A thermal processing method for fine particle reinforced aluminum alloy composite material

Through the multi-directional cooling forging method, the agglomeration problem in fine particle-reinforced aluminum alloy composite materials is solved, the particles are evenly distributed and the mechanical properties are improved, and the requirements for high modulus, high strength and fatigue performance are met.

CN116179974BActive Publication Date: 2024-10-25ALUMICS MATERIALS INSTIUTUTE ANHUI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310153900.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-23
Publication Date
2024-10-25
Estimated Expiration
2043-02-23

AI Technical Summary

Technical Problem

Fine particle reinforced aluminum alloy composite materials are prone to agglomeration during thermal processing, resulting in limited mechanical properties and uneven particle distribution, making it difficult to meet the requirements for high modulus, high strength and fatigue performance.

Method used

A multi-directional cooling forging method is adopted, and through six passes of forging treatment, the forging direction and temperature range of the aluminum alloy composite material are gradually changed to uniformly disperse the particles and improve the microstructure.

Benefits of technology

It significantly improves the strength, plasticity and mechanical properties of composite materials, eliminates anisotropy, and is suitable for the processing of industrial large-size workpieces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116179974B_ABST
    Figure CN116179974B_ABST
Patent Text Reader

Abstract

The invention discloses a hot working method for a fine particle reinforced aluminum alloy composite material. The aluminum alloy composite material is homogenized and extruded, and then subjected to multi-directional temperature reduction forging and finally heat treatment, thereby providing a simple and easy-to-operate hot working method to improve the uniform distribution of particles in the fine particle reinforced aluminum alloy composite material, improve the mechanical properties of the composite material and improve the anisotropy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to metal material processing, in particular to a thermal processing method for a fine particle reinforced aluminum alloy composite material. Background Art

[0002] Aluminum alloy is widely used in the aerospace field due to its medium strength, good plasticity, good corrosion resistance and excellent damage tolerance. However, with the development of the aerospace and automotive fields, aluminum alloy materials are difficult to meet the requirements of high modulus, high strength and fatigue performance. Particle-reinforced metal matrix composites have received more attention and extremely broad application prospects in the fields of aerospace and automobiles due to their high specific strength, high specific modulus, excellent wear resistance and fatigue performance.

[0003] Reducing the particle size can improve the mechanical properties of the composite material. When the size of the reinforcing particles is reduced to below micrometers, the strength and plasticity, processing performance and weldability of the composite material can be significantly improved. However, as the particle size decreases, the specific surface area increases, resulting in serious agglomeration in the alloy melt, which limits the further improvement of the mechanical properties and is prone to forming anisotropic distribution characteristics during subsequent deformation processing. In short, the uneven distribution of particles limits the strengthening effect of the reinforcing particles, which is ultimately not conducive to the improvement of mechanical properties. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a heat processing method for a fine particle reinforced aluminum alloy composite material, which is characterized in that it comprises the steps of: homogenizing and extruding a rectangular aluminum alloy composite material, and then performing multi-directional cooling forging; the multi-directional cooling forging treatment comprises six passes: the rectangular aluminum alloy composite material comprises three faces A, B, and C with common vertices, the forging direction of the first pass is parallel to the extrusion direction of the rectangular aluminum alloy composite material, the forging face is face A, the cooling range is 550-400°C, and then water cooling is performed, and after forging, the long axis direction of the rectangular body is parallel to face A; the forging direction of the second pass is parallel to the long axis direction, the forging face is face B, the cooling range is 500-350°C, and then water cooling is performed, and after forging, the long axis direction of the rectangular body is parallel to face B; the third pass is parallel to the long axis direction, the forging face is face B, the cooling range is 500-350°C, and then water cooling is performed, and after forging, the long axis direction of the rectangular body is parallel to face B; The forging direction of each pass is parallel to the long axis direction, the forging surface is the C surface, the temperature reduction interval is 450-300℃, and then water cooling is performed. After forging, the long axis direction of the cuboid is parallel to the C surface; the forging direction of the fourth pass is parallel to the long axis direction, the forging surface is the A surface again, the temperature reduction interval is 550-400℃, and then water cooling is performed. After forging, the long axis direction of the cuboid is parallel to the A surface again; the forging direction of the fifth pass is parallel to the long axis direction, the forging surface is the B surface again, the temperature reduction interval is 500-350℃, and then water cooling is performed. After forging, the long axis direction of the cuboid is parallel to the B surface again; the forging direction of the sixth pass is parallel to the long axis direction, the forging surface is the C surface again, the temperature reduction interval is 450-400℃, and then water cooling is performed. After forging, the long axis direction of the cuboid is parallel to the C surface again.

[0005] Furthermore, the aluminum alloy composite material is a TiB2 particle reinforced 7075 alloy composite material.

[0006] Furthermore, the average size of TiB2 is less than 1 micron and the mass fraction is 1%.

[0007] Furthermore, the aluminum alloy composite material is a TiB2 particle reinforced 7055 alloy composite material.

[0008] Furthermore, the average size of TiB2 is less than 1 micron and the mass fraction is 5%.

[0009] Furthermore, the aluminum alloy composite material is a TiB2 particle reinforced 2024 alloy composite material which is an aluminum-based composite material.

[0010] Furthermore, the average size of TiB2 is less than 1 micron and the mass fraction is 6%.

[0011] Furthermore, the aluminum alloy composite material is a TiB2 particle reinforced 6061 alloy composite material which is an aluminum-based composite material.

[0012] Furthermore, the average size of TiB2 is less than 1 micron and the mass fraction is 10%.

[0013] The invention provides a hot working method for homogenizing agglomerated particles in a fine particle reinforced Al-based composite material. Through the hot working method, the phenomenon of particle agglomeration in the fine particle reinforced Al-based composite material is improved, and the particles are evenly dispersed and distributed in the aluminum alloy matrix, thereby improving the comprehensive mechanical properties of the composite material and significantly improving the anisotropy of the mechanical properties. The microstructure of the fine particle reinforced aluminum alloy composite material below the micron size shows that nanoparticles usually have serious agglomeration near the grain boundary, and the microstructure inhomogeneity limits the improvement of strength and fatigue properties. After the prepared fine particle reinforced aluminum-based composite material is hot extruded and deformed, and then based on a multi-directional forging method, after six multi-directional cooling forgings, the agglomerated fine reinforcement particles are dispersed, and the matrix grains are significantly refined, which is beneficial to improve the strength and plasticity of the alloy. The mechanical property test results show that the hot working process improves the strength and plasticity of the composite material at the same time, and the anisotropy is basically eliminated. The process method of the invention is simple and easy to operate, can effectively improve the comprehensive mechanical properties of the deformed particle reinforced aluminum alloy composite material, and is suitable for the processing and application of large-sized workpieces in industrialization.

[0014] The concept, specific structure and technical effects of the present invention will be further described below in conjunction with the accompanying drawings to fully understand the purpose, characteristics and effects of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a schematic diagram of the multi-directional six-pass cooling forging in the present invention;

[0016] Figure 2 is a microstructure morphology diagram of the extruded aluminum-based composite material of the present invention;

[0017] Figure 3 This is a microstructure morphology diagram of the aluminum-based composite material after six deformations in the present invention. DETAILED DESCRIPTION

[0018] The following describes several preferred embodiments of the present invention with reference to the drawings in the specification, so that the technical content is clearer and easier to understand. The present invention can be embodied in many different forms of embodiments, and the protection scope of the present invention is not limited to the embodiments mentioned in the text.

[0019] The invention provides a thermal processing method for agglomerated reinforced particles in dispersed fine particle reinforced Al-based composite materials, wherein the aluminum alloy composite material is homogenized and extruded, then subjected to multi-directional temperature reduction forging, and finally subjected to heat treatment.

[0020] The multi-directional cooling forging process includes six passes. The first forging direction is parallel to the extrusion direction of the rectangular aluminum alloy composite material, and the cooling range is 550-400℃, and then water cooling. The second forging direction is perpendicular to the first forging direction, that is, parallel to the long axis direction, and the cooling range is 500-350℃, and then water cooling. The third forging direction is perpendicular to the second forging direction, that is, parallel to the long axis direction, and the cooling range is 450-300℃, and then water cooling. The fourth forging direction is perpendicular to the third forging direction, that is, parallel to the long axis direction, and the cooling range is 550-400℃, and then water cooling. The fifth forging direction is perpendicular to the fourth forging direction, that is, parallel to the long axis direction, and the cooling range is 500-350℃, and then water cooling. The sixth forging direction is perpendicular to the fifth forging direction, that is, parallel to the long axis direction, and the cooling range is 450-400℃, and then water cooling.

[0021] Example 1

[0022] TiB2 particle reinforced 7075 alloy composite is an aluminum-based composite material, with an average TiB2 size of less than 1 micron and a mass fraction of 1%. Figure 1 The multi-directional six-pass cooling forging process is carried out, and the force direction of each pass of hot working is perpendicular to the deformation direction of the previous pass, which is conducive to the shear deformation between the particle strips, thereby evenly dispersing the particles, and then obtaining an aluminum-based composite material with uniform distribution of enhanced particles. Specifically, Figure 1 As shown, the aluminum-based composite material is a cuboid, and the cuboid includes three common vertex vertical surfaces A, B, and C. The first forging direction is parallel to the extrusion direction of the cuboid aluminum alloy composite material, the forging surface is the A surface, the temperature drop range is 550-400℃, and then water cooling. The second forging direction is perpendicular to the first forging direction, that is, parallel to the long axis direction, the forging surface is the B surface, the temperature drop range is 500-350℃, and then water cooling. The third forging direction is perpendicular to the second forging direction, that is, parallel to the long axis direction, the forging surface is the C surface, the temperature drop range is 450-300℃, and then water cooling. The fourth forging direction is perpendicular to the third forging direction, that is, parallel to the long axis direction, the forging surface is the A surface, the temperature drop range is 550-400℃, and then water cooling. The fifth forging direction is perpendicular to the fourth forging direction, that is, parallel to the long axis direction, the forging surface is the B surface, the temperature drop range is 500-350℃, and then water cooling. The sixth forging direction is perpendicular to the fifth forging direction, that is, parallel to the long axis direction, the forging surface is the C surface, the temperature drop range is 450-400℃, and then water cooling. The final composite material has a room temperature yield strength of 660MPa, a tensile strength of 760MPa, and an elongation of 15%.

[0023] Example 2

[0024] TiB2 particle reinforced 7055 alloy composite material is an aluminum-based composite material, with an average TiB2 size of less than 1 micron and a mass fraction of 5%. Figure 1 The multi-directional six-pass cooling forging process is carried out, and the force direction of each pass of hot working is perpendicular to the deformation direction of the previous pass, which is conducive to the shear deformation between the particle strips, thereby evenly dispersing the particles, and then obtaining an aluminum-based composite material with uniform distribution of enhanced particles. Specifically, Figure 1 As shown, the aluminum-based composite material is a cuboid, and the cuboid includes three common vertex vertical surfaces A, B, and C. The first forging direction is parallel to the extrusion direction of the cuboid aluminum alloy composite material, the forging surface is the A surface, the temperature drop range is 550-400℃, and then water cooling. The second forging direction is perpendicular to the first forging direction, that is, parallel to the long axis direction, the forging surface is the B surface, the temperature drop range is 500-350℃, and then water cooling. The third forging direction is perpendicular to the second forging direction, that is, parallel to the long axis direction, the forging surface is the C surface, the temperature drop range is 450-300℃, and then water cooling. The fourth forging direction is perpendicular to the third forging direction, that is, parallel to the long axis direction, the forging surface is the A surface, the temperature drop range is 550-400℃, and then water cooling. The fifth forging direction is perpendicular to the fourth forging direction, that is, parallel to the long axis direction, the forging surface is the B surface, the temperature drop range is 500-350℃, and then water cooling. The sixth forging direction is perpendicular to the fifth forging direction, that is, parallel to the long axis direction, the forging surface is the C surface, the temperature drop range is 450-400℃, and then water cooling. The final composite material has a room temperature yield strength of 700MPa, a tensile strength of 800MPa, and an elongation of 12%.

[0025] Example 3

[0026] TiB2 particle reinforced 2024 alloy composite is an aluminum-based composite material with an average TiB2 size of less than 1 micron and a mass fraction of 6%. Figure 1 The multi-directional six-pass cooling forging process is carried out, and the force direction of each pass of hot working is perpendicular to the deformation direction of the previous pass, which is conducive to the shear deformation between the particle strips, thereby evenly dispersing the particles, and then obtaining an aluminum-based composite material with uniform distribution of enhanced particles. Specifically, Figure 1As shown, the aluminum-based composite material is a cuboid, and the cuboid includes three common vertex vertical surfaces A, B, and C. The first forging direction is parallel to the extrusion direction of the cuboid aluminum alloy composite material, the forging surface is the A surface, the temperature drop range is 550-400℃, and then water cooling. The second forging direction is perpendicular to the first forging direction, that is, parallel to the long axis direction, the forging surface is the B surface, the temperature drop range is 500-350℃, and then water cooling. The third forging direction is perpendicular to the second forging direction, that is, parallel to the long axis direction, the forging surface is the C surface, the temperature drop range is 450-300℃, and then water cooling. The fourth forging direction is perpendicular to the third forging direction, that is, parallel to the long axis direction, the forging surface is the A surface, the temperature drop range is 550-400℃, and then water cooling. The fifth forging direction is perpendicular to the fourth forging direction, that is, parallel to the long axis direction, the forging surface is the B surface, the temperature drop range is 500-350℃, and then water cooling. The sixth forging direction is perpendicular to the fifth forging direction, that is, parallel to the long axis direction, the forging surface is the C surface, the temperature drop range is 450-400℃, and then water cooling. The final room temperature yield strength of the composite material is 450MPa, the tensile strength is 610MPa, and the elongation is 16%.

[0027] Example 4

[0028] TiB2 particle reinforced 6061 alloy composite material is an aluminum-based composite material, with an average TiB2 size of less than 1 micron and a mass fraction of 10%. Figure 1 The multi-directional six-pass cooling forging process is carried out, and the force direction of each pass of hot working is perpendicular to the deformation direction of the previous pass, which is conducive to the shear deformation between the particle strips, thereby evenly dispersing the particles, and then obtaining an aluminum-based composite material with uniform distribution of enhanced particles. Specifically, Figure 1As shown, the aluminum-based composite material is a cuboid, and the cuboid includes three common vertex vertical surfaces A, B, and C. The first forging direction is parallel to the extrusion direction of the cuboid aluminum alloy composite material, the forging surface is the A surface, the temperature drop range is 550-400℃, and then water cooling. The second forging direction is perpendicular to the first forging direction, that is, parallel to the long axis direction, the forging surface is the B surface, the temperature drop range is 500-350℃, and then water cooling. The third forging direction is perpendicular to the second forging direction, that is, parallel to the long axis direction, the forging surface is the C surface, the temperature drop range is 450-300℃, and then water cooling. The fourth forging direction is perpendicular to the third forging direction, that is, parallel to the long axis direction, the forging surface is the A surface, the temperature drop range is 550-400℃, and then water cooling. The fifth forging direction is perpendicular to the fourth forging direction, that is, parallel to the long axis direction, the forging surface is the B surface, the temperature drop range is 500-350℃, and then water cooling. The sixth forging direction is perpendicular to the fifth forging direction, that is, parallel to the long axis direction, the forging surface is the C surface, the cooling range is 450-400℃, and then water cooling. Finally, the room temperature yield strength is 320MPa, the tensile strength is 380MPa, and the elongation is 10%.

[0029] from Figure 2 It can be seen that after extrusion deformation, the particles in the aluminum matrix composite material show obvious agglomeration.

[0030] from Figure 3 It can be seen that after six multi-directional deformations, the agglomeration of TiB2 particles in the aluminum-based composite material is significantly improved, and the particles are evenly distributed in the alloy matrix.

[0031] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in the field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in the technical field based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for hot working of a fine particle reinforced aluminum alloy composite material, characterized in that: Includes steps: After homogenizing and extruding the rectangular aluminum alloy composite material, multi-directional cooling forging is performed; The multi-directional cooling forging process includes six passes: the rectangular parallelepiped of the aluminum alloy composite material includes three faces A, B, and C with the same vertices. The forging direction of the first pass is parallel to the extrusion direction of the rectangular parallelepiped aluminum alloy composite material, the forging face is face A, the cooling range is 550-400℃, and then water cooling. After forging, the long axis direction of the rectangular parallelepiped is parallel to face A; the second forging direction is parallel to the long axis direction, the forging face is face B, the cooling range is 500-350℃, and then water cooling. After forging, the long axis direction of the rectangular parallelepiped is parallel to face B; the third forging direction is parallel to the long axis direction, the forging face is face C, the cooling range is 450-300℃, and then water cooling. After forging, the long axis direction of the cuboid is parallel to the C surface; the fourth forging direction is parallel to the long axis direction, the forging surface is the A surface again, the temperature drop interval is 550-400℃, and then water cooling, after forging, the long axis direction of the cuboid is parallel to the A surface again; the fifth forging direction is parallel to the long axis direction, the forging surface is the B surface again, the temperature drop interval is 500-350℃, and then water cooling, after forging, the long axis direction of the cuboid is parallel to the B surface again; the sixth forging direction is parallel to the long axis direction, the forging surface is the C surface again, the temperature drop interval is 450-400℃, and then water cooling, after forging, the long axis direction of the cuboid is parallel to the C surface again.

2. The hot working method of the fine particle reinforced aluminum alloy composite material according to claim 1, wherein: The aluminum alloy composite material is a TiB2 particle reinforced 7075 alloy composite material.

3. The hot working method of the fine particle reinforced aluminum alloy composite material according to claim 2, wherein: The average size of TiB2 is less than 1 micron and the mass fraction is 1%.

4. The hot working method of the fine particle reinforced aluminum alloy composite material according to claim 1, wherein: The aluminum alloy composite material is a TiB2 particle reinforced 7055 alloy composite material.

5. The hot working method of the fine particle reinforced aluminum alloy composite material according to claim 4, wherein: The average size of TiB2 is less than 1 micron and the mass fraction is 5%.

6. The hot working method of the fine particle reinforced aluminum alloy composite material according to claim 1, wherein: The aluminum alloy composite material is a TiB2 particle reinforced 2024 alloy composite material and is an aluminum-based composite material.

7. The hot working method of the fine particle reinforced aluminum alloy composite material according to claim 6, wherein: The average size of TiB2 is less than 1 micron and the mass fraction is 6%.

8. The hot working method of the fine particle reinforced aluminum alloy composite material according to claim 1, wherein: The aluminum alloy composite material is a TiB2 particle reinforced 6061 alloy composite material and is an aluminum-based composite material.

9. The hot working method of the fine particle reinforced aluminum alloy composite material according to claim 8, wherein: The average size of TiB2 is less than 1 micron and the mass fraction is 10%.