A method for preparing butyl rubber with low cyclic oligomer content

By introducing a proton capture agent and controlling the reaction conditions during the preparation process of butyl rubber, the generation of cyclic oligomers is reduced, the problem of cyclic oligomer generation in the existing technology is solved, and the bonding performance of butyl rubber is improved. and cure speed, suitable for a variety of applications.

CN116178603BActive Publication Date: 2024-10-18SHANDONG CHAMBROAD SINOPOLY NEW MATERIAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310241461.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-14
Publication Date
2024-10-18
Estimated Expiration
2043-03-14

AI Technical Summary

Technical Problem

There is the generation of cyclic oligomers in the existing butyl rubber production, especially the halogenated cyclic oligomers produced during the halogenation reaction, which are undesirable in some applications and difficult to blend and co-vulcanize with other rubbers, affecting its performance.

Method used

In the preparation process of butyl rubber, proton capture agents are introduced, such as 2,6-di-tert-butylpyridine, 4-methyl-2,6-di-tert-butylpyridine, etc., and are combined with isobutylene, isoprene, chlorine Methane, etc. are used for the reaction, and Lewis acid and initiator are used to control the reaction conditions to reduce the formation of cyclic oligomers.

Benefits of technology

It effectively reduces the content of C13H24 and C21H40 cyclic oligomers in butyl rubber, improves its bonding performance and vulcanization speed, making it more suitable for blending and co-vulcanization with other rubbers, and is suitable for pharmaceutical sealants, medical devices and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004124311810000051
    Figure BDA0004124311810000051
  • Figure BDA0004124311810000061
    Figure BDA0004124311810000061
Patent Text Reader

Abstract

The present invention provides a method for preparing butyl rubber with low cyclic oligomer content, comprising: introducing a proton scavenger during the preparation process. The present invention introduces a proton scavenger into the butyl rubber polymerization process, such as one or more of 2,6-di-tert-butylpyridine, 4-methyl-2,6-di-tert-butylpyridine, 2,4,6-tri-tert-butylpyridine, piperidine, triethylamine, and 4-hydroxy-2,2,6,6-tetramethylpiperidine-1-oxyl free radicals. The proton scavenger in the present invention can capture free protons in the system, inhibit and eliminate uncontrollable initiation caused by trace amounts of free protons that may exist in the system, thereby reducing the content of oligomers initiated by protons, and the prepared butyl rubber has lower cyclic oligomers (C 13 H 24 and C 21 H 40 )content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of copolymers, and in particular relates to a method for preparing butyl rubber with low cyclic oligomer content, and specifically relates to a method for producing isoolefin and multiolefin copolymers containing proton scavengers and the isoolefin and multiolefin copolymers produced therefrom. Background Art

[0002] Butyl rubber (IIR) is a kind of synthetic rubber, synthesized from isobutylene and a small amount of isoprene. Isoprene is randomly distributed on the molecular chain, and its content accounts for 0.6mol% to 3.0mol% of the main chain. Butyl rubber has excellent air tightness, water tightness, heat aging resistance, damping and shock absorption, electrical insulation, chemical stability, and good ozone resistance and weather resistance. Butyl rubber is difficult to blend and co-vulcanize with other general rubbers due to its low molecular chain polarity, poor adhesion, low unsaturation, and slow vulcanization speed. Butyl rubber is used in inner tubes, vulcanized bladders, capacitor plugs, sealants, damping blocks, latex gloves, and ball bladders.

[0003] Halogenated butyl rubber is a chemically modified product of butyl rubber. It is made by dissolving butyl rubber in a non-polar solvent, and the allyl group on its molecular chain undergoes a substitution reaction with halogen to transform into an allyl halide structure. Halogenated butyl rubber retains the original properties of butyl rubber. The introduction of halogen atoms changes the polarity of the molecular chain and improves the bonding performance; the presence of highly active allyl halide atoms increases the vulcanization speed, allowing it to be co-vulcanized with general-purpose elastomers.

[0004] Since the industrial production of butyl rubber, the raw material route, production process and structure of the polymerization reactor have not changed much. Generally, methyl chloride is used as a diluent, and Lewis acid (aluminum trichloride or ethylaluminum dichloride) and proton donor (hydrogen halide, alcohol, phenol, carboxylic acid and sulfonic acid and water) are used as the initiation system. Controlling the amount of these two can adjust the conversion rate of the monomer and the molecular weight of the product. However, polymerization initiated by proton acid alone will produce oligomers. In the production of butyl rubber, there will be C 13 H 24 and C 21 H 40 Cyclic oligomers are generated. The halogenation reaction of butyl rubber also leads to the halogenation reaction of cyclic oligomers to form halogenated products. Such cyclic oligomers, especially halogenated cyclic oligomers, are undesirable in drug seals, closures, blood sampling plugs, medical devices and food grade applications. Therefore, it is very necessary to reduce the halogenated cyclic oligomers in halogenated butyl rubber. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a method for preparing butyl rubber with a low cyclic oligomer content. The butyl rubber prepared by the method provided by the present invention has a low cyclic oligomer content.

[0006] The present invention provides a method for preparing butyl rubber with low cyclic oligomer content, comprising:

[0007] A proton scavenger is introduced during the preparation process.

[0008] Preferably, the proton scavenger is selected from one or more of 2,6-di-tert-butylpyridine, 4-methyl-2,6-di-tert-butylpyridine, 2,4,6-tri-tert-butylpyridine, piperidine, triethylamine, and 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl free radical.

[0009] Preferably, specifically including:

[0010] Isobutylene, isoprene, methyl chloride and a proton scavenger are reacted.

[0011] Preferably, Lewis acid is used in the reaction process.

[0012] Preferably, an initiator is used in the reaction process.

[0013] Preferably, the reaction time is 5 to 30 minutes.

[0014] Preferably, after the reaction is completed, ethanol is used to terminate the reaction.

[0015] Preferably, after the reaction is completed, the step further comprises:

[0016] The unreacted raw materials were removed by flash evaporation.

[0017] Preferably, after the reaction is completed, the step further comprises:

[0018] The resulting reaction product is mixed with an antioxidant.

[0019] Preferably, after the reaction is completed, the step further comprises:

[0020] The rubber is boiled in a water bath and then the water is removed to obtain butyl rubber.

[0021] The present invention introduces a proton scavenger into the butyl rubber polymerization process, such as one or more of 2,6-di-tert-butylpyridine, 4-methyl-2,6-di-tert-butylpyridine, and 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl free radical, which can reduce the C 13 H 24 and C 21 H 40 Content of cyclic oligomers. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] The present invention provides a method for preparing butyl rubber with low cyclic oligomer content, comprising:

[0024] A proton scavenger is introduced during the preparation process.

[0025] In the present invention, the method for preparing the butyl rubber with low cyclic oligomer content preferably specifically comprises:

[0026] Isobutylene, isoprene, methyl chloride and a proton scavenger are reacted.

[0027] In the present invention, the proton scavenger is preferably selected from one or more of 2,6-di-tert-butylpyridine, 4-methyl-2,6-di-tert-butylpyridine, 2,4,6-tri-tert-butylpyridine, piperidine, triethylamine, and 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl free radical.

[0028] In the present invention, Lewis acid is preferably used in the reaction process; the Lewis acid is preferably a hexane solution of ethylaluminum dichloride, and the concentration of the hexane solution of ethylaluminum dichloride is preferably 15-25wt%, more preferably 20wt%.

[0029] In the present invention, a dichloromethane solution of HCl is preferably used in the reaction process; the dichloromethane solution of HCl is preferably prepared by bubbling anhydrous HCl gas into dichloromethane.

[0030] In the present invention, the reaction is preferably carried out under the action of an initiator, and the initiator preferably includes:

[0031] Dichloromethane, HCl, and ethylaluminum dichloride.

[0032] In the present invention, the initiator is preferably prepared by the dichloromethane solution of the above-mentioned Lewis acid and HCl; the concentration of ethylaluminum dichloride in the initiator is preferably 0.1-0.3wt%, more preferably 0.2wt%; the molar ratio of HCl to ethylaluminum dichloride is preferably 1:(3-5), more preferably 1:4.

[0033] In the present invention, it is preferred that the initiator is cooled to the reaction temperature.

[0034] In the present invention, the mass ratio of isobutylene, isoprene, methyl chloride and proton scavenger is preferably 100:(2-5):(300-150):(0.01-1), more preferably 100:(3-4):(200-250):(0.05-0.8), and most preferably 100:3.5:230:(0.1-0.5); the mass ratio of isobutylene and initiator is preferably 1:(0.3-3), more preferably 1:(0.5-2), and most preferably 1:(1-1.5).

[0035] In the present invention, the reaction is preferably carried out in a reactor; the reactor is preferably a stainless steel reactor; the reactor is preferably replaced with a dry inert gas; the reaction is preferably carried out in an inert gas; the inert gas is preferably a dry inert gas; the inert gas is preferably nitrogen; the volume of the reactor is preferably 3 to 5 L, more preferably 4 L; the reactor is preferably an externally electrically driven jacketed reactor with a double-layer four-blade stainless steel impeller, and the temperature of the jacket and the reactor is preferably measured by a thermocouple; preferably, a circulating C-125 refrigerant is introduced into the jacket to control the temperature of the reactor to the reaction temperature.

[0036] In the present invention, the reaction temperature is preferably -85 to -97.5°C, more preferably -90 to -95°C, and most preferably -93°C; the reaction time is preferably 5 to 30 minutes, more preferably 10 to 20 minutes, and most preferably 15 minutes.

[0037] In the present invention, after the reaction is completed, ethanol is preferably used to terminate the reaction, and the ethanol is preferably cold ethanol.

[0038] In the present invention, the termination reaction preferably further comprises:

[0039] The obtained reaction product is mixed with hexane and then flash-evaporated to remove methyl chloride and unreacted isobutylene and isoprene.

[0040] In the present invention, the hexane is preferably cold hexane; the temperature of the flash evaporation is preferably 40-50°C, more preferably 45°C.

[0041] In the present invention, after the flash evaporation is completed, the glue solution is fully dissolved and then mixed with the antioxidant.

[0042] In the present invention, the dissolution time is preferably 2 to 4 hours, more preferably 3 hours; the antioxidant is preferably antioxidant 390; the mass of the antioxidant is preferably 0.03 to 0.07% of the mass of the glue, more preferably 0.05%.

[0043] In the present invention, after mixing with the antioxidant, the n-hexane is preferably removed by a water bath method, and then water is removed to obtain butyl rubber.

[0044] In the present invention, the water bath method preferably uses a water bath pot with hot water to boil the rubber to remove the n-hexane; the temperature of the hot water is preferably 98-100° C.; and the water removal is preferably carried out by an open mixing mill.

[0045] The present invention introduces a proton scavenger into the butyl rubber polymerization process, such as one or more of 2,6-di-tert-butylpyridine, 4-methyl-2,6-di-tert-butylpyridine, 2,4,6-tri-tert-butylpyridine, piperidine, triethylamine, and 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl free radical. The proton scavenger in the present invention can capture free protons in the system, inhibit and eliminate uncontrollable initiation caused by trace amounts of free protons that may exist in the system, thereby reducing the content of oligomers initiated by protons, and the prepared butyl rubber has lower cyclic oligomers (C 13 H 24 and C 21 H 40 )content.

[0046] Examples 1 to 5 and Comparative Example 1

[0047] The 4L stainless steel reactor was replaced with dry nitrogen to ensure that all examples were polymerized in dry inert gas. The 4L reactor was an externally electrically driven jacketed reactor with a double-layer four-blade stainless steel impeller. The temperature of the jacket and the reactor was measured by a thermocouple. The reactor was cooled to the desired reaction temperature of -85 to -97.5°C by passing a circulating C-125 refrigerant into the jacket.

[0048] High-purity isobutylene, isoprene, and methyl chloride were taken from the production unit and used as they were; the Lewis acid was a 20 wt% ethylaluminum dichloride-hexane solution. Anhydrous HCl gas was bubbled into the chromatographic dichloromethane to prepare a HCl / CH2Cl2 solution, and a 0.1 mol / L standard solution was used to titrate the HCl concentration in the HCl / CH2Cl2 solution.

[0049] At the polymerization temperature, add isobutylene, isoprene, methyl chloride, and a proton scavenger to a reactor cooled to the reaction temperature. Prepare an HCl / ethylaluminum dichloride initiator system in dichloromethane (using a 20wt% ethylaluminum dichloride / hexane solution and an HCl / CH2Cl2 solution) so that the concentration of ethylaluminum dichloride is 0.2wt%, the molar ratio of HCl to ethylaluminum dichloride is 1:4, and the initiator system is cooled to the reaction temperature. Use a microinjection pump to add the cooled initiator system to the reactor, and add cold ethanol to terminate the reaction after 5 to 30 minutes of reaction. Add about 2L of cold hexane to the reactor, and slowly heat the reactor to 45°C to flash off methyl chloride and unreacted isobutylene and isoprene. After the glue solution is fully dissolved for 2 to 4 hours, add 0.05wt% of antioxidant 390. Take out the glue solution, boil the glue in a water bath containing 98 to 100°C hot water until the n-hexane is removed, and remove water with an open mill to obtain a butyl rubber product.

[0050] The molecular weight of the product was determined by GPC (gel permeation chromatography). The unsaturation of the product was determined by 1H-NMR (nuclear magnetic hydrogen spectrum). The oligomer content (C) of the product was determined by gas chromatography-hydrogen flame ionization detector (GC-FID). 13 H 24 and C 21 H 40 The reaction raw materials, the amounts of reaction raw materials used and the test results obtained in Examples 1 to 5 and Comparative Example 1 are as follows:

[0051]

[0052]

[0053] The present invention introduces a proton scavenger into the butyl rubber polymerization process, such as one or more of 2,6-di-tert-butylpyridine, 4-methyl-2,6-di-tert-butylpyridine, 2,4,6-tri-tert-butylpyridine, piperidine, triethylamine, and 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl free radical. The proton scavenger in the present invention can capture free protons in the system, inhibit and eliminate uncontrollable initiation caused by trace amounts of free protons that may exist in the system, thereby reducing the content of oligomers initiated by protons, and the prepared butyl rubber has lower cyclic oligomers (C 13 H 24 and C 21 H 40 )content.

[0054] Although the present invention has been described and illustrated with reference to specific embodiments of the present invention, these descriptions and illustrations do not limit the present invention. It will be clearly understood by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention as defined by the appended claims, so that specific circumstances, materials, material compositions, materials, methods or processes are suitable for the goals, spirit and scope of the present application. All such modifications are intended to be within the scope of the appended claims. Although the methods disclosed herein have been described with reference to specific operations performed in a specific order, it should be understood that these operations may be combined, subdivided or reordered to form equivalent methods without departing from the teachings of the present invention. Therefore, unless specifically indicated herein, the order and grouping of operations are not limitations of the present application.

Claims

1. A method for preparing butyl rubber with low cyclic oligomer content, comprising: The isobutylene, isoprene, methyl chloride and a proton scavenger are reacted; the reaction time is 5 to 30 minutes, and the reaction temperature is -90 to -95°C; after the reaction is completed, ethanol is used to terminate the reaction; the mass ratio of the isobutylene, isoprene, methyl chloride and the proton scavenger is 100:3.5:230:(0.1 to 0.5); the mass ratio of the isobutylene and the initiator is 1:(1 to 1.5); The reaction is carried out under the action of an initiator; the initiator comprises: ethylaluminum dichloride, HCl and dichloromethane; the concentration of ethylaluminum dichloride in the initiator is 0.1-0.3 wt %, and the molar ratio of HCl to ethylaluminum dichloride is 1:(3-5); The proton scavenger is selected from 2,4,6-tri-tert-butylpyridine and / or 4-hydroxy-2,2,6,6-tetramethylpiperidin-1-oxyl free radical.

2. The preparation method according to claim 1, characterized in that: After the reaction is completed, it also includes: The unreacted raw materials were removed by flash evaporation.

3. The preparation method according to claim 1, characterized in that: After the reaction is completed, it also includes: The resulting reaction product is mixed with an antioxidant.

4. The preparation method according to claim 1, characterized in that: After the reaction is completed, it also includes: The rubber is boiled in a water bath and then the water is removed to obtain butyl rubber.

Citation Information

Patent Citations

  • Resource-saving preparation method of isoolefine and conjugated diene copolymer

    CN101357960A