Diffusion method and solar cell manufacturing method
By adopting a two-step diffusion process and variable-temperature oxygen-containing propulsion technology in the diffusion process of solar cells, the problem of shallow junctions and high sheet resistance in PN junction preparation is solved, and the photoelectric conversion efficiency and battery performance of solar cells are improved.
Patent Information
- Application Number
- CN202310293657.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-23
AI Technical Summary
The existing preparation method of PN junction in solar cells is difficult to achieve shallow junction and high sheet resistance, which affects the performance of the cell.
A two-step diffusion process is adopted, by controlling the gas flow and temperature during the heating and cooling process in the diffusion furnace, and utilizing phosphorus diffusion and variable temperature oxygen-containing propulsion technology to form a shallow junction while improving diffusion uniformity and gettering effect.
It achieves the formation of shallower junction depth, improves the photoelectric conversion efficiency and battery performance of solar cells, and meets the demand for high sheet resistance.
Smart Images

Figure CN116153772B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of solar cells, and in particular to a diffusion method and a method for manufacturing a solar cell. Background Art
[0002] The diffusion process is a step in the production of solar cells. Specifically, diffusion is the process of preparing the PN junction, which is the core structure of the solar cell. In the current production of solar cells, the preparation method of the PN junction mostly adopts a low-pressure diffusion process to improve the diffusion uniformity and thus improve the quality of the PN junction. The quality of the PN junction has an important influence on the efficiency of the solar cell. The better the PN junction quality, the higher the battery performance.
[0003] As the process continues to improve, the PN junction is gradually developing towards a shallow junction with high square resistance. Therefore, how to obtain a shallow junction with high square resistance in solar cells is a topic that the industry is considering. Summary of the invention
[0004] In view of the above shortcomings of the related art, the purpose of the present disclosure is to provide a diffusion method and a solar cell manufacturing method to solve the technical problem of low square resistance of solar cells in the related art.
[0005] The first aspect of the present disclosure provides a diffusion method, which includes at least two diffusion processes, each diffusion process including the following steps:
[0006] When the silicon wafer is placed in a diffusion furnace, a source is supplied to the diffusion furnace to diffuse phosphorus into the silicon wafer;
[0007] The temperature in the diffusion furnace is raised to push the phosphorus into the silicon wafer;
[0008] The temperature in the diffusion furnace is lowered based on the temperature at the end of the heating process, and oxygen is introduced during the temperature reduction process to perform temperature-variable oxygen-containing propulsion on the silicon wafer;
[0009] After at least two steps of source-through pushing processes, the temperature inside the diffusion furnace is lowered, and then the diffusion furnace is opened to take out the silicon wafer.
[0010] Optionally, in the first diffusion process of the at least two-step diffusion process, the temperature in the diffusion furnace is increased, including:
[0011] The temperature in the diffusion furnace is raised within a range of 825-840°C, and large nitrogen and small nitrogen without phosphorus are introduced. The flow rate of large nitrogen is 1200-1500sccm, and the flow rate of small nitrogen without phosphorus is 400-600sccm. The heating time range is 6-8min.
[0012] Optionally, in the first diffusion process of the at least two-step diffusion process, the temperature in the diffusion furnace is lowered based on the temperature at the end of the temperature increase, and the temperature reduction range is 20-30° C.;
[0013] When the temperature is lowered, oxygen is introduced to perform variable temperature oxygen-containing advancement of the silicon wafer, including:
[0014] During cooling, oxygen, bulk nitrogen and non-phosphorus-carrying nitrogen are introduced, the flow range of oxygen is 900-1200sccm, the flow range of bulk nitrogen is 600-900sccm, the flow range of non-phosphorus-carrying nitrogen is 400-600sccm, and the cooling time range is 7-9min.
[0015] Optionally, in a first diffusion process of at least two diffusion processes, a source is passed into a diffusion furnace to diffuse phosphorus into the silicon wafer, comprising:
[0016] The temperature in the diffusion furnace is controlled at 775-790°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow rate of oxygen is 450-650sccm, and the flow rate of phosphorus-carrying nitrogen is 700-850sccm. The time range is 2-4min.
[0017] Optionally, the at least two-step diffusion process is configured as a two-step diffusion process, wherein in the second step diffusion process, a source is passed into the diffusion furnace to diffuse phosphorus into the silicon wafer, comprising:
[0018] The temperature in the diffusion furnace is controlled at 795-810°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow rate of oxygen is 450-650sccm, and the flow rate of phosphorus-carrying nitrogen is 700-850sccm. The time range is 3-5min.
[0019] Optionally, in the second diffusion process, the temperature in the diffusion furnace is increased, including:
[0020] The temperature in the diffusion furnace is raised in the range of 850-870°C, and large nitrogen and small nitrogen without phosphorus are introduced. The flow rate of large nitrogen is in the range of 1200-1500sccm, and the flow rate of small nitrogen without phosphorus is in the range of 400-600sccm. The heating time range is 7-9min.
[0021] Optionally, in the second diffusion process, the temperature in the diffusion furnace is lowered based on the temperature at the end of the heating process, and the temperature reduction range is 20-30°C;
[0022] When the temperature is lowered, oxygen is introduced to perform variable temperature oxygen-containing advancement of the silicon wafer, including:
[0023] During cooling, oxygen, bulk nitrogen and small nitrogen without phosphorus are introduced, the flow range of oxygen is 900-1200sccm, the flow range of bulk nitrogen is 600-900sccm, the flow range of small nitrogen without phosphorus is 400-600sccm, and the cooling time range is 5-7min.
[0024] Optionally, the diffusion method includes a two-step diffusion process, and the first diffusion process includes:
[0025] When the silicon wafer is placed in the diffusion furnace, the temperature in the diffusion furnace is controlled at 780°C, oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of oxygen is 500sccm, the flow rate of phosphorus-carrying nitrogen is 800sccm, and the time is 3 minutes, so as to diffuse phosphorus into the silicon wafer;
[0026] The temperature in the diffusion furnace was raised to 830°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1400sccm, and the flow rate of small nitrogen without phosphorus was 500sccm. The time was 7 minutes to push phosphorus into the silicon wafer.
[0027] Based on the temperature at the end of the heating process, the temperature in the diffusion furnace is lowered to 800°C. During the temperature reduction process, oxygen, nitrogen and nitrogen without phosphorus are introduced. The flow rate of oxygen is 1000sccm, the flow rate of nitrogen is 800sccm, and the flow rate of nitrogen without phosphorus is 500sccm. The temperature reduction time is 8min, so as to perform variable temperature oxygen-containing advancement on the silicon wafer.
[0028] The second diffusion process includes:
[0029] The temperature in the diffusion furnace is controlled at 800°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow rate of oxygen is 500 sccm, and the flow rate of phosphorus-carrying nitrogen is 800 sccm. The time is 4 minutes, so as to diffuse phosphorus into the silicon wafer.
[0030] The temperature in the diffusion furnace was raised to 860°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1400sccm, and the flow rate of small nitrogen without phosphorus was 500sccm. The time was 8 minutes, so that phosphorus was pushed into the silicon wafer.
[0031] Based on the end temperature of the heating in the second step diffusion process, the temperature in the diffusion furnace is cooled to 830°C. Oxygen, large nitrogen and small nitrogen without phosphorus are introduced during the cooling. The flow rate of oxygen is 1000sccm, the flow rate of large nitrogen is 800sccm, and the flow rate of small nitrogen without phosphorus is 500sccm. The cooling time is 6 minutes to perform variable temperature oxygen advancement on the silicon wafer.
[0032] Optionally, the diffusion method includes a two-step diffusion process, and the first diffusion process includes:
[0033] When the silicon wafer is placed in the diffusion furnace, the temperature in the diffusion furnace is controlled at 775°C, oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of oxygen is 450sccm, the flow rate of phosphorus-carrying nitrogen is 700sccm, and the time is 2min, so as to diffuse phosphorus into the silicon wafer;
[0034] The temperature in the diffusion furnace was raised to 825°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1200sccm, and the flow rate of small nitrogen without phosphorus was 400sccm. The time was 6 minutes to push phosphorus into the silicon wafer.
[0035] Based on the temperature at the end of the heating process, the temperature in the diffusion furnace is lowered to 795°C. During the temperature reduction process, oxygen, nitrogen and nitrogen without phosphorus are introduced. The flow rate of oxygen is 900sccm, the flow rate of nitrogen is 600sccm, and the flow rate of nitrogen without phosphorus is 400sccm. The temperature reduction time is 7min, so as to perform variable temperature oxygen-containing advancement on the silicon wafer.
[0036] The second diffusion process includes:
[0037] The temperature in the diffusion furnace is controlled at 795°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow rate of oxygen is 450 sccm, and the flow rate of phosphorus-carrying nitrogen is 700 sccm. The time is 3 minutes, so as to diffuse phosphorus into the silicon wafer.
[0038] The temperature in the diffusion furnace was raised to 850°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1200sccm, and the flow rate of small nitrogen without phosphorus was 400sccm. The time was 7 minutes to push phosphorus into the silicon wafer.
[0039] Based on the end temperature of the heating in the second step diffusion process, the temperature in the diffusion furnace is cooled to 820°C. Oxygen, large nitrogen and small nitrogen without phosphorus are introduced during the cooling. The flow rate of oxygen is 900sccm, the flow rate of large nitrogen is 600sccm, and the flow rate of small nitrogen without phosphorus is 400sccm. The cooling time is 7 minutes to perform variable temperature oxygen advancement on the silicon wafer.
[0040] Optionally, the diffusion method includes a two-step diffusion process, and the first diffusion process includes:
[0041] When the silicon wafer is placed in the diffusion furnace, the temperature in the diffusion furnace is controlled at 790°C, oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of oxygen is 650sccm, the flow rate of phosphorus-carrying nitrogen is 850sccm, and the time is 4 minutes, so as to diffuse phosphorus into the silicon wafer;
[0042] The temperature in the diffusion furnace was raised to 840°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1500sccm, and the flow rate of small nitrogen without phosphorus was 600sccm. The time was 8 minutes to push phosphorus into the silicon wafer.
[0043] Based on the temperature at the end of the heating process, the temperature in the diffusion furnace is lowered to 810°C. During the temperature reduction process, oxygen, nitrogen and nitrogen without phosphorus are introduced. The flow rate of oxygen is 1200sccm, the flow rate of nitrogen is 900sccm, and the flow rate of nitrogen without phosphorus is 600sccm. The temperature reduction time is 9min, so as to perform variable temperature oxygen-containing advancement on the silicon wafer.
[0044] The second diffusion process includes:
[0045] The temperature in the diffusion furnace is controlled at 810°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow rate of oxygen is 650sccm, and the flow rate of phosphorus-carrying nitrogen is 850sccm. The time is 5 minutes, so as to diffuse phosphorus into the silicon wafer.
[0046] The temperature in the diffusion furnace was raised to 870°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1500sccm, and the flow rate of small nitrogen without phosphorus was 600sccm. The time was 9 minutes to push phosphorus into the silicon wafer.
[0047] Based on the end temperature of the heating in the second step diffusion process, the temperature in the diffusion furnace is cooled to 840°C. Oxygen, large nitrogen and small nitrogen without phosphorus are introduced during the cooling. The flow rate of oxygen is 1200sccm, the flow rate of large nitrogen is 900sccm, and the flow rate of small nitrogen without phosphorus is 600sccm. The cooling time is 7 minutes to perform variable temperature oxygen advancement on the silicon wafer.
[0048] A second aspect of the present disclosure provides a method for manufacturing a solar cell, comprising:
[0049] Use the above diffusion method to diffuse on the front side of the silicon wafer to form an emitter;
[0050] Remove the phosphosilicate glass formed during the diffusion process;
[0051] forming a front passivation film and a front anti-reflection film on the emitter in sequence;
[0052] Forming a back passivation film and a back anti-reflection film on the back of the silicon wafer in sequence from top to bottom;
[0053] Electrodes are formed on the front anti-reflection film and the back anti-reflection film, respectively.
[0054] As described above, the embodiments of the present disclosure provide a diffusion method and a method for manufacturing a solar cell. In the process of variable temperature oxygen-containing advancement, by cooling, the diffusion rate of phosphorus can be reduced, which is conducive to forming a shallow junction and improving the uniformity of diffusion. At the same time, by cooling, the lower temperature can allow impurities to be better segregated into the impurity absorption area, improve the impurity absorption effect on the silicon wafer, reduce the recombination center inside the silicon wafer, and improve the photoelectric conversion efficiency of the solar cell. Therefore, the embodiments of the present disclosure can obtain a shallower junction depth to meet the requirements of high square resistance while ensuring the uniformity of square resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 A flow chart showing a diffusion method according to an embodiment of the present disclosure.
[0056] Figure 2 A flow chart showing a method for manufacturing a solar cell according to an embodiment of the present disclosure. DETAILED DESCRIPTION
[0057] The following describes the embodiments of the present disclosure through specific examples, and those skilled in the art can easily understand other advantages and effects of the present disclosure from the information disclosed in the present disclosure. The present disclosure can also be implemented or applied through other different specific embodiments, and the details in the present disclosure can also be modified or changed in various ways according to different viewpoints and application systems without departing from the spirit of the present disclosure. It should be noted that the embodiments and features in the embodiments in the present disclosure can be combined with each other without conflict.
[0058] The following is a detailed description of the embodiments of the present disclosure with reference to the accompanying drawings so that those skilled in the art can easily implement the present disclosure. The present disclosure can be embodied in many different forms and is not limited to the embodiments described herein.
[0059] In the representations of the present disclosure, the reference terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" and the like mean that the specific features, structures, materials, or characteristics represented in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure. Moreover, the specific features, structures, materials, or characteristics represented may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples represented in the present disclosure and the features of different embodiments or examples, unless they are mutually contradictory.
[0060] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the representation of the present disclosure, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0061] Although not defined differently, all terms, including technical and scientific terms used herein, have the same meaning as those generally understood by those skilled in the art to which the present disclosure belongs. Terms defined in commonly used dictionaries are additionally interpreted as having meanings consistent with relevant technical literature and the message of the present disclosure, and shall not be overly interpreted as ideal or very formal meanings unless defined.
[0062] Figure 1 A flow chart showing a diffusion method provided by an embodiment of the present disclosure is shown as follows: Figure 1 As shown, the diffusion method includes:
[0063] Step 110: When the silicon wafer is placed in a diffusion furnace, a source is passed into the diffusion furnace to diffuse phosphorus into the silicon wafer;
[0064] Step 120: Raise the temperature in the diffusion furnace to push phosphorus into the silicon wafer;
[0065] Step 130: Cooling down the diffusion furnace based on the temperature at the end of the heating process, and introducing oxygen during the cooling process to perform temperature-variable oxygen-containing propulsion on the silicon wafer;
[0066] Step 140: After at least two steps of the source-pushing process, the temperature in the diffusion furnace is lowered, and then the diffusion furnace is opened to take out the silicon wafer.
[0067] In the disclosed embodiment, during the variable temperature oxygen-containing advancement process, by cooling, the phosphorus diffusion rate can be reduced, which is conducive to forming a shallow junction and improving the diffusion uniformity. At the same time, by cooling, the lower temperature can better condense impurities into the impurity-gettering area, improve the impurity-gettering effect on the silicon wafer, reduce the recombination center inside the silicon wafer, and improve the photoelectric conversion efficiency of the solar cell.
[0068] Therefore, the embodiments of the present disclosure can obtain a shallower junction depth to meet the requirement of high square resistance while ensuring the uniformity of square resistance.
[0069] Furthermore, through a multi-step diffusion process, phosphorus impurities can be continuously diffused into the interior of the silicon wafer, reducing the phosphorus concentration on the surface of the silicon wafer, avoiding the accumulation of phosphorus near the surface layer, and showing a greater sharpness on the phosphorus concentration distribution curve, that is, increasing the phosphorus concentration gradient distribution, which makes it easy to form a drift field for carrier transport, increase the carrier lifetime, and further improve the efficiency of the battery cell.
[0070] In the embodiment of the present disclosure, in the first diffusion process of at least two diffusion processes, a source is passed into a diffusion furnace to diffuse phosphorus into a silicon wafer, specifically comprising the following steps:
[0071] The temperature in the diffusion furnace is controlled at 775-790°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow rate of oxygen is 450-650sccm, and the flow rate of phosphorus-carrying nitrogen is 700-850sccm. The time range is 2-4min.
[0072] In this process, the source is used to deposit phosphorus. In this process, oxygen reacts with the silicon wafer to form silicon oxide, and then phosphorus diffuses through the silicon oxide, which can reduce the phosphorus diffusion rate, improve diffusion uniformity, reduce surface concentration, and reduce carrier surface recombination.
[0073] Wherein, small nitrogen refers to nitrogen carrying a phosphorus source (phosphorus oxychloride). Specifically, pure nitrogen is passed into a liquid phosphorus source in a phosphorus source bottle to carry the liquid phosphorus source, forming small nitrogen, which is further passed into a diffusion furnace. At this time, small nitrogen carrying phosphorus refers to nitrogen carrying a phosphorus source.
[0074] In the first step of the diffusion process, after the source is turned on, the temperature in the diffusion furnace is increased to allow the phosphorus after the source is turned on to further advance into the silicon wafer. In this process, the temperature in the diffusion furnace is increased, and large nitrogen and small nitrogen without phosphorus are introduced. The flow rate of large nitrogen is in the range of 1200-1500sccm, and the flow rate of small nitrogen without phosphorus is in the range of 400-600sccm. The heating time range is 6-8min.
[0075] In this embodiment, the temperature is increased to cause phosphorus atoms to diffuse from the surface of the silicon wafer to the inside of the silicon wafer, so that the phosphorus concentration on the surface of the silicon wafer is reduced.
[0076] Among them, large nitrogen refers to pure nitrogen, and small nitrogen without phosphorus refers to pure nitrogen that does not flow through the phosphorus source bottle, that is, does not carry the phosphorus source, and enters the diffusion furnace through the corresponding pipeline. In this case, small nitrogen without phosphorus is purer than small nitrogen with phosphorus, and its function is to remove the phosphorus source remaining in the flow channel of the small nitrogen with phosphorus mentioned above and bring it into the diffusion furnace.
[0077] In the embodiment of the present disclosure, in the first diffusion process, the temperature in the diffusion furnace is lowered based on the temperature at the end of the heating process, and the temperature reduction range is 20-30°C;
[0078] When the temperature is lowered, oxygen is introduced to perform variable temperature oxygen-containing advancement of the silicon wafer, including:
[0079] During cooling, oxygen, bulk nitrogen and small nitrogen without phosphorus are introduced, the flow range of oxygen is 900-1200sccm, the flow range of bulk nitrogen is 600-900sccm, the flow range of small nitrogen without phosphorus is 400-600sccm, and the cooling time range is 7-9min.
[0080] In this embodiment, by controlling the temperature reduction range, the junction depth can be effectively reduced without affecting the diffusion of phosphorus, thereby obtaining a high square resistance.
[0081] In an embodiment of the present disclosure, in the second diffusion process of a two-step diffusion process, a secondary source is passed into the diffusion furnace to further diffuse phosphorus into the silicon wafer. At this time, the temperature in the diffusion furnace is controlled at 795-810°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow range of oxygen is 450-650sccm, and the flow range of phosphorus-carrying nitrogen is 700-850sccm, and the time range is 3-5min.
[0082] Compared with the first source passing, the source passing temperature in this step is higher, so that phosphorus can be continuously diffused into the silicon wafer at high temperature.
[0083] In the embodiment of the present disclosure, in the second diffusion process, the temperature in the diffusion furnace is increased, including:
[0084] The temperature in the diffusion furnace is raised in the range of 850-870°C, and large nitrogen and small nitrogen without phosphorus are introduced. The flow rate of large nitrogen is in the range of 1200-1500sccm, and the flow rate of small nitrogen without phosphorus is in the range of 400-600sccm. The heating time range is 7-9min.
[0085] This can promote the further diffusion of phosphorus impurities into the silicon wafer.
[0086] In the embodiment of the present disclosure, in the second step diffusion process, the temperature in the diffusion furnace is lowered based on the temperature at the end of the heating, and the temperature reduction range is 20-30°C;
[0087] When the temperature is lowered, oxygen is introduced to perform variable temperature oxygen-containing advancement of the silicon wafer, including:
[0088] During cooling, oxygen, bulk nitrogen and small nitrogen without phosphorus are introduced, the flow range of oxygen is 900-1200sccm, the flow range of bulk nitrogen is 600-900sccm, the flow range of small nitrogen without phosphorus is 400-600sccm, and the cooling time range is 5-7min.
[0089] In this embodiment, the phosphorus diffusion depth is controlled by lowering the temperature, which is beneficial to forming a shallow junction high square resistance solar cell.
[0090] The present disclosure also provides a specific embodiment 1 including a two-step diffusion process:
[0091] The first step of the diffusion process includes:
[0092] When the silicon wafer is placed in the diffusion furnace, the temperature in the diffusion furnace is controlled at 780°C, oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of oxygen is 500sccm, the flow rate of phosphorus-carrying nitrogen is 800sccm, and the time is 3 minutes, so as to diffuse phosphorus into the silicon wafer;
[0093] The temperature in the diffusion furnace was raised to 830°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1400sccm, and the flow rate of small nitrogen without phosphorus was 500sccm. The time was 7 minutes to push phosphorus into the silicon wafer.
[0094] Based on the temperature at the end of the heating process, the temperature in the diffusion furnace is lowered to 800°C. During the temperature reduction process, oxygen, nitrogen and nitrogen without phosphorus are introduced. The flow rate of oxygen is 1000sccm, the flow rate of nitrogen is 800sccm, and the flow rate of nitrogen without phosphorus is 500sccm. The temperature reduction time is 8min, so as to perform variable temperature oxygen-containing advancement on the silicon wafer.
[0095] The second diffusion process includes:
[0096] The temperature in the diffusion furnace is controlled at 800°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow rate of oxygen is 500 sccm, and the flow rate of phosphorus-carrying nitrogen is 800 sccm. The time is 4 minutes, so as to diffuse phosphorus into the silicon wafer.
[0097] The temperature in the diffusion furnace was raised to 860°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1400sccm, and the flow rate of small nitrogen without phosphorus was 500sccm. The time was 8 minutes, so that phosphorus was pushed into the silicon wafer.
[0098] Based on the end temperature of the heating in the second step diffusion process, the temperature in the diffusion furnace is cooled to 830°C. Oxygen, large nitrogen and small nitrogen without phosphorus are introduced during the cooling. The flow rate of oxygen is 1000sccm, the flow rate of large nitrogen is 800sccm, and the flow rate of small nitrogen without phosphorus is 500sccm. The cooling time is 6 minutes to perform variable temperature oxygen advancement on the silicon wafer.
[0099] The present disclosure also provides a specific embodiment 2 including a two-step diffusion process:
[0100] When the silicon wafer is placed in the diffusion furnace, the temperature in the diffusion furnace is controlled at 775°C, oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of oxygen is 450sccm, the flow rate of phosphorus-carrying nitrogen is 700sccm, and the time is 2min, so as to diffuse phosphorus into the silicon wafer;
[0101] The temperature in the diffusion furnace was raised to 825°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1200sccm, and the flow rate of small nitrogen without phosphorus was 400sccm. The time was 6 minutes to push phosphorus into the silicon wafer.
[0102] Based on the temperature at the end of the heating process, the temperature in the diffusion furnace is lowered to 795°C. During the temperature reduction process, oxygen, nitrogen and nitrogen without phosphorus are introduced. The flow rate of oxygen is 900sccm, the flow rate of nitrogen is 600sccm, and the flow rate of nitrogen without phosphorus is 400sccm. The temperature reduction time is 7min, so as to perform variable temperature oxygen-containing advancement on the silicon wafer.
[0103] The second diffusion process includes:
[0104] The temperature in the diffusion furnace is controlled at 795°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow rate of oxygen is 450 sccm, and the flow rate of phosphorus-carrying nitrogen is 700 sccm. The time is 3 minutes, so as to diffuse phosphorus into the silicon wafer.
[0105] The temperature in the diffusion furnace was raised to 850°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1200sccm, and the flow rate of small nitrogen without phosphorus was 400sccm. The time was 7 minutes to push phosphorus into the silicon wafer.
[0106] Based on the end temperature of the heating in the second step diffusion process, the temperature in the diffusion furnace is cooled to 820°C. Oxygen, large nitrogen and small nitrogen without phosphorus are introduced during the cooling. The flow rate of oxygen is 900sccm, the flow rate of large nitrogen is 600sccm, and the flow rate of small nitrogen without phosphorus is 400sccm. The cooling time is 7 minutes to perform variable temperature oxygen advancement on the silicon wafer.
[0107] The present disclosure also provides a specific embodiment 3 including a two-step diffusion process:
[0108] The first step of the diffusion process includes:
[0109] When the silicon wafer is placed in the diffusion furnace, the temperature in the diffusion furnace is controlled at 790°C, oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of oxygen is 650sccm, the flow rate of phosphorus-carrying nitrogen is 850sccm, and the time is 4 minutes, so as to diffuse phosphorus into the silicon wafer;
[0110] The temperature in the diffusion furnace was raised to 840°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1500sccm, and the flow rate of small nitrogen without phosphorus was 600sccm. The time was 8 minutes to push phosphorus into the silicon wafer.
[0111] Based on the temperature at the end of the heating process, the temperature in the diffusion furnace is lowered to 810°C. During the temperature reduction process, oxygen, nitrogen and nitrogen without phosphorus are introduced. The flow rate of oxygen is 1200sccm, the flow rate of nitrogen is 900sccm, and the flow rate of nitrogen without phosphorus is 600sccm. The temperature reduction time is 9min, so as to perform variable temperature oxygen-containing advancement on the silicon wafer.
[0112] The second diffusion process includes:
[0113] The temperature in the diffusion furnace is controlled at 810°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace. The flow rate of oxygen is 650sccm, and the flow rate of phosphorus-carrying nitrogen is 850sccm. The time is 5 minutes, so as to diffuse phosphorus into the silicon wafer.
[0114] The temperature in the diffusion furnace was raised to 870°C, and large nitrogen and small nitrogen without phosphorus were introduced. The flow rate of large nitrogen was 1500sccm, and the flow rate of small nitrogen without phosphorus was 600sccm. The time was 9 minutes to push phosphorus into the silicon wafer.
[0115] Based on the end temperature of the heating in the second step diffusion process, the temperature in the diffusion furnace is cooled to 840°C. Oxygen, large nitrogen and small nitrogen without phosphorus are introduced during the cooling. The flow rate of oxygen is 1200sccm, the flow rate of large nitrogen is 900sccm, and the flow rate of small nitrogen without phosphorus is 600sccm. The cooling time is 7 minutes to perform variable temperature oxygen advancement on the silicon wafer.
[0116] The diffusion method of any of the above embodiments of the present disclosure is applied to a solar cell manufacturing method, specifically, Figure 2 As shown, the solar cell manufacturing method may include:
[0117] Step 210: Use the above diffusion method to diffuse on the front side of the silicon wafer to form an emitter.
[0118] In an optional embodiment, a textured surface is formed on the front side of the silicon wafer before executing step 210, and the silicon wafer is P-type silicon. Specifically, a wet or dry etching technology is selected to form a textured surface on the front side of the silicon wafer through a texture making device.
[0119] Step 220: Remove the phospho-silicate glass (PSG) formed during the diffusion process.
[0120] Specifically, an alkaline solution is used to remove the PSG and surrounding PN junctions.
[0121] Before executing step 220 , laser scanning is performed on the emitter to form a heavily doped region.
[0122] Step 230: sequentially forming a front passivation film and a front anti-reflection film on the emitter.
[0123] Step 240: forming a back passivation film and a back anti-reflection film on the back side of the silicon wafer in sequence from top to bottom.
[0124] Before forming the back passivation film, a back oxide layer is formed first, so that the back passivation film covers the back oxide layer.
[0125] Step 250: forming electrodes on the front anti-reflection film and the back anti-reflection film respectively.
[0126] Specifically, the electrodes are formed using screen printing and electrical injection processes.
[0127] Based on the improved diffusion process of the disclosed embodiment, the solar cell of the embodiment has good power conversion efficiency.
[0128] The above embodiments are merely illustrative of the principles and effects of the present disclosure, and are not intended to limit the present disclosure. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present disclosure. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present disclosure shall still be covered by the claims of the present disclosure.
Claims
1. A diffusion method, characterized in that: The method comprises at least two diffusion processes, each of which comprises the following steps: When the silicon wafer is placed in a diffusion furnace, a source is supplied to the diffusion furnace to diffuse phosphorus into the silicon wafer; Raising the temperature in the diffusion furnace to push the phosphorus into the silicon wafer; Cooling the diffusion furnace based on the temperature at the end of the heating process, and introducing oxygen during the cooling process to perform temperature-variable oxygen-containing propulsion on the silicon wafer; After the at least two-step diffusion process, the temperature in the diffusion furnace is lowered, and then the diffusion furnace is opened to take out the silicon wafer; In the first diffusion process of the at least two diffusion processes, the step of heating the diffusion furnace comprises: The temperature in the diffusion furnace is raised to 825-840° C., and large nitrogen and small nitrogen without phosphorus are introduced. The flow rate of the large nitrogen is in the range of 1200-1500 sccm, the flow rate of the small nitrogen without phosphorus is in the range of 400-600 sccm, and the heating time range is 6-8 min. In the first diffusion process of the at least two-step diffusion process, a source is supplied to a diffusion furnace to diffuse phosphorus into the silicon wafer, including: The temperature in the diffusion furnace is controlled at 775-790°C, and oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of the oxygen is in the range of 450-650sccm, the flow rate of the phosphorus-carrying nitrogen is in the range of 700-850sccm, and the time range is 2-4min; In the first diffusion process of the at least two-step diffusion process, the temperature in the diffusion furnace is lowered based on the temperature at the end of the heating process, and the temperature reduction range is 20-30° C.; When the temperature is lowered, oxygen is introduced to perform temperature-variable oxygen-containing propulsion on the silicon wafer, comprising: When cooling, oxygen, large nitrogen and small nitrogen without phosphorus are introduced, the flow range of oxygen is 900-1200sccm, the flow range of large nitrogen is 600-900sccm, the flow range of small nitrogen without phosphorus is 400-600sccm, and the cooling time range is 7-9min; The at least two-step diffusion process is configured as a two-step diffusion process, wherein in the second step of the diffusion process, the source is passed into the diffusion furnace to diffuse phosphorus into the silicon wafer, comprising: The temperature in the diffusion furnace is controlled at 795-810° C., oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of the oxygen is in the range of 450-650 sccm, the flow rate of the phosphorus-carrying nitrogen is in the range of 700-850 sccm, and the time range is 3-5 min; In the second diffusion process, the temperature in the diffusion furnace is increased, including: The temperature in the diffusion furnace is raised to 850-870°C, and large nitrogen and small nitrogen without phosphorus are introduced. The flow rate of the large nitrogen is 1200-1500sccm, the flow rate of the small nitrogen without phosphorus is 400-600sccm, and the heating time range is 7-9min.
2. The diffusion method according to claim 1, characterized in that: In the second diffusion process, the temperature in the diffusion furnace is lowered based on the temperature at the end of the heating process, and the temperature reduction range is 20-30° C.; When the temperature is lowered, oxygen is introduced to perform temperature-variable oxygen-containing propulsion on the silicon wafer, comprising: During cooling, oxygen, bulk nitrogen and non-phosphorus-carrying small nitrogen are introduced, the flow range of oxygen is 900-1200sccm, the flow range of bulk nitrogen is 600-900sccm, the flow range of non-phosphorus-carrying small nitrogen is 400-600sccm, and the cooling time range is 5-7min.
3. The diffusion method according to claim 1, characterized in that: The diffusion method includes a two-step diffusion process, and the first step of the diffusion process includes: When a silicon wafer is placed in a diffusion furnace, the temperature in the diffusion furnace is controlled at 780° C., oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of the oxygen is 500 sccm, the flow rate of the phosphorus-carrying nitrogen is 800 sccm, and the time is 3 minutes, so as to diffuse phosphorus into the silicon wafer; The temperature in the diffusion furnace is raised to 830° C., and large nitrogen and small nitrogen without phosphorus are introduced, the flow rate of the large nitrogen is 1400 sccm, and the flow rate of the small nitrogen without phosphorus is 500 sccm, and the time is 7 minutes, so that the phosphorus is pushed into the inside of the silicon wafer; Based on the temperature at the end of the heating, the temperature in the diffusion furnace is lowered to 800° C., and oxygen, large nitrogen and small nitrogen without phosphorus are introduced during the temperature reduction, the flow rate of the oxygen is 1000 sccm, the flow rate of the large nitrogen is 800 sccm, the flow rate of the small nitrogen without phosphorus is 500 sccm, and the temperature reduction time is 8 minutes, so as to perform temperature-variable oxygen-containing advancement on the silicon wafer; The second diffusion process includes: The temperature in the diffusion furnace is controlled at 800° C., oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of the oxygen is 500 sccm, the flow rate of the phosphorus-carrying nitrogen is 800 sccm, and the time is 4 minutes, so as to diffuse phosphorus into the silicon wafer; The temperature in the diffusion furnace is raised to 860° C., and large nitrogen and small nitrogen without phosphorus are introduced, the flow rate of the large nitrogen is 1400 sccm, and the flow rate of the small nitrogen without phosphorus is 500 sccm, and the time is 8 minutes, so that the phosphorus is pushed into the inside of the silicon wafer; Based on the terminal temperature of the heating in the second-step diffusion process, the temperature inside the diffusion furnace is cooled to 830°C. During the cooling process, oxygen, large nitrogen and small nitrogen without phosphorus are introduced. The flow rate of oxygen is 1000sccm, the flow rate of large nitrogen is 800sccm, and the flow rate of small nitrogen without phosphorus is 500sccm. The cooling time is 6 minutes to perform variable temperature oxygen-containing advancement on the silicon wafer.
4. The diffusion method according to claim 1, characterized in that: The diffusion method includes a two-step diffusion process, and the first step of the diffusion process includes: When a silicon wafer is placed in a diffusion furnace, the temperature in the diffusion furnace is controlled at 775° C., oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of the oxygen is 450 sccm, the flow rate of the phosphorus-carrying nitrogen is 700 sccm, and the time is 2 minutes, so as to diffuse phosphorus into the silicon wafer; The temperature in the diffusion furnace is raised to 825° C., and large nitrogen and small nitrogen without phosphorus are introduced, the flow rate of the large nitrogen is 1200 sccm, and the flow rate of the small nitrogen without phosphorus is 400 sccm, and the time is 6 minutes, so that the phosphorus is pushed into the inside of the silicon wafer; Based on the temperature at the end of the heating, the temperature in the diffusion furnace is lowered to 795° C., and oxygen, large nitrogen and small nitrogen without phosphorus are introduced during the temperature reduction. The flow rate of the oxygen is 900 sccm, the flow rate of the large nitrogen is 600 sccm, the flow rate of the small nitrogen without phosphorus is 400 sccm, and the temperature reduction time is 7 minutes, so as to perform temperature-variable oxygen-containing advancement on the silicon wafer; The second diffusion process includes: The temperature in the diffusion furnace is controlled at 795° C., oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of the oxygen is 450 sccm, the flow rate of the phosphorus-carrying nitrogen is 700 sccm, and the time is 3 minutes, so as to diffuse phosphorus into the silicon wafer; The temperature in the diffusion furnace is raised to 850° C., and large nitrogen and small nitrogen without phosphorus are introduced, the flow rate of the large nitrogen is 1200 sccm, and the flow rate of the small nitrogen without phosphorus is 400 sccm, and the time is 7 minutes, so that the phosphorus is pushed into the inside of the silicon wafer; Based on the terminal temperature of the heating in the second-step diffusion process, the temperature in the diffusion furnace is cooled to 820°C. During the cooling, oxygen, large nitrogen and small nitrogen without phosphorus are introduced. The flow rate of oxygen is 900sccm, the flow rate of large nitrogen is 600sccm, and the flow rate of small nitrogen without phosphorus is 400sccm. The cooling time is 7 minutes to perform variable temperature oxygen-containing advancement on the silicon wafer.
5. The diffusion method according to claim 1, characterized in that: The diffusion method includes a two-step diffusion process, and the first step of the diffusion process includes: When a silicon wafer is placed in a diffusion furnace, the temperature in the diffusion furnace is controlled at 790° C., oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of the oxygen is 650 sccm, the flow rate of the phosphorus-carrying nitrogen is 850 sccm, and the time is 4 minutes, so as to diffuse phosphorus into the silicon wafer; The temperature in the diffusion furnace is raised to 840° C., and large nitrogen and small nitrogen without phosphorus are introduced, the flow rate of the large nitrogen is 1500 sccm, and the flow rate of the small nitrogen without phosphorus is 600 sccm, and the time is 8 minutes, so that the phosphorus is pushed into the inside of the silicon wafer; Based on the temperature at the end of the heating, the temperature in the diffusion furnace is lowered to 810° C., and oxygen, large nitrogen and small nitrogen without phosphorus are introduced during the cooling, the flow rate of oxygen is 1200 sccm, the flow rate of large nitrogen is 900 sccm, the flow rate of small nitrogen without phosphorus is 600 sccm, and the cooling time is 9 minutes, so as to perform variable temperature oxygen-containing advancement on the silicon wafer; The second diffusion process includes: The temperature in the diffusion furnace is controlled at 810° C., oxygen and phosphorus-carrying nitrogen are introduced into the diffusion furnace, the flow rate of the oxygen is 650 sccm, the flow rate of the phosphorus-carrying nitrogen is 850 sccm, and the time is 5 minutes, so as to diffuse phosphorus into the silicon wafer; The temperature in the diffusion furnace is raised to 870° C., and large nitrogen and small nitrogen without phosphorus are introduced, the flow rate of the large nitrogen is 1500 sccm, and the flow rate of the small nitrogen without phosphorus is 600 sccm, and the time is 9 minutes, so that the phosphorus is pushed into the inside of the silicon wafer; Based on the terminal temperature of the heating in the second-step diffusion process, the temperature in the diffusion furnace is cooled to 840°C. During the cooling, oxygen, large nitrogen and small nitrogen without phosphorus are introduced. The flow rate of oxygen is 1200sccm, the flow rate of large nitrogen is 900sccm, and the flow rate of small nitrogen without phosphorus is 600sccm. The cooling time is 7 minutes to perform variable temperature oxygen-containing advancement on the silicon wafer.
6. A method for manufacturing a solar cell, characterized in that: include: Using the diffusion method described in any one of claims 1 to 5 to diffuse on the front side of the silicon wafer to form an emitter; Remove the phosphosilicate glass formed during the diffusion process; forming a front passivation film and a front anti-reflection film on the emitter in sequence; Forming a back passivation film and a back anti-reflection film on the back of the silicon wafer in sequence from top to bottom; Electrodes are formed on the front anti-reflection film and the back anti-reflection film, respectively.