A method for the synergistic deep reduction of copper smelting slag by high-carbon fly ash and biochar to recover iron.
The fayalite in the copper smelting slag is converted into metallic iron through a mixed reducing agent of high-carbon fly ash and biochar, which solves the problems of low iron recycling efficiency and the use of non-renewable fuel in the existing technology, and achieves high efficiency and environmental protection. The iron recycling effect.
Patent Information
- Application Number
- CN202310208470.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-07
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-03-07
AI Technical Summary
In the existing technology, the recycling efficiency of iron in copper smelting slag is low, and non-renewable fossil fuel pulverized coal is commonly used as a reducing agent, resulting in resource waste and environmental pollution.
Using high-carbon fly ash and biochar as mixed reducing agents, the fayalite in copper smelting slag is converted into metallic iron particles through high-temperature reduction, and enriched and recycled through grinding and magnetic separation to reduce the use of fossil fuels and environmental pollution.
It achieves efficient recycling of iron in copper smelting slag, reduces the use of non-renewable fossil fuels, reduces environmental impact, and improves the recovery rate and grade of metallic iron to meet the raw material needs of the steel industry.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a method for recovering iron by synergistic deep reduction of copper smelting slag with high-carbon fly ash and biochar. Background Art
[0002] Copper smelting slag is a non-ferrous metal slag produced in the copper smelting process, and its resource utilization has received widespread attention. The iron content in copper smelting slag is generally around 40%, which is higher than the average grade of existing iron ore. Recovering iron resources from copper smelting slag can not only alleviate the pressure on iron ore resources, but also improve the recycling of copper smelting slag resources by mines, providing a practical solution for the secondary utilization of resources. However, most of the iron in copper smelting slag exists in the form of iron olivine, which is difficult to recycle by conventional mineral processing methods. As a renewable and high-quality reducing agent, biochar materials are increasingly valued by researchers at home and abroad in reducing and recovering metallic iron. Biochar materials are rich in carbon, widely available, and renewable. Rational use can reduce fossil fuel consumption and reduce air pollution. High-carbon fly ash is the main solid waste discharged from coal-fired power plants, which contains some unburned carbon and various oxide components.
[0003] Patent CN113578521A discloses a combined smelting process for recovering iron from copper slag flotation tailings, which mixes the magnetic concentrate of copper slag flotation tailings after stage grinding and magnetic separation with coal powder for deep reduction roasting, and grinds and magnetically separates the roasted product to obtain reduced iron powder and magnetic tailings. Although this process can fully recover the iron in copper smelting slag, the reducing agent used is non-renewable fossil fuel coal powder, which consumes a large amount of non-renewable resources. Summary of the invention
[0004] In view of the large amount of iron elements present in copper smelting slag after flotation recovery of copper, the present invention provides a method for recovering iron from copper smelting slag by synergistic deep reduction of high-carbon fly ash and biochar, wherein biochar is a renewable material and high-carbon fly ash is a solid waste from industrial production. The two are mixed as a reducing agent, and high-temperature reduction is used to reduce the iron olivine in the copper smelting slag to metallic iron particles, which are then enriched and recovered by grinding and magnetic separation after aggregation and growth. In addition, by further processing the copper smelting slag waste, the supply of metallic iron can be increased and the impact of metal production on the environment can be reduced. This method can not only reduce the accumulation of copper smelting slag, but also recycle fly ash, while reducing the use of non-renewable fossil fuel coal, thereby achieving the goal of "treating waste with waste, saving energy and reducing emissions".
[0005] In order to achieve the purpose of the present invention, the technical solution adopted by the present invention is as follows:
[0006] A method for recovering iron by synergistic deep reduction of copper smelting slag by high-carbon fly ash and biochar of the present invention comprises the following steps:
[0007] S1. Prepare materials
[0008] The biochar is crushed to obtain biochar powder for later use;
[0009] Dry the copper smelting slag after flotation recovery of copper for later use;
[0010] S2. Mixing
[0011] The high-carbon fly ash and the biochar are uniformly mixed to obtain a mixed reducing agent;
[0012] The copper smelting slag and the mixed reducing agent are mixed evenly to obtain a mixed material;
[0013] Place the mixed material in a crucible, and spread a 2±1mm layer of mixed reducing agent on top to ensure a reducing atmosphere, and cover the crucible;
[0014] S3, Deep Restore
[0015] The crucible containing the mixed material is subjected to deep reduction at 1200°C to 1300°C, and after reduction, it is cooled to room temperature by water cooling and dried to obtain a deep reduction product;
[0016] S4, Grinding and Magnetic Separation
[0017] After the deep reduction product is ground, it is subjected to magnetic separation to obtain magnetic concentrate and magnetic tailings.
[0018] In the above step S1, the copper smelting slag used is the copper smelting slag after flotation recovery of copper, containing 38%-43% by mass of total iron, and the iron mainly exists in the form of fayalite;
[0019] In the above step S1, the biochar and the fixed carbon in the high-carbon fly ash are the main reactants of the reduction reaction, the mass percentage of the fixed carbon in the biochar used is 62.43-68.21%, and the mass percentage of the fixed carbon in the high-carbon fly ash used is 22.34-35.61%;
[0020] In the above step S1, CaO in the high carbon fly ash plays a role in promoting the reduction reaction, and no additional additives need to be added. The mass percentage of CaO in the high carbon fly ash is 5.64-10.92%;
[0021] In the above step S2, the mass ratio of biochar to high carbon fly ash is 1:(2-1);
[0022] In the above step S2, the mixing ratio of the copper smelting slag and the mixed reducing agent is determined by the stoichiometric molar ratio of the oxygen loss of the iron compounds in the copper smelting slag and the fixed carbon in the mixed reducing agent; that is, the carbon-oxygen molar ratio, which is 1.5-2.0;
[0023] The main reaction formula in the above step S3 is:
[0024] Fe2SiO4+C=2Fe+CO 2(g) +2SiO2
[0025] Fe2SiO4+2C+2CaO=2Fe+2CO (g) +Ca2SiO4
[0026] The CaO contained in high carbon fly ash reduces the Gibbs free energy of the reduction reaction of fayalite, which is beneficial to the reduction reaction.
[0027] In the above step S3, the deep reduction time is 60 to 90 minutes;
[0028] In the above step S3, the temperature of the box-type resistance furnace is 1200° C. to 1300° C.;
[0029] In the above step S3, the metallization rate of the product after deep reduction treatment is ≥ 90%;
[0030] In the above step S4, the grinding time is 5 minutes, the grinding fineness is -0.074mm and the content is more than 90%;
[0031] In the above step S4, the magnetic field strength of the magnetic separation is 660-1200 kA / m;
[0032] In the above step S4, the total iron grade of the magnetic concentrate obtained after the deep reduction product is subjected to magnetic separation is ≥90%, and the iron recovery rate is ≥90%.
[0033] Compared with the existing method for recycling iron from copper smelting slag, the characteristics and advantages of the present invention are: for copper smelting slag after flotation recovery of copper, the combined beneficiation and smelting process is adopted compared with the conventional magnetic separation and leaching process to achieve efficient recycling of iron in the copper smelting slag, and the iron silicate (fayalite) is converted into metallic iron through deep reduction by a reducing agent, and finally a high-quality deep-reduced iron product is obtained, providing high-quality raw materials for the subsequent steel industry; renewable biochar and solid waste high-carbon fly ash are used as a mixed reducing agent, which greatly reduces pollution to the environment, reduces the use of fossil fuels, treats waste with waste, and is simple to operate; the high-carbon fly ash in the mixed reducing agent contains a certain amount of CaO, which can promote the reduction reaction, and no other additives need to be added, saving costs. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with embodiments.
[0035] In the copper smelting slag used in the embodiment of the present invention, the ore minerals are mainly fayalite, magnetite and a small amount of hematite, copper mainly exists in the form of chalcopyrite, and the gangue minerals are mainly quartz.
[0036] The mass percentage of TFe in copper smelting slag is 38% to 43%, the mass percentage of SiO2 is 28% to 35%, the mass percentage of Al2O3 is 3% to 7%, and the remainder is Zn, Ca, Mg, S, Pb and Cu, among which:
[0037] The components contained in the copper smelting slag used in Example 1 and the mass percentage of each component are: TFe 40.45%, SiO2 30.54%; the components contained in the copper smelting slag used in Example 2 and the mass percentage of each component are: TFe 39.69%, SiO2 35.41%; the components contained in the copper smelting slag used in Example 3 and the mass percentage of each component are: TFe 40.03%, SiO2 30.89%; the components contained in the copper smelting slag used in Example 4 and the mass percentage of each component are: TFe 42.86%, SiO2 29.42%; the components contained in the copper smelting slag used in Example 5 and the mass percentage of each component are: TFe 41.65%, SiO2 32.85%; the components contained in the copper smelting slag used in Example 6 and the mass percentage of each component are: TFe 38.69%, SiO2 33.56%; the copper smelting slag used in Example 7 contains 39.32% TFe and 28.65% SiO2;
[0038] The components and mass percentages of the components contained in the high carbon fly ash used in Example 1 are: C28.36%, CaO6.58%; the components and mass percentages of the components contained in the high carbon fly ash used in Example 2 are: C 20.54%, CaO 10.94%; the components and mass percentages of the components contained in the high carbon fly ash used in Example 3 are: C32.72%, CaO 5.94%; the components and mass percentages of the components contained in the high carbon fly ash used in Example 4 are: C 25.63%, CaO 7.25%; the components and mass percentages of the components contained in the high carbon fly ash used in Example 5 are: C 29.34%, CaO 6.34%; the components and mass percentages of the components contained in the high carbon fly ash used in Example 6 are: C 30.68%, CaO 8.56%; the components contained in the high carbon fly ash used in Example 7 and the mass percentage of each component are: C 23.56%, CaO 7.54%;
[0039] In the embodiment of the present invention, a KSL-1400 box-type resistance furnace (muffle furnace) is used for deep reduction, and the temperature inside the furnace is 1200-1300°C.
[0040] In the embodiment of the present invention, a rod mill is used for grinding the ore, and the deep reduction product is ground to a -0.074 mm content of more than 90%.
[0041] In the embodiment of the present invention, magnetic separation adopts a magnetic separation tube, the magnetic separation time is 3 to 5 minutes, and the magnetic field strength is 660 to 1200 kA / m.
[0042] In the example of the present invention, the copper smelting slag is placed in an oven for 3 to 5 hours to dry out the moisture before use.
[0043] In the examples of the present invention, except for the mixed biochar and high-carbon fly ash, there is no need to introduce any reducing gas into the furnace or add any reducing agent, nor is there any need to add other additives.
[0044] Example 1
[0045] The copper smelting slag used in this embodiment was taken from a copper smelter in Inner Mongolia, with an iron content of 40.45%. The slag was dried and set aside. The biochar was crushed to obtain biochar powder, which was set aside. The high-carbon fly ash and the biochar were mixed evenly to obtain a mixed reducing agent. The mass ratio of the biochar powder to the high-carbon fly ash in the mixed reducing agent was 1:1.5.
[0046] The copper smelting slag is mixed with a mixed reducing agent to obtain a mixed material with a carbon-oxygen molar ratio of 2.0. The mixed material is placed in a crucible, and a layer of 2±1 mm of the mixed reducing agent is spread on the top to ensure a reducing atmosphere, and the crucible is covered;
[0047] The crucible containing the mixed material is placed in a muffle furnace at a temperature of 1300°C. The actual reduction time is 90 minutes. The reduced product is subjected to magnetic separation to obtain a magnetic concentrate. After the above process, a deep reduction product with a metallization rate of 96.15% can be obtained. After magnetic separation, an iron concentrate product with an iron grade of 96.74% and a recovery rate of 92.72% can be obtained, which meets the requirements of subsequent smelting.
[0048] Comparative Example 1-1
[0049] The same as Example 1, except that the reduction temperature is 1150°C. After testing, it is found that the metallization rate of the deep reduction product is 82.36%, the iron grade of the magnetic concentrate is 85.29%, and the recovery rate is 81.96%. The reason is that the reduction reaction is an endothermic reaction. Increasing the temperature is conducive to the forward progress of the reduction reaction and the generation of more metallic iron. A lower temperature is not conducive to the generation of metallic iron.
[0050] Example 2
[0051] The copper smelting slag used in this embodiment was taken from a copper smelter in Inner Mongolia, with an iron content of 39.69%. The slag was dried and set aside. The biochar was crushed to obtain biochar powder, which was set aside. The high-carbon fly ash and the biochar were mixed evenly to obtain a mixed reducing agent. The mass ratio of the biochar to the high-carbon fly ash was 1:1.
[0052] The copper smelting slag is mixed with the mixed reducing agent to obtain a mixed material with a carbon-oxygen ratio of 2.0. The mixed material is placed in a crucible, and a layer of 2±1 mm of the mixed reducing agent is spread on the top to ensure a reducing atmosphere, and the crucible is covered;
[0053] The crucible containing the mixed material is placed in a muffle furnace at a temperature of 1200°C. The actual reduction time is 90 minutes. The reduced product is subjected to magnetic separation to obtain a magnetic concentrate. After the above process, a deep reduction product with a metallization rate of 90.68% can be obtained. After magnetic separation, an iron concentrate product with an iron grade of 94.53% and a recovery rate of 91.64% can be obtained, which meets the requirements of subsequent smelting.
[0054] Comparative Example 2-1
[0055] The same as Example 2, except that the mass ratio of biochar to high-carbon fly ash is 1:3. After testing, it was found that the metallization rate of the deep reduction product was 86.21%, the iron grade of the magnetic concentrate was 88.52%, and the recovery rate was 87.13%. The reason is that there are more other oxides in the high-carbon fly ash, and too much high-carbon fly ash is not conducive to the formation of metallic iron.
[0056] Comparative Example 2-2
[0057] The same as Example 2, except that the mass ratio of biochar to high-carbon fly ash is 2:1. After testing, it was found that the metallization rate of the deep reduction product was 90.35%, the iron grade of the magnetic concentrate was 90.22%, and the recovery rate was 89.68%. The reason is that the content of high-carbon fly ash is small, the CaO content in the mixed material is reduced, and the reduction reaction is more difficult to carry out.
[0058] Example 3
[0059] The copper smelting slag used in this embodiment was taken from a copper smelter in Yunnan, with an iron content of 40.03%. The slag was dried and set aside. The biochar was crushed to obtain biochar powder, which was set aside. The high-carbon fly ash and the biochar were mixed evenly to obtain a mixed reducing agent. The mass ratio of the biochar powder to the high-carbon fly ash in the mixed reducing agent was 1:2.
[0060] The copper smelting slag is mixed with the mixed reducing agent to obtain a mixed material with a carbon-oxygen ratio of 2.0. The mixed material is placed in a crucible, and a layer of 2±1 mm of the mixed reducing agent is spread on the top to ensure a reducing atmosphere, and the crucible is covered;
[0061] The crucible containing the mixed material is placed in a muffle furnace at a temperature of 1300°C. The actual reduction time is 75 minutes. The reduced product is subjected to magnetic separation to obtain a magnetic concentrate. After the above process, a deep reduction product with a metallization rate of 90.67% can be obtained. After magnetic separation, an iron concentrate product with an iron grade of 95.21% and a recovery rate of 91.76% can be obtained, which meets the requirements of subsequent smelting.
[0062] Example 4
[0063] The copper smelting slag used in this embodiment was taken from a copper smelter in Liaoning, with an iron content of 42.86%. The slag was dried and set aside. The biochar was crushed to obtain biochar powder, which was set aside. The high-carbon fly ash and the biochar were mixed evenly to obtain a mixed reducing agent. The mass ratio of the biochar to the high-carbon fly ash in the mixed reducing agent was 1:1.5.
[0064] The copper smelting slag is mixed with a reducing agent to obtain a mixed material with a carbon-oxygen ratio of 2.0. The mixed material is placed in a crucible, and a layer of 2±1 mm of the mixed reducing agent is spread on the top to ensure a reducing atmosphere, and the crucible is covered;
[0065] The crucible containing the mixed material is placed in a muffle furnace at a temperature of 1250°C. The actual reduction time is 75 minutes. The reduced product is subjected to magnetic separation to obtain a magnetic concentrate. After the above process, a deep reduction product with a metallization rate of 93.56% can be obtained. After magnetic separation, an iron concentrate product with an iron grade of 94.38% and a recovery rate of 92.32% can be obtained, which meets the requirements of subsequent smelting.
[0066] Example 5
[0067] The copper smelting slag used in this embodiment was taken from a copper smelter in Jiangxi Province, with an iron content of 41.65%. The slag was dried and set aside. The biochar was crushed to obtain biochar powder, which was set aside. The high-carbon fly ash and the biochar were mixed evenly to obtain a mixed reducing agent. The mass ratio of the biochar to the high-carbon fly ash in the mixed reducing agent was 1:1.
[0068] The copper smelting slag is mixed with the mixed reducing agent to obtain a mixed material with a carbon-oxygen ratio of 2.0. The mixed material is placed in a crucible, and a layer of 2±1 mm of the mixed reducing agent is spread on the top to ensure a reducing atmosphere, and the crucible is covered;
[0069] The crucible containing the mixed material is placed in a muffle furnace at a temperature of 1275°C. The actual reduction time is 90 minutes. The reduced product is subjected to magnetic separation to obtain a magnetic concentrate. After the above process, a deep reduction product with a metallization rate of 94.26% can be obtained. After magnetic separation, an iron concentrate product with an iron grade of 96.32% and a recovery rate of 94.25% can be obtained, which meets the requirements of subsequent smelting.
[0070] Comparative Example 5-1
[0071] The same as Example 5, except that the reduction time is 45 minutes, and the metallization rate of the reduced product is 84.35%, the total iron grade of the magnetic concentrate is 89.69%, and the iron recovery rate is 92.31%. The reason is that extending the reduction time is conducive to the conversion of iron-containing compounds in the reduced material into metallic iron, and the reduction time is short, the iron-containing compounds in the reduced material cannot be completely converted into metallic iron, and the metallization rate is low.
[0072] Example 6
[0073] The copper smelting slag used in this embodiment was taken from a copper smelter in Baotou, with an iron content of 38.69%. The slag was dried and set aside. The biochar was crushed to obtain biochar powder, which was set aside. The high-carbon fly ash and the biochar were mixed evenly to obtain a mixed reducing agent. The mass ratio of the biochar to the high-carbon fly ash in the mixed reducing agent was 1:1.5.
[0074] The copper smelting slag is mixed with the mixed reducing agent to obtain a mixed material with a carbon-oxygen ratio of 1.75. The mixed material is placed in a crucible, and a layer of 2±1 mm of the mixed reducing agent is spread on the top to ensure a reducing atmosphere, and the crucible is covered;
[0075] The crucible containing the mixed material is placed in a muffle furnace at a temperature of 1250°C. The actual reduction time is 90 minutes. The reduced product is subjected to magnetic separation to obtain a magnetic concentrate with a magnetic separation field strength of 1000 kA / m. After the above process, a deep reduction product with a metallization rate of 96.52% can be obtained. After magnetic separation, an iron concentrate product with an iron grade of 94.21% and a recovery rate of 90.48% can be obtained, which meets the subsequent smelting requirements.
[0076] Comparative Example 6-1
[0077] The same as Example 6, except that the magnetic separation field strength is 1500 kA / m. After testing, it was found that the metallization rate of the deep reduction product was 96.52%, the iron grade of the magnetic concentrate was 86.52%, and the recovery rate was 92.35%. The reason is that the increase in the magnetic field intensity causes some weakly magnetic reduction products to enter the magnetic concentrate, resulting in a decrease in the grade of the magnetic concentrate.
[0078] Example 7
[0079] The copper smelting slag used in this embodiment was taken from a copper smelter in Liaoning, with an iron content of 39.32%. The slag was dried and set aside. The biochar was crushed to obtain biochar powder, which was set aside. The high-carbon fly ash and the biochar were mixed evenly to obtain a mixed reducing agent. The mixed reducing agent had a mass ratio of 1:1 between the biochar and the high-carbon fly ash.
[0080] The copper smelting slag is mixed with the mixed reducing agent to obtain a mixed material with a carbon-oxygen ratio of 1.75. The mixed material is placed in a crucible, and a layer of 2±1 mm of the mixed reducing agent is spread on the top to ensure a reducing atmosphere, and the crucible is covered;
[0081] The crucible containing the mixed material is placed in a muffle furnace at a temperature of 1200°C. The actual reduction time is 75 minutes. The reduced product is subjected to magnetic separation to obtain a magnetic concentrate. After the above process, a deep reduction product with a metallization rate of 94.52% can be obtained. After magnetic separation, an iron concentrate product with an iron grade of 93.54% and a recovery rate of 92.96% can be obtained, which meets the requirements of subsequent smelting.
[0082] Comparative Example 7-1
[0083] The same as Example 7, except that only biochar was added as a reducing agent. After testing, it was found that the metallization rate of the deep reduction product was 89.65%, the iron grade of the magnetic concentrate was 90.02%, and the recovery rate was 91.35%. The reason is that only biochar was added, and the main reaction in the reduction process was Fe2SiO4+C=2Fe+CO 2(g) +2SiO2, its Gibbs free energy is higher, the reaction is not easy to proceed, and less metallic iron is produced.
[0084] Comparative Example 7-2
[0085] The same as Example 7, except that only high-carbon fly ash is added as a reducing agent. After testing, it is found that the metallization rate of the deep reduction product is 85.32%, the iron grade of the magnetic concentrate is 82.36%, and the recovery rate is 89.52%. The reason is that the high-carbon fly ash has a lower fixed carbon content, relatively less reducing substances, and more impurities in the fly ash, resulting in a lower metallization rate, magnetic concentrate grade and recovery rate.
Claims
1. A method for recovering iron by deep reduction of copper smelting slag using high-carbon fly ash and biochar, characterized in that: The high-carbon fly ash and biochar are mixed evenly to obtain a mixed reducing agent; the copper smelting slag and the mixed reducing agent are mixed evenly to obtain a mixed material; the mixed material is deeply reduced, cooled to room temperature, and dried to obtain a deeply reduced product; the deeply reduced product is ground and then magnetically separated to obtain a magnetically separated concentrate and a magnetically separated tailings; In terms of mass ratio, the ratio of biochar to high carbon fly ash is 1:(2~1); The magnetic field strength of magnetic separation is 660~1200kA / m; The metallization rate of the product after deep reduction treatment is ≥90%; the total iron grade of the magnetic concentrate obtained after magnetic separation of the deep reduction product is ≥90%, and the iron recovery rate is ≥90%; The deep reduction temperature is 1200℃~1300℃, and the deep reduction time is 60~90 min.
2. The method for recovering iron by deep reduction of copper smelting slag using high carbon fly ash and biochar according to claim 1, characterized in that: The copper smelting slag used is the copper smelting slag after flotation recovery of copper, which contains 38%-43% of total iron by mass, and the iron mainly exists in the form of fayalite.
3. The method for recovering iron by deep reduction of copper smelting slag using high carbon fly ash and biochar according to claim 1, characterized in that: The mass percentage of fixed carbon in biochar is 62.43%~68.21%, the mass percentage of fixed carbon in high-carbon fly ash is 22.34%~35.61%; the mass percentage of CaO in high-carbon fly ash is 5.64%~10.92%.
4. The method for recovering iron by deep reduction of copper smelting slag using high carbon fly ash and biochar according to claim 1, characterized in that: The mixing ratio of the copper smelting slag and the mixed reducing agent is determined by the stoichiometric molar ratio of the oxygen loss of the iron compounds in the copper smelting slag and the fixed carbon in the mixed reducing agent, specifically, the carbon-oxygen molar ratio is 1.5-2.
0.
5. The method for recovering iron by deep reduction of copper smelting slag using high carbon fly ash and biochar according to claim 1, characterized in that: The grinding time is 5 minutes, the grinding fineness is -0.074mm and the content is more than 90%.
Citation Information
Cited By
Method for recovering iron from high-iron tungsten smelting slag through selective hydrogen reduction-magnetic separation
CN122168892A