the first adhesive layer onto the parts of the high-pressure gas cylinder body to obtain a first gas cylinder to be cured, wherein the first adhesive layer is sandwiched between the first metal coating layer and the high-pressure gas cylinder body;
[0012] (4) performing a self-tightening treatment and an adhesive curing treatment on the first gas cylinder in sequence, so that the first metal coating layer is tightly bonded to the composite material layer of the gas cylinder body, thereby obtaining a second gas cylinder;
[0013] (5) providing a rectangular second metal coating layer, wherein the length of the second metal coating layer is slightly larger than the circumference of the barrel, and the width of the second metal coating layer is the same as the height of the barrel;
[0014] (6) coating DW-3 low-temperature epoxy adhesive on one side of the second metal coating layer to form a second adhesive layer;
[0015] (7) the second metal coating layer is just covered on the outer surface of the cylinder body to obtain a third gas cylinder to be cured, and the second adhesive layer is sandwiched between the second metal coating layer and the cylinder body;
[0016] (8) The third gas cylinder is subjected to a self-tightening treatment and an adhesive curing treatment in sequence, so that the second metal coating layer is tightly bonded to the composite material layer of the cylinder body, thereby obtaining a fourth gas cylinder.
[0017] In a specific embodiment, the autogenous tightening step in step (4) includes:
[0018] Step A1: applying a low tension to the outer surface of the first metal coating layer with an isolation film for a first winding, so as to preliminarily increase the contact pressure between the first metal coating layer and the high-pressure gas cylinder body;
[0019] Step A2, applying low tension to the isolation film winding area with yellow glue for a second winding, so as to further increase the contact pressure between the first metal coating layer and the high-pressure gas cylinder body;
[0020] and / or,
[0021] The autogenous tightening step in step (8) includes:
[0022] Step A3, applying a low tension to the outer surface of the second metal coating layer with an isolation film for a first winding, so as to preliminarily increase the contact pressure between the second metal coating layer and the high-pressure gas cylinder body;
[0023] Step A4: Use yellow glue to apply low tension to the isolation film winding area for a second winding to further increase the contact pressure between the second metal coating layer and the high-pressure gas cylinder body.
[0024] In a specific embodiment, the adhesive curing step in step (4) comprises:
[0025] Step B1, wrapping the first gas cylinder that has completed the self-tightening treatment with a breathable felt, placing it in a vacuum bag provided with a vacuum nozzle, and sealing it;
[0026] Step B2: Wrap the first gas cylinder in the vacuum bag with a breathable felt, place it vertically in the autoclave with the bottle mouth facing upward, connect the vacuum nozzle to the vacuum tube, and cure the first adhesive layer according to a first preset curing process, wherein the first preset curing process includes:
[0027] The temperature was raised to 60°C at a heating rate of 1°C / min, and kept at 60°C for 8 hours, and then cooled with the furnace. During the entire curing process, the vacuum bag was evacuated to 0.1MPa, and the autoclave was pressurized to 0.05MPa;
[0028] and / or,
[0029] The bonding and curing step in step (8) comprises:
[0030] Step B3, wrapping the third gas cylinder that has completed the self-tightening process with a breathable felt, placing it in a vacuum bag provided with a vacuum nozzle, and sealing it;
[0031] Step B4: Wrap the third gas cylinder in the vacuum bag with a breathable felt, place it vertically in the autoclave with the bottle mouth facing upward, connect the vacuum nozzle to the vacuum tube, and cure the second adhesive layer according to a second preset curing process, wherein the second preset curing process includes:
[0032] The temperature was raised to 60° C. at a heating rate of 1° C. / min, and kept at 60° C. for 8 hours, and then cooled with the furnace. During the entire curing process, the vacuum bag was evacuated to 0.1 MPa, and the autoclave was pressurized to 0.05 MPa.
[0033] In a specific embodiment, the metal coating layer further includes a third metal coating layer, and the step (8) further includes the following steps:
[0034] (9) providing a rectangular third metal coating layer, and coating the DW-3 low-temperature epoxy adhesive on one side of the third metal coating layer to form a third adhesive layer;
[0035] (10) Covering the third metal coating layer on the outer surface of the fourth gas cylinder to obtain a fifth gas cylinder, wherein the third metal coating layer completely covers the second metal coating layer and covers a portion of the bottom coating layer and a portion of the head coating layer, and the third adhesive layer is located on the inner side of the third metal coating layer;
[0036] (11) The fifth gas cylinder is subjected to a self-tightening treatment and an adhesive curing treatment in sequence, so that the third metal coating layer is tightly bonded to the fourth gas cylinder, thereby obtaining the high-pressure gas cylinder.
[0037] In a specific embodiment, the third metal coating layer of the high-pressure gas cylinder includes a main body portion that just covers the second metal coating layer, a first overlap portion and a second overlap portion extending from both ends of the main body portion in a direction away from the main body portion, and a third overlap portion extending from one side of the main body portion along the circumferential direction of the cylinder body, wherein the first overlap portion covers a portion of the bottom coating layer, the second overlap portion covers a portion of the head coating layer, and the third overlap portion covers a portion of the main body portion, a portion of the first overlap portion and a portion of the second overlap portion.
[0038] In a specific embodiment, along the long axis direction of the high-pressure gas cylinder, the lengths of the first overlapping portion and the second overlapping portion are both 15 to 20 mm, and along the circumferential direction of the high-pressure gas cylinder, the length of the third overlapping portion is 15 to 20 mm.
[0039] In a specific embodiment, the step (2) also includes the step of anodizing the provided first metal coating layer, the step (5) also includes the step of anodizing the provided second metal coating layer, and the step (9) also includes the step of anodizing the provided third metal coating layer.
[0040] In a specific embodiment, the metal coating layer is a lightweight aluminum alloy with a thickness of 0.3 to 1 mm.
[0041] The present invention also provides a high-pressure gas cylinder, which is manufactured using the high-pressure gas cylinder manufacturing method described above.
[0042] The beneficial effects of the present invention include at least:
[0043] 1. The present invention provides a high-pressure gas cylinder, comprising a high-pressure gas cylinder body, and a metal cladding layer coated on the outer surface of the high-pressure gas cylinder body, the shell wall of the high-pressure gas cylinder body comprises a metal lining and a composite material layer from the inside to the outside, the metal cladding layer and the composite material layer are bonded by DW-3 low-temperature epoxy adhesive, and the metal cladding layer is a lightweight aluminum alloy with a thickness of 0.3 to 1 mm; thus, the shell wall of the high-pressure gas cylinder adopts a composite structure of metal lining + composite material layer + metal cladding layer, and the composite material layer is isolated from contact with liquid oxygen or liquid hydrogen by the metal cladding layer, so as to solve the defects of the high-pressure gas cylinder in the prior art when used in a liquid oxygen or liquid hydrogen environment, and has the advantages of good impact resistance and good anti-leakage effect.
[0044] 2. In the manufacturing method of the high-pressure gas cylinder provided by the present invention, the metal coating layer adopts segmented coating and adhesive curing. First, the bottom cover, the head cover and the bottle mouth area of the high-pressure gas cylinder body are coated with metal by the first metal coating layer, and then the barrel area of the high-pressure gas cylinder body is coated with metal by the second metal coating layer. Finally, the outermost layer of the high-pressure gas cylinder body that has completed the first metal coating and the second metal coating is coated with metal again, so that the metal coating layer can be closely attached to the composite material layer and completely cover the composite material layer. The operation method does not require complex tooling design and has the advantages of simple operation and low cost.
[0045] In addition to the above-described purposes, features and advantages, the present invention has other purposes, features and advantages. The present invention will be further described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 A schematic structural diagram of a high-pressure gas cylinder body at one angle provided by an embodiment of the present invention;
[0047] Figure 2 A schematic structural diagram of a high-pressure gas cylinder provided at one angle according to an embodiment of the present invention;
[0048] Figure 3 A schematic structural diagram of a high-pressure gas cylinder provided by an embodiment of the present invention from another angle;
[0049] Figure 4 A schematic flow chart of the steps of a method for manufacturing a high-pressure gas cylinder provided in one embodiment of the present invention;
[0050] Figure 5 A schematic structural diagram of the first gas cylinder corresponding to step S30 at one angle;
[0051] Figure 6 This is a structural schematic diagram of placing the first gas cylinder in an autoclave for adhesive curing corresponding to step S40;
[0052] Figure 7 is a schematic structural diagram of a third gas cylinder corresponding to step S70 at an angle;
[0053] Figure 8 This is a physical picture of the product prepared by the manufacturing method of the present invention.
[0054] Description of reference numerals:
[0055]
[0056] DETAILED DESCRIPTION
[0057] The embodiments of the present invention are described in detail below with reference to the accompanying drawings. However, the present invention can be defined and covered by various different implementations according to the claims.
[0058] See also Figures 1 to 3 The present invention provides a high-pressure gas cylinder 100, which is an improved composite material gas cylinder for use in a liquid oxygen environment or a liquid hydrogen environment, and can effectively avoid the problems of liquid oxygen compatibility and liquid hydrogen permeability.
[0059] The high-pressure gas cylinder 100 includes a high-pressure gas cylinder body 10 and a metal cladding layer 20 coated on the outer surface of the high-pressure gas cylinder body 10. The shell wall 110 of the high-pressure gas cylinder body 10 includes a metal lining 111 and a composite material layer 112 from the inside to the outside. The metal cladding layer 20 and the composite material layer are bonded by DW-3 low-temperature epoxy adhesive. The metal cladding layer 20 is a lightweight aluminum alloy with a thickness of 0.3 to 1 mm, which is used to isolate the composite material layer 112 from contact with liquid oxygen or liquid hydrogen.
[0060] The shell wall 110 of the high-pressure gas cylinder 100 of the present invention adopts a composite structure of metal lining + composite material layer + metal coating layer, which gives full play to the respective advantages of metal and composite material and meets the requirements of impact resistance and leakage prevention; moreover, the composite material layer is protected by the double layers of metal lining and metal coating layer, which can effectively avoid the problems of liquid oxygen compatibility and liquid hydrogen permeability.
[0061] In this embodiment, the metal lining 111 is an aluminum alloy lining.
[0062] In this embodiment, the composite material layer 112 is a fiber-reinforced resin-based composite material.
[0063] In this embodiment, the metal cladding layer 20 uses Al-Mn series rust-proof aluminum alloy 3A21 as the metal cladding material of the composite material layer. The alloy is characterized by high strength, good plasticity and excellent processing performance.
[0064] In this embodiment, the high-pressure gas cylinder body 10 has a receiving space for accommodating gas or liquid, and includes a cylinder body 11 located in the middle, a bottom seal 12 and a head seal 13 respectively arranged at both ends of the cylinder body 11, and a bottle mouth 14 connected to the head seal 13.
[0065] In this embodiment, the cylinder body 11 is a hollow cylindrical body, the bottom seal 12 and the head seal 13 are ellipsoidal heads, butterfly heads or hemispherical heads, and the two have the same structure, but a through hole is provided at the connection position between the head seal 13 and the bottle mouth 14 to connect the bottle mouth 14 with the receiving space of the high-pressure gas cylinder body 10. The bottle mouth 14 adopts a conventional design and serves as an inlet when filling the receiving space with gas or liquid.
[0066] The metal cladding layer 20 completely covers the high-pressure gas cylinder body 10 to prevent the composite material layer 112 from contacting liquid oxygen or liquid hydrogen. The metal cladding layer 20 can have exactly the same shape as the high-pressure gas cylinder body 10. In the present embodiment, the metal cladding layer 20 has the same shape as the high-pressure gas cylinder body 10.
[0067] In this embodiment, the metal cladding layer 20 includes a first metal cladding layer 21 , a second metal cladding layer 22 , and a third metal cladding layer 23 .
[0068] The first metal coating layer 21 includes a bottom cover coating layer 211 matching the shape of the bottom cover 12, a head cover coating layer 212 matching the shape of the head cover 13, and a bottle mouth cover layer 213 matching the shape of the bottle mouth 14. The shape matching here can be considered as the same shape.
[0069] The second metal coating 22 and the third metal coating 23 both have two states. Before processing, the second metal coating 22 and the third metal coating 23 are both rectangular. After processing, the second metal coating 22 matches the shape of the barrel 11, and the third metal coating 23 covers the outer surface of the second metal coating 22, and the area is slightly larger than the shape of the barrel 11. The part exceeding the barrel 11 covers the bottom coating 211, the head coating 212 and the second metal coating 22.
[0070] It can be understood that in the above description, the metal cladding layer 20 has the same shape as the high-pressure gas cylinder body 10, which means that after processing, the metal cladding layer 20 has the same shape as the high-pressure gas cylinder body 10.
[0071] It should be noted that the shape matching mentioned above refers to the same shape. For example, the height of the barrel is L, and the radius of the barrel is r. Then, before processing, ignoring the thickness of the barrel, the length of the rectangular second metal coating is 2πr. Considering the thickness of the barrel, assuming that the thickness of the barrel is d, the length of the rectangular second metal coating is 2π(r+d); the width of the rectangular second metal coating is L. In this way, the second metal coating 22 is wound along the circumference of the barrel 11, and the second metal coating 22 just covers the barrel 11.
[0072] After processing, the third metal coating 23 of the high-pressure gas cylinder 100 includes a main body 231 that just covers the second metal coating 22, a first overlap portion 232 and a second overlap portion 233 extending from both ends of the main body 231 in a direction away from the main body 231, and a third overlap portion 234 extending from one side of the main body 231 along the circumferential direction of the barrel 11, wherein the first overlap portion 232 covers a portion of the bottom coating 211, the second overlap portion 233 covers a portion of the head coating 212, and the third overlap portion 234 covers a portion of the main body 231, a portion of the first overlap portion 232 and a portion of the second overlap portion 233.
[0073] Preferably, along the long axis direction of the high-pressure gas cylinder 100, the lengths of the first overlap portion 232 and the second overlap portion 233 are both 15 to 20 mm, and along the circumferential direction of the high-pressure gas cylinder 100, the length of the third overlap portion 234 is 15 to 20 mm.
[0074] That is, the width of the rectangular third metal coating 23 is the length of the barrel 11 plus the first overlap portion 232 and the second overlap portion 233, and the length of the third metal coating 23 is the circumferential length of the second metal coating 22 plus the length of the third overlap portion 234.
[0075] In this embodiment, the first overlap portion 232 covers the connection position between the main body 231 and the bottom cover layer 211, the second overlap portion 233 covers the connection position between the main body 231 and the head cover layer 212, and the third overlap portion 234 covers the intersection position of the two side edges of the main body 231 itself. In this way, it can better ensure that the metal cover layer 20 can completely cover the composite material layer, thereby solving the problems existing in the prior art.
[0076] The present invention also provides a method for manufacturing a high-pressure gas cylinder. The structure of the high-pressure gas cylinder is as described above. Since the structural part of the high-pressure gas cylinder has been described in detail above, it will not be repeated below.
[0077] See also Figure 4 , the manufacturing method comprises the following steps:
[0078] S10, providing a high-pressure gas cylinder body 10, wherein the high-pressure gas cylinder body 10 comprises a cylinder body 11 located in the middle, a bottom cover 12 and a head cover 13 respectively arranged at two ends of the cylinder body 11, and a bottle mouth 14 connected to the head cover 13, and a shell wall 110 of the high-pressure gas cylinder body 10 comprises a metal lining 111 and a composite material layer 112 in sequence from inside to outside;
[0079] The high-pressure gas cylinder body can be manufactured using conventional processing methods or directly purchased commercially.
[0080] S20, providing a first metal cladding layer 21, and coating the DW-3 low-temperature epoxy adhesive on the inner side of the first metal cladding layer 21 to form a first adhesive layer 31, wherein the first metal cladding layer 21 includes a bottom cladding layer 211 matching the shape of the bottom cladding 12, a head cladding layer 212 matching the shape of the head cladding 13, and a bottle mouth cladding layer 213 matching the shape of the bottle mouth 14;
[0081] The manufacturing method of each part of the first metal coating layer 21 adopts a conventional processing method, which may specifically include: based on the structural parameters of the high-pressure gas cylinder body 10, calculating the structural parameters of each part of the first metal coating layer 21, then designing a mold, and then processing based on the mold, and the processing technology includes multiple stamping, drawing, flanging and hole expansion.
[0082] The DW-3 low-temperature epoxy adhesive applied in this step is used to connect the first metal cladding layer 21 and the high-pressure gas cylinder body 10 .
[0083] S30, sleeve each part of the first metal coating layer 21 coated with the first adhesive layer 31 on each part of the high-pressure gas cylinder body 10 to obtain a first gas cylinder to be cured, wherein the first adhesive layer is sandwiched between the first metal coating layer 21 and the high-pressure gas cylinder body 10;
[0084] Specifically, the bottom cover layer 211 coated with the first glue layer is respectively sleeved on the bottom cover 12, and the head cover layer 212 coated with the first glue layer 31 is sleeved on the head cover 13, and then the bottle mouth cover layer 213 coated with the first glue layer 31 is sleeved on the bottle mouth 14 and one end of the bottle mouth cover layer 213 is inserted into the gap between the head cover layer 211 and the head cover 13, and finally the gap around the bottle mouth 14 is filled by glue injection, so as to obtain the first gas cylinder to be cured.
[0085] Please refer to Figure 5 , Figure 5 This is a schematic structural diagram of the first gas cylinder corresponding to step S30 at one angle.
[0086] S40, sequentially performing a self-tightening treatment and an adhesive curing treatment on the first gas cylinder, so that the first metal coating layer 21 is tightly bonded to the composite material layer 112 of the gas cylinder body 10, to obtain a second gas cylinder;
[0087] The self-tightening process is specifically as follows:
[0088] Step A1: applying a low tension to the outer surface of the first metal coating layer 21 with an isolation film 41 for a first winding, so as to preliminarily increase the contact pressure between the first metal coating layer 21 and the high-pressure gas cylinder body 10;
[0089] Specifically, the number of turns of the first winding can be determined according to the operation process, and can be 5 turns, or 6 turns, etc., which are not exhaustively listed here, and only need to be able to prevent the first metal coating layer from moving.
[0090] Step A2: Use yellow glue 42 to apply low tension to the isolation film winding area for a second winding to further increase the contact pressure between the first metal coating layer 21 and the high-pressure gas cylinder body 10.
[0091] Specifically, the denser the second winding is, the better. When all the winding areas of the isolation film are wound, it can be regarded as a condition for the end of the second winding.
[0092] The step of self-tightening treatment is provided to ensure that the first metal coating layer is positioned correctly after the adhesive is cured.
[0093] The bonding and curing step comprises:
[0094] Step B1, wrapping the first gas cylinder that has completed the self-tightening treatment with a breathable felt 43, placing it in a vacuum bag 50 provided with a vacuum nozzle 51, and sealing it;
[0095] In this embodiment, the vacuum bag is composed of an upper vacuum bag and a lower vacuum bag. The first gas cylinder wrapped with breathable felt 43 is first placed horizontally in the lower vacuum bag, and then the first gas cylinder is covered with an upper vacuum bag, and then sealed with black glue 60.
[0096] Step B2: Wrap the first gas cylinder in the vacuum bag 50 with the breathable felt 43, and place it vertically in the autoclave 70 with the bottle mouth facing upwards, connect the vacuum nozzle 51 to the vacuum tube 71, and cure the first adhesive layer according to a first preset curing process, wherein the first preset curing process includes:
[0097] The temperature was raised to 60° C. at a heating rate of 1° C. / min, and kept at 60° C. for 8 hours, and then cooled with the furnace. During the entire curing process, the vacuum bag was evacuated to 0.1 MPa, and the autoclave was pressurized to 0.05 MPa.
[0098] The purpose of wrapping with breathable felt again in this step is to prevent the vacuum bag from being accidentally scratched or torn during subsequent tests; the bottle is placed vertically in the autoclave with the bottle mouth facing upward to prevent the rubber layer from flowing and causing blockage of the bottle mouth.
[0099] In this embodiment, after the first gas cylinder is placed vertically on the autoclave workbench, the bottom and the top of the first gas cylinder need to be fixed to prevent movement.
[0100] Please refer to Figure 6 , Figure 6 This is a structural schematic diagram of placing the first gas cylinder in an autoclave for adhesive curing corresponding to step S40.
[0101] S50, providing a rectangular second metal coating layer 22, wherein the length of the second metal coating layer is slightly larger than the circumference of the barrel, and the width of the second metal coating layer is the same as the height of the barrel;
[0102] The size of the second metal coating 22 is calculated based on the size of the barrel. The second metal coating 22 needs to just cover the outer surface of the barrel. Considering the shell wall thickness of the barrel, the length of the second metal coating needs to be slightly larger than the circumference of the barrel.
[0103] S60, coating DW-3 low-temperature epoxy adhesive on one side of the second metal coating layer to form a second adhesive layer;
[0104] The DW-3 low temperature epoxy adhesive applied in this step is used to connect the second metal cladding layer and the barrel.
[0105] S70, the second metal coating layer is just covered on the outer surface of the cylinder body to obtain a third gas cylinder to be cured, and the second adhesive layer is sandwiched between the second metal coating layer and the cylinder body;
[0106] The second metal coating 22 has two states. Before processing, the second metal coating 22 is rectangular. During processing, the first side of the second metal coating 22 is first bonded to the barrel, and then the second metal coating 22 is rolled along the circumferential direction of the barrel 11. After rolling, the second side of the second metal coating 22 opposite to the first side is connected to the first side, so that the second metal coating 22 just covers the outer surface of the barrel 22. At this time, the second metal coating has the same shape as the barrel, which is a cylindrical barrel.
[0107] Please refer to Figure 7 , Figure 7 It is a structural schematic diagram of the third gas cylinder corresponding to step S70 at an angle.
[0108] S80, sequentially performing a self-tightening treatment and an adhesive curing treatment on the third gas cylinder so that the second metal coating layer is tightly bonded to the composite material layer of the cylinder body, thereby obtaining a fourth gas cylinder.
[0109] The autogenous tightening process comprises:
[0110] Step A3, applying low tension to the outer surface of the second metal coating layer with an isolation film for the first winding, so as to preliminarily increase the contact pressure between the second metal coating layer and the barrel;
[0111] Step A4: Use yellow glue to apply low tension to the isolation film winding area for a second winding to further increase the contact pressure between the second metal coating layer and the cylinder body.
[0112] The step of self-tightening treatment is provided to ensure that the second metal coating layer is positioned correctly after the adhesive is cured.
[0113] The bonding and curing step comprises:
[0114] Step B3, wrapping the third gas cylinder that has completed the self-tightening process with a breathable felt, placing it in a vacuum bag provided with a vacuum nozzle, and sealing it;
[0115] Step B4: Wrap the third gas cylinder in the vacuum bag with a breathable felt, place it vertically in the autoclave with the bottle mouth facing upward, connect the vacuum nozzle to the vacuum tube, and cure the second adhesive layer according to a second preset curing process, wherein the second preset curing process includes:
[0116] The temperature was raised to 60° C. at a heating rate of 1° C. / min, and kept at 60° C. for 8 hours, and then cooled with the furnace. During the entire curing process, the vacuum bag was evacuated to 0.1 MPa, and the autoclave was pressurized to 0.05 MPa.
[0117] The purpose of wrapping with breathable felt again in this step is to prevent the vacuum bag from being accidentally scratched or torn during subsequent tests; the bottle is placed vertically in the autoclave with the bottle mouth facing upward to prevent the rubber layer from flowing and causing blockage of the bottle mouth.
[0118] It should be noted that the high-pressure gas cylinders are named as the first gas cylinder, the second gas cylinder, the third gas cylinder, the fourth gas cylinder, etc. in the method steps in order to distinguish the different states of the high-pressure gas cylinders during the processing process. For example, the first gas cylinder refers to the state in which the first metal coating layer has just been coated, and the second gas cylinder refers to the state in which the first adhesive layer has been completely cured. The third gas cylinder refers to the state in which the second metal coating layer has just been coated, and the fourth gas cylinder refers to the state in which the second adhesive layer has been completely cured.
[0119] Preferably, the manufacturing method further comprises the step of covering the third metal cladding layer on the second metal cladding layer and the connection between the second metal cladding layer and other parts. Specifically,
[0120] Please refer to Figure 2 and Figure 3 , the step S80 further includes the following steps:
[0121] Step D1, providing a rectangular third metal cladding layer, and coating the DW-3 low-temperature epoxy adhesive on one side of the third metal cladding layer to form a third adhesive layer;
[0122] Specifically, through orthogonal process experiments and simulations, it was found that the reasonable overlap length of the outermost third metal coating layer in the axial and circumferential directions is 15 to 20 mm, and the third metal coating layer size required to wrap the gas cylinder is cut out.
[0123] In this embodiment, the width of the rectangular third metal coating 23 is the length of the barrel 11 plus the first overlap portion 232 and the second overlap portion 233, and the length of the third metal coating 23 is the circumferential length of the second metal coating 22 plus the length of the third overlap portion 234.
[0124] The DW-3 low temperature epoxy adhesive is applied to connect the third metal cladding layer with the first metal cladding layer and the second metal cladding layer.
[0125] Step D2, covering the outer surface of the fourth gas cylinder with the third metal coating layer to obtain a fifth gas cylinder, wherein the third metal coating layer completely covers the second metal coating layer and covers part of the bottom cover and part of the head cover, and the third adhesive layer is located on the inner side of the third metal coating layer;
[0126] The third metal coating 23 has two states. Before processing, the third metal coating 23 is rectangular. During processing, the first side of the third metal coating 23 is first bonded to the second metal coating, and then the third metal coating 23 is rolled along the circumferential direction of the barrel 11. After the rolling is completed, the second side of the third metal coating 23 opposite to the first side exceeds the first side and is connected to the main body of the third metal coating 23, that is, the third overlapping portion 234 of the third metal coating 23 is connected to the main body 231; the first overlapping portion 232 is connected to the bottom coating 211, and the second overlapping portion 233 is connected to the head coating 212.
[0127] Step D3, sequentially performing a self-tightening treatment and an adhesive curing treatment on the fifth gas cylinder so that the third metal coating layer is tightly bonded to the fourth gas cylinder to obtain the high-pressure gas cylinder.
[0128] The self-tightening process is specifically as follows:
[0129] Step A5, applying a low tension to the outer surface of the third metal coating layer 23 with an isolation film for the first winding, so as to preliminarily increase the contact pressure between the third metal coating layer 23 and the fourth gas cylinder;
[0130] Specifically, the number of turns of the first winding can be determined according to the operation process, and can be 5 turns, or 6 turns, etc., which are not exhaustively listed here, and only need to be able to prevent the first metal coating layer from moving.
[0131] Step A6: Use yellow glue to apply low tension to the isolation film winding area for a second winding to further increase the contact pressure between the third metal coating layer and the fourth gas cylinder.
[0132] Specifically, the denser the second winding is, the better. When all the winding areas of the isolation film are wound, it can be regarded as a condition for the end of the second winding.
[0133] The step of self-tightening treatment is provided to ensure that the third metal cladding layer is positioned correctly after the adhesive is cured.
[0134] The bonding and curing step comprises:
[0135] Step B5, wrapping the fifth gas cylinder that has completed the self-tightening process with a breathable felt, placing it in a vacuum bag provided with a vacuum nozzle, and sealing it;
[0136] In this embodiment, the vacuum bag consists of an upper vacuum bag and a lower vacuum bag. The fifth gas cylinder wrapped with breathable felt is first placed horizontally in the lower vacuum bag, and then the fifth gas cylinder is covered with an upper vacuum bag, and then sealed with black glue.
[0137] Step B6: Wrap the fifth gas cylinder in the vacuum bag with breathable felt, place it vertically in the autoclave with the bottle mouth facing upward, connect the vacuum nozzle to the vacuum tube, and cure the third adhesive layer according to the second preset curing process, wherein the third preset curing process includes:
[0138] The temperature was raised to 60° C. at a heating rate of 1° C. / min, and kept at 60° C. for 8 hours, and then cooled with the furnace. During the entire curing process, the vacuum bag was evacuated to 0.1 MPa, and the autoclave was pressurized to 0.05 MPa.
[0139] The purpose of wrapping with breathable felt again in this step is to prevent the vacuum bag from being accidentally scratched or torn during subsequent tests; the bottle is placed vertically in the autoclave with the bottle mouth facing upward to prevent the rubber layer from flowing and causing blockage of the bottle mouth.
[0140] In this embodiment, after the fifth gas cylinder is placed vertically on the autoclave workbench, the bottom and the top of the fifth gas cylinder need to be fixed to prevent movement.
[0141] Preferably, the step S20 further includes the step of anodizing the provided first metal cladding layer, the step S50 further includes the step of anodizing the provided second metal cladding layer, and the step D1 further includes the step of anodizing the provided third metal cladding layer.
[0142] Specifically, the anodizing treatment adopts phosphoric acid anodizing treatment.
[0143] By anodizing the first metal cladding layer, the second metal cladding layer and the third metal cladding layer, the roughness of the surfaces of the first metal cladding layer, the second metal cladding layer and the third metal cladding layer can be increased to improve the bonding strength with the DW-3 low-temperature epoxy adhesive.
[0144] Preferably, the metal cladding layer is a lightweight aluminum alloy with a thickness of 0.3 to 1 mm.
[0145] When the thickness of the metal cladding layer is less than 0.3 mm, the metal cladding layer is easily broken during the stamping process. When the thickness of the metal cladding layer is greater than 1 mm, it is difficult to form.
[0146] The present invention also provides a high-pressure gas cylinder, which is manufactured by the manufacturing method described above. Figure 8 , Figure 8 This is a physical picture of the product prepared by the manufacturing method of the present invention.
[0147] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. A method for manufacturing a high-pressure gas cylinder, characterized in that: The high-pressure gas cylinder is used in a liquid oxygen environment or a liquid hydrogen environment, and comprises a high-pressure gas cylinder body and a metal coating layer coated on the outer surface of the high-pressure gas cylinder body, wherein the metal coating layer is used to isolate the high-pressure gas cylinder body from contact with liquid oxygen or liquid hydrogen, and the metal coating layer comprises a first metal coating layer and a second metal coating layer. The method comprises the following steps: (1) providing a high-pressure gas cylinder body, the high-pressure gas cylinder body comprising a cylinder body located in the middle, a bottom seal and a head seal respectively arranged at two ends of the cylinder body, and a bottle mouth connected to the head seal, the shell wall of the high-pressure gas cylinder body comprising a metal lining and a composite material layer in sequence from inside to outside; (2) providing a first metal coating layer, and coating the inner side of the first metal coating layer with DW-3 low-temperature epoxy adhesive to form a first adhesive layer, wherein the first metal coating layer includes a bottom cover coating layer matching the bottom cover shape, a head cover coating layer matching the head cover shape, and a bottle mouth coating layer matching the bottle mouth shape; (3) sleeve the parts of the first metal coating layer coated with the first adhesive layer onto the parts of the high-pressure gas cylinder body to obtain a first gas cylinder to be cured, wherein the first adhesive layer is sandwiched between the first metal coating layer and the high-pressure gas cylinder body; (4) performing a self-tightening treatment and an adhesive curing treatment on the first gas cylinder in sequence, so that the first metal coating layer is tightly bonded to the composite material layer of the gas cylinder body, thereby obtaining a second gas cylinder; (5) providing a rectangular second metal coating layer, wherein the length of the second metal coating layer is slightly larger than the circumference of the barrel, and the width of the second metal coating layer is the same as the height of the barrel; (6) coating DW-3 low-temperature epoxy adhesive on one side of the second metal coating layer to form a second adhesive layer; (7) the second metal coating layer is just covered on the outer surface of the cylinder body to obtain a third gas cylinder to be cured, and the second adhesive layer is sandwiched between the second metal coating layer and the cylinder body; (8) The third gas cylinder is subjected to a self-tightening treatment and an adhesive curing treatment in sequence, so that the second metal coating layer is tightly bonded to the composite material layer of the cylinder body, thereby obtaining a fourth gas cylinder.
2. The method for manufacturing a high-pressure gas cylinder according to claim 1, characterized in that: The autogenous tightening step in step (4) comprises: Step A1: applying a low tension to the outer surface of the first metal coating layer with an isolation film for a first winding, so as to preliminarily increase the contact pressure between the first metal coating layer and the high-pressure gas cylinder body; Step A2, applying low tension to the isolation film winding area with yellow glue for a second winding, so as to further increase the contact pressure between the first metal coating layer and the high-pressure gas cylinder body; and / or, The autogenous tightening step in step (8) includes: Step A3, applying a low tension to the outer surface of the second metal coating layer with an isolation film for a first winding, so as to preliminarily increase the contact pressure between the second metal coating layer and the high-pressure gas cylinder body; Step A4: Use yellow glue to apply low tension to the isolation film winding area for a second winding to further increase the contact pressure between the second metal coating layer and the high-pressure gas cylinder body.
3. The method for manufacturing a high-pressure gas cylinder according to claim 1, characterized in that: The bonding and curing step in step (4) comprises: Step B1, wrapping the first gas cylinder that has completed the self-tightening treatment with a breathable felt, placing it in a vacuum bag provided with a vacuum nozzle, and sealing it; Step B2: Wrap the first gas cylinder in the vacuum bag with a breathable felt, place it vertically in the autoclave with the bottle mouth facing upward, connect the vacuum nozzle to the vacuum tube, and cure the first adhesive layer according to a first preset curing process, wherein the first preset curing process includes: The temperature was raised to 60°C at a heating rate of 1°C / min, and kept at 60°C for 8 hours, and then cooled with the furnace. During the entire curing process, the vacuum bag was evacuated to 0.1MPa, and the autoclave was pressurized to 0.05MPa; and / or, The bonding and curing step in step (8) comprises: Step B3, wrapping the third gas cylinder that has completed the self-tightening process with a breathable felt, placing it in a vacuum bag provided with a vacuum nozzle, and sealing it; Step B4: Wrap the third gas cylinder in the vacuum bag with a breathable felt, place it vertically in the autoclave with the bottle mouth facing upward, connect the vacuum nozzle to the vacuum tube, and cure the second adhesive layer according to a second preset curing process, wherein the second preset curing process includes: The temperature was raised to 60° C. at a heating rate of 1° C. / min, and kept at 60° C. for 8 hours, and then cooled with the furnace. During the entire curing process, the vacuum bag was evacuated to 0.1 MPa, and the autoclave was pressurized to 0.05 MPa.
4. The method for manufacturing a high-pressure gas cylinder according to any one of claims 1 to 3, characterized in that: The metal coating layer further includes a third metal coating layer, and the step (8) further includes the following steps: (9) providing a rectangular third metal coating layer, and coating the DW-3 low-temperature epoxy adhesive on one side of the third metal coating layer to form a third adhesive layer; (10) Covering the third metal coating layer on the outer surface of the fourth gas cylinder to obtain a fifth gas cylinder, wherein the third metal coating layer completely covers the second metal coating layer and covers a portion of the bottom coating layer and a portion of the head coating layer, and the third adhesive layer is located on the inner side of the third metal coating layer; (11) The fifth gas cylinder is subjected to a self-tightening treatment and an adhesive curing treatment in sequence, so that the third metal coating layer is tightly bonded to the fourth gas cylinder, thereby obtaining the high-pressure gas cylinder.
5. The method for manufacturing a high-pressure gas cylinder according to claim 4, characterized in that: The third metal coating layer of the high-pressure gas cylinder includes a main body portion just covering the second metal coating layer, a first overlap portion and a second overlap portion extending from both ends of the main body portion in a direction away from the main body portion, and a third overlap portion extending from one side of the main body portion along the circumferential direction of the cylinder body, wherein the first overlap portion covers a portion of the bottom coating layer, the second overlap portion covers a portion of the head coating layer, and the third overlap portion covers a portion of the main body portion, a portion of the first overlap portion and a portion of the second overlap portion.
6. The method for manufacturing a high-pressure gas cylinder according to claim 5, characterized in that: Along the long axis direction of the high-pressure gas cylinder, the lengths of the first overlapping portion and the second overlapping portion are both 15 to 20 mm, and along the circumferential direction of the high-pressure gas cylinder, the length of the third overlapping portion is 15 to 20 mm.
7. The method for manufacturing a high-pressure gas cylinder according to claim 4, characterized in that: The step (2) further includes the step of anodizing the first metal coating layer provided, the step (5) further includes the step of anodizing the second metal coating layer provided, and the step (9) further includes the step of anodizing the third metal coating layer provided.
8. The method for manufacturing a high-pressure gas cylinder according to claim 4, characterized in that: The metal cladding layer is a light aluminum alloy with a thickness of 0.3 to 1 mm.
9. A high-pressure gas cylinder, characterized in that: The high-pressure gas cylinder is manufactured by the method for manufacturing a high-pressure gas cylinder according to any one of claims 1 to 8.
Citation Information
Patent Citations
Spherical composite gas cylinder for spaceflight
CN105674041A
Die-cast formation gas storage cylinder and manufacturing method thereof
CN111271595A
Low-temperature high-pressure gas cylinder capable of directly filling LNG and avoiding BOG (boil off gas) emission
CN111623230A
Composite material gas cylinder liquid oxygen isolation protection layer and mounting method
CN113217804A
Method for manufacturing metal-plastic high pressure tank and a metal-plastic tank