A method for preparing low-cost biomedical titanium alloy spherical powder

Through steps such as low-energy ball milling, vacuum sintering, hydrogenation and radio frequency plasma spheroidization, the problems of microstructure inhomogeneity and low production efficiency of titanium-zirconium-niobium alloy and titanium-zirconium-niobium-tantalum alloy powder are solved, achieving low-cost, spherical The preparation of powders with high and low impurity content significantly improves the composition uniformity and fluidity of the material.

CN116174726BActive Publication Date: 2024-10-22JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211102556.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-10-22
Estimated Expiration
2042-09-09

AI Technical Summary

Technical Problem

It is difficult to effectively prepare titanium-zirconium-niobium alloy and titanium-zirconium-niobium-tantalum alloy powder with low cost, high sphericity and low impurity content using existing technology. Traditional powder metallurgy processes have problems with microstructure inhomogeneity and low production efficiency. Additive manufacturing methods The raw material performance requirements are high and the process is complex. The traditional non-spherical powder preparation process is difficult to meet the sphericity and fluidity requirements.

Method used

The low-energy ball milling method is used to mechanically combine the elemental powders of titanium, zirconium, niobium or tantalum, followed by high-temperature vacuum sintering and hydrogenation, and finally through radio frequency plasma spheroidization and dehydrogenation treatment to achieve pre-alloying, refinement and spherification of the powder. change.

Benefits of technology

Through this method, titanium-zirconium-niobium alloy or titanium-zirconium-niobium-tantalum alloy powder with small particle size, uniform composition, good dispersion, high fluidity and low oxygen content is obtained, which significantly improves the composition uniformity and production efficiency of the material and reduces the cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116174726B_ABST
    Figure CN116174726B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing low-cost biomedical titanium alloy spherical powder, which comprises the following steps: S1: low-energy ball milling: taking titanium, zirconium, niobium or titanium, zirconium, niobium, tantalum single powder or hydride powder, ball milling according to the designed component ratio to obtain composite powder; S2: hydrogenation: high-temperature vacuum sintering of the composite powder to achieve pre-alloying, and then hydrogenation to obtain hydrogen-containing alloy powder; S3: radio frequency plasma spheroidization and dehydrogenation treatment of the hydrogen-containing alloy powder. The method can realize the short process preparation of titanium zirconium niobium alloy powder or titanium zirconium niobium tantalum alloy powder with low cost, good sphericity and low impurity content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing low-cost biomedical titanium alloy spherical powder, belonging to the technical field of preparation of medical titanium alloy spherical powder. Background Art

[0002] Titanium-zirconium-niobium alloy and titanium-zirconium-niobium-tantalum alloy have low elastic modulus, good corrosion resistance, non-toxicity and good biocompatibility, and have been proven to be excellent biomedical titanium alloys. Although the traditional powder metallurgy process is low-cost, the diffusion rate of niobium and tantalum in the titanium matrix is ​​very low. Therefore, the microstructures of titanium-zirconium-niobium alloy and titanium-zirconium-niobium-tantalum alloy prepared by this process generally have low porosity and poor uniformity of organizational composition. In addition, it is necessary to heal the pores and adjust the organizational uniformity through roll forging, rolling, heat treatment and other means to meet the requirements of the final product for material performance, but it causes a deterioration in production efficiency and cost.

[0003] Additive manufacturing has the characteristics of short cycle, integrated forming and tissue regulation, and support for personalized customization. It has been used to manufacture parts with complex configurations such as artificial implant joints. However, this method has very high requirements on the chemical composition, sphericity, fluidity and other properties of the raw material spherical powder. In addition, titanium alloy powder is different from conventional metal powders such as nickel-based high-temperature alloys. Its strong room temperature oxygen absorption characteristics and high-temperature reaction activity make the titanium alloy powder preparation process different from conventional metal powders. On the other hand, the preparation process of traditional non-spherical titanium powder (such as hydrogenation dehydrogenation process (HDH)) is difficult to meet the requirements of metal additive manufacturing for sphericity and fluidity.

[0004] Both the plasma rotating electrode method (PREP) and the argon atomization method (GA) require the molten alloy liquid to be obtained first. The high-temperature activity of high-melting-point metals such as niobium and tantalum and titanium and zirconium metals makes their melting process complicated and difficult to control. Moreover, the plasma rotating electrode method is difficult to achieve effective control of the atmosphere, and the particle size of the powder that can be prepared is limited, and the production cost is high; although the powder prepared by the argon atomization method can reduce the impact of the preparation process on the impurity content of the powder, there are problems such as hollow powder; the plasma spheroidization method can prepare spherical powder with dense interior, but the powder oxygen content is high; this is the deficiency of the existing technology. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing low-cost biomedical titanium alloy spherical powder in view of the shortcomings of the prior art. The method can realize a short process for preparing titanium-zirconium-niobium alloy powder or titanium-zirconium-niobium-tantalum alloy powder with low cost, good sphericity and low impurity content.

[0006] This scheme is achieved through the following technical measures: A method for preparing low-cost biomedical titanium alloy spherical powder, which includes the following steps:

[0007] S1: Low-energy ball milling: Take titanium, zirconium, niobium or titanium, zirconium, niobium, tantalum single powder or hydride powder, and ball mill according to the designed component ratio to obtain composite powder;

[0008] S2: hydrogenation: the composite powder is subjected to high temperature vacuum sintering to achieve pre-alloying, and then hydrogenated to obtain hydrogen-containing alloy powder;

[0009] S3: The hydrogen-containing alloy powder is subjected to radio frequency plasma spheroidization and dehydrogenation treatment.

[0010] Preferably, the process of low-energy ball milling in step S1 is: take titanium, zirconium, niobium or titanium, zirconium, niobium, tantalum element powder or hydride powder with an average particle size less than 100 μm, and perform low-speed ball milling at a speed of 100-250 rpm / min for 1-2 hours under inert gas protection or in a vacuum environment according to the designed component ratio to obtain a composite powder.

[0011] Preferably, the hydrogenation process in step S2 is as follows: placing the composite powder obtained in step S1 in a vacuum sintering furnace, and evacuating the vacuum sintering furnace to a vacuum of 1.0×10 -3 Pa and then heated to 1200℃ and kept warm for 2-3h. After the vacuum sintering furnace is cooled to 650℃, high-purity hydrogen is introduced into the vacuum sintering furnace to keep the hydrogen partial pressure in the furnace at 0.5MPa and keep warm for 1-2h and then cool to obtain hydrogen-containing pre-alloyed powder. After screening, hydrogen-containing alloy powder with an average particle size of less than 100μm is obtained.

[0012] Preferably, in step S3, the hydrogen-containing alloy powder rapidly absorbs heat to hydrogen explode and cools to generate fine spherical alloy powder during the radio frequency plasma spheroidization process, and then undergoes dehydrogenation treatment to obtain spherical titanium-zirconium-niobium alloy powder or titanium-zirconium-niobium-tantalum alloy powder with an average particle size of 50 μm.

[0013] Preferably, during the radio frequency plasma spheroidization process in step S3, the powder feeding rate of the hydrogen-containing alloy powder is 50-100 g / min, and the plasma output power is 40 kW.

[0014] Preferably, the dehydrogenation treatment process of step S3 is: placing the spheroidized powder in a vacuum sintering furnace, and when the vacuum degree reaches below 1.0×10-3Pa, heating to 750°C at 5-15°C / min, keeping the temperature for 60-120min, and then cooling the furnace.

[0015] Beneficial effects of the present invention: The present invention realizes mechanical bonding between different types of powders and improves the overall uniformity of the composition of the composite powder through a ball milling process, and realizes pre-alloying and hydrogenation of the composite powder using a vacuum sintering-hydrogenation process. The dehydrogenation behavior of the hydrogen-containing alloy powder can effectively suppress the pollution of the powder and the oxidation of the powder in the ball milling process, while the high vacuum environment, instantaneous high temperature-cooling and hydrogen explosion phenomenon of the hydrogen-containing alloy powder in the radio frequency plasma spheroidization process are conducive to further improving the degree of uniformity of the composition and the degree of particle size refinement of the alloy powder, and finally obtains titanium-zirconium-niobium alloy powder or titanium-zirconium-niobium-tantalum alloy powder with fine particle size, uniform composition, good dispersibility and fluidity, high spheroidization rate and low oxygen content. It can be seen that compared with the prior art, the present invention has outstanding substantive characteristics and significant progress, and the beneficial effects of its implementation are also obvious. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The process flow chart of a specific embodiment of the present invention. DETAILED DESCRIPTION

[0017] In order to clearly illustrate the technical features of this solution, this solution is described below through specific implementation methods and in conjunction with the accompanying drawings.

[0018] A method for preparing low-cost biomedical titanium alloy spherical powder comprises the following steps:

[0019] S1: Low-energy ball milling: Take titanium, zirconium, niobium or titanium, zirconium, niobium, tantalum powder or hydride powder, and ball mill according to the designed composition ratio to obtain composite powder; Specifically, the process of low-energy ball milling is: take titanium, zirconium, niobium or titanium, zirconium, niobium, tantalum powder or hydride powder with an average particle size of less than 100 μm, and perform low-speed ball milling at a speed of 100-250 rpm / min for 1-2 hours under the protection of inert gas (such as argon) or in a vacuum environment according to the designed composition ratio to obtain composite powder;

[0020] S2: hydrogenation: the composite powder is subjected to high temperature vacuum sintering to achieve pre-alloying, and then hydrogenated to obtain hydrogen-containing alloy powder; specifically, the hydrogenation process is: the composite powder obtained in step S1 is placed in a vacuum sintering furnace, and the vacuum sintering furnace is evacuated to 1.0×10 -3 Pa, and then heated to 1200°C and kept warm for 2-3h. After the vacuum sintering furnace is cooled to 650°C, high-purity hydrogen is introduced into the vacuum sintering furnace to keep the hydrogen partial pressure in the furnace at 0.5MPa and keep warm for 1-2h before cooling to obtain hydrogen-containing pre-alloyed powder. After sieving, hydrogen-containing alloy powder with an average particle size of less than 100μm is obtained.

[0021] S3: The hydrogen-containing alloy powder is subjected to radio frequency plasma spheroidization and dehydrogenation treatment. During the radio frequency plasma spheroidization process, the hydrogen-containing alloy powder quickly absorbs heat, hydrogen explodes and cools to form fine spherical alloy powder. After dehydrogenation treatment, spherical titanium-zirconium-niobium alloy powder or titanium-zirconium-niobium-tantalum alloy powder with an average particle size of 50μm is obtained. During the radio frequency plasma spheroidization process, the powder feeding rate of the hydrogen-containing alloy powder is 50-100g / min, and the plasma output power is 40kw. The dehydrogenation treatment process is: the spheroidized powder is placed in a vacuum sintering furnace. When the vacuum degree reaches below 1.0×10-3Pa, the temperature is raised to 750℃ at a rate of 5-15℃ / min, and the temperature is kept for 60-120min, and then the furnace is cooled.

[0022] Example 1 (Preparation of titanium-zirconium-niobium alloy powder)

[0023] A method for preparing low-cost biomedical titanium alloy spherical powder comprises the following steps:

[0024] S1: According to the atomic ratio of 55.5Ti-26Zr-18.5Nb, the corresponding mass of TiH2, ZrH2, and Nb powders were ball-milled at 200 rpm / min for 90 min under inert gas protection to obtain a composite powder;

[0025] S2: The milled composite powder is sent into a vacuum sintering furnace. When the vacuum degree in the vacuum sintering furnace reaches 1.0×10 -3 Pa, start to heat up to 1200℃ at a rate of 10℃ / min and keep it warm for 120min; then cool the furnace to 650℃ and start to introduce hydrogen into the vacuum sintering furnace to keep the hydrogen partial pressure in the furnace at 0.5Mpa and keep it warm for 1h before cooling to obtain hydrogen-containing pre-alloyed powder, and obtain hydrogen-containing alloy powder with an average particle size of less than 100μm through screening.

[0026] S3: The hydrogen-containing alloy powder with an average particle size of less than 100μm is subjected to radio frequency plasma spheroidization. In this process, the hydrogen-containing alloy powder quickly absorbs heat, hydrogen explodes and cools to form fine spherical alloy powder. The plasma output power is 40kw; the spheroidized powder is placed in a vacuum sintering furnace. When the vacuum degree reaches below 1.0×10-3Pa, the temperature is increased to 750℃ at 5℃ / min and kept at this temperature for 90min. The furnace is then cooled to finally obtain spherical 55.5Ti-26Zr-18.5Nb alloy powder.

[0027] Example 2 (Preparation of Titanium-Zirconium-NbO2-Tantalum Alloy Powder)

[0028] A method for preparing low-cost biomedical titanium alloy spherical powder comprises the following steps:

[0029] S1: According to the atomic ratio of Ti-35Nb-7Zr-5Ta, the corresponding mass of TiH2, Nb, ZrH2, and Ta powders were ball-milled at 200 rpm / min for 120 min under inert gas protection to obtain a composite powder;

[0030] S2: The milled composite powder is sent into a vacuum sintering furnace. When the vacuum degree in the vacuum sintering furnace reaches 1.0×10 -3 Pa, start to heat up to 1200℃ at a rate of 10℃ / min and keep it warm for 180min; then cool the furnace to 650℃ and start to introduce hydrogen into the vacuum sintering furnace to keep the hydrogen partial pressure in the furnace at 0.5Mpa and keep it warm for 2h before cooling to obtain hydrogen-containing pre-alloyed powder, and obtain hydrogen-containing alloy powder with an average particle size of less than 100μm through screening.

[0031] S3: The hydrogen-containing alloy powder with an average particle size of less than 100μm is subjected to radio frequency plasma spheroidization. In this process, the hydrogen-containing alloy powder quickly absorbs heat, hydrogen explodes and cools to form fine spherical alloy powder. The plasma output power is 40kw; the spheroidized powder is placed in a vacuum sintering furnace. When the vacuum degree reaches below 1.0×10-3Pa, the temperature is increased to 750℃ at a rate of 15℃ / min and kept at this temperature for 120min. The furnace is then cooled to finally obtain spherical Ti-35Nb-7Zr-5Ta alloy powder.

[0032] Comparative Example 1 (Preparation of Titanium-Zirconium-Niobium Alloy Powder)

[0033] A method for preparing low-cost biomedical titanium alloy spherical powder comprises the following steps:

[0034] S1: According to the atomic ratio of 55.5Ti-26Zr-18.5Nb, the corresponding mass of TiH2, ZrH2, and Nb powders were ball-milled at 350 rpm / min for 90 min under inert gas protection to obtain a composite powder;

[0035] S2: The milled composite powder is sent into a vacuum sintering furnace. When the vacuum degree in the vacuum sintering furnace reaches 1.0×10 -3 After Pa, the temperature was raised to 1200°C at a rate of 10°C / min and kept at that temperature for 120min; then the furnace was cooled; and hydrogen-containing alloy powder with an average particle size of less than 100 μm was obtained by screening.

[0036] S3: The alloy powder with an average particle size of less than 100 μm is subjected to radio frequency plasma spheroidization, and the plasma output power is 40 kW; finally, spherical 55.5Ti-26Zr-18.5Nb alloy powder is obtained.

[0037] Comparative Example 2 (Preparation of Titanium-Zirconium-NbO2-Tantalum Alloy Pow

[0038] A method for preparing low-cost biomedical titanium alloy spherical powder comprises the following steps:

[0039] S1: According to the atomic ratio of Ti-35Nb-7Zr-5Ta, the corresponding mass of TiH2, Nb, ZrH2, and Ta powders were ball-milled at 350 rpm / min for 120 min under inert gas protection to obtain composite powder;

[0040] S2: The milled composite powder is sent into a vacuum sintering furnace. When the vacuum degree in the vacuum sintering furnace reaches 1.0×10 -3 After Pa, the temperature was raised to 1200°C at a rate of 10°C / min and kept at that temperature for 180min; then the furnace was cooled; and alloy powder with an average particle size of less than 100μm was obtained by screening.

[0041] S3: subjecting alloy powder having an average particle size of less than 100 μm to radio frequency plasma spheroidization, with a plasma output power of 40 kW; obtaining spherical Ti-35Nb-7Zr-5Ta alloy powder.

[0042] Example No. Ball milling conditions hydrogenation <![CDATA[Particle size (D 90 )]]> Liquidity Oxygen content (%) Nitrogen content (%) Hydrogen content (%) Example 1 200rpm 90min yes ~55μm 38s / 50g 0.16 0.03 0.012 Example 2 200rpm 120min yes ~51μm 37s / 50g 0.18 0.04 0.009 Comparative Example 1 350rpm 90min no ~75μm 55s / 50g 0.26 0.09 0.012 Comparative Example 2 350rpm 120min no ~73μm 57s / 50g 0.31 0.11 0.01

[0043] Table 1. Process conditions and powder properties of the examples

[0044] As shown in Table 1, high-energy ball milling leads to an increase in the impurity content of the powder; in comparison, low-speed ball milling can effectively inhibit the increase in the impurity content of the powder; hydrogenation allows the hydrogen-containing alloy powder to quickly absorb heat during the RF plasma spheroidization process to produce hydrogen explosion to generate finer spherical alloy powder, thereby significantly improving the powder refinement and spheroidization effects and significantly enhancing the fluidity; dehydrogenation treatment further reduces the impurity content of the powder.

[0045] Technical features not described in the present invention can be implemented by existing technologies and will not be described in detail here. The present invention is not limited to the above specific embodiments, and changes, modifications, additions or substitutions made by ordinary technicians in the field within the essential scope of the present invention should also fall within the protection scope of the present invention.

Claims

1. A method for preparing low-cost biomedical titanium alloy spherical powder, characterized by: It includes the following steps: S1: Low-energy ball milling: Take titanium, zirconium, niobium or titanium, zirconium, niobium, tantalum single powder or hydride powder, and ball mill according to the designed component ratio to obtain composite powder; The process of low-energy ball milling is as follows: taking titanium, zirconium, niobium or titanium, zirconium, niobium, tantalum single substance powder or hydride powder with an average particle size of less than 100 μm, and subjecting it to low-speed ball milling for 1-2 hours at a speed of 100-250 rpm / min under inert gas protection or in a vacuum environment according to the designed component ratio to obtain a composite powder; S2: hydrogenation: the composite powder is subjected to high temperature vacuum sintering to achieve pre-alloying, and then hydrogenated to obtain hydrogen-containing alloy powder; The hydrogenation process is as follows: the composite powder obtained in step S1 is placed in a vacuum sintering furnace, and the vacuum sintering furnace is evacuated to 1.0×10 -3 Pa, and then heated to 1200°C and kept warm for 2-3h. After the vacuum sintering furnace is cooled to 650°C, high-purity hydrogen is introduced into the vacuum sintering furnace to keep the hydrogen partial pressure in the furnace at 0.5MPa and keep warm for 1-2h before cooling to obtain hydrogen-containing pre-alloyed powder. After sieving, hydrogen-containing alloy powder with an average particle size of less than 100μm is obtained. S3: The hydrogen-containing alloy powder is subjected to radio frequency plasma spheroidization and dehydrogenation treatment.

2. The method for preparing low-cost biomedical titanium alloy spherical powder according to claim 1, characterized in that: In step S3, the hydrogen-containing alloy powder rapidly absorbs heat to hydrogen explode and cools to generate fine spherical alloy powder during the radio frequency plasma spheroidization process, and then undergoes dehydrogenation treatment to obtain spherical titanium-zirconium-niobium alloy powder or titanium-zirconium-niobium-tantalum alloy powder with an average particle size of 50 μm.

3. The method for preparing low-cost biomedical titanium alloy spherical powder according to claim 2, characterized in that: During the radio frequency plasma spheroidization process in step S3, the powder feeding rate of the hydrogen-containing alloy powder is 50-100 g / min, and the plasma output power is 40 kW.

4. The method for preparing low-cost biomedical titanium alloy spherical powder according to claim 3, characterized in that: The dehydrogenation process of step S3 is as follows: the spheroidized powder is placed in a vacuum sintering furnace, and when the vacuum degree reaches 1.0×10 -3 After the temperature drops below Pa, heat up to 750℃ at a rate of 5-15℃ / min, keep warm for 60-120min, and then cool in the furnace.