A fiber catalytic membrane based on conjugated microporous polymer and its preparation method and application
Through fiber catalytic membranes based on conjugated microporous polymers, the problems of insufficient exposure of active sites of heterogeneous catalysts and low utilization of active oxygen species are solved, and efficient organic pollutant degradation is achieved.
Patent Information
- Application Number
- CN202310155007.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-22
AI Technical Summary
The problems of insufficient exposure of active sites of heterogeneous catalysts, catalyst loss, and low utilization of active oxygen species lead to low degradation efficiency of organic pollutants in water.
Using fiber catalytic membranes based on conjugated microporous polymers, nanofiber membranes are prepared through electrospinning technology, and conjugated microporous polymers are grown in situ on the membranes, combined with Buchwald-Hartwig coupling reactions, to form stable large-ratio nanofiber membranes. The fiber network with fully exposed surface area and active sites combines with advanced oxidation technology to degrade organic pollutants.
It significantly reduces the diffusion distance of organic pollutant molecules to the active sites on the membrane surface, improves the mass transfer efficiency and activation efficiency of the catalytic system, enhances the utilization of active oxygen species, and achieves efficient organic pollutant removal.
Smart Images

Figure CN116180454B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano materials and water treatment, and particularly relates to a fiber catalytic membrane based on a conjugated microporous polymer and a preparation method and application thereof. Background Art
[0002] The efficient degradation of persistent organic pollutants (such as pharmaceuticals, endocrine disruptors, personal care products, etc.) is a key challenge facing the current environmental pollution control. At present, heterogeneous advanced oxidation technology (AOP) achieves successful degradation of organic pollutants in water by generating reactive oxygen species (ROS; hydroxyl radicals, sulfate radicals, and singlet oxygen, etc.) with strong oxidizing ability. As the core material for generating reactive oxygen species, heterogeneous catalysts can overcome the inherent defects of homogeneous advanced oxidation technology, such as secondary pollution and difficulty in catalyst recovery. However, the particulate catalysts dispersed in water face the following problems: ① Agglomeration of particulate catalysts reduces the exposure of active sites; ② Low mass transfer efficiency leads to residual PMS in the system, reducing the oxidation capacity of the heterogeneous catalytic system; ③ The generated ROS cannot quickly contact the target pollutants, resulting in self-quenching of reactive oxygen species or ineffective oxidation reactions (such as reactions with water molecules). In order to achieve an efficient catalytic oxidation system, in addition to the reasonable design and exposure of the catalyst active sites, improvements are still needed in the operation mode of the reactor.
[0003] In recent years, scientists have used methods such as material dimensionality reduction, size control, and crystal surface control to expose the active sites of catalysts as much as possible, thereby enhancing the efficiency of catalytic reactions and achieving the production of a large number of free radicals. However, the lifetime of free radicals is extremely short, which is not conducive to their full diffusion in water. Therefore, how to design a catalytic oxidation reaction system, reduce the mass transfer distance of free radicals to target pollutants, enhance the utilization efficiency of active oxygen species, and achieve efficient removal of organic pollutants is of great significance to the development of water environment treatment technology. Summary of the invention
[0004] The technical problems to be solved by the present invention are: insufficient exposure of active sites of heterogeneous catalysts, catalyst loss and low utilization of active oxygen species. The present invention utilizes the unique inherent microporous characteristics of conjugated microporous polymers and the high flux characteristics of nanofiber membranes to invent a fiber catalytic membrane based on conjugated microporous polymers that has high catalytic active sites, confined precise activation of persulfate, size screening and confined enhanced mass transfer characteristics.
[0005] A method for preparing a fiber catalytic membrane based on a conjugated microporous polymer of the present invention comprises:
[0006] (1) Dissolve polyacrylonitrile in N,N-dimethylformamide solution, add a certain amount of p-phenylenediamine, stir for a period of time to prepare a spinning solution;
[0007] (2) preparing an electrospinning membrane using an electrospinning apparatus, and then drying the electrospinning membrane in a vacuum drying oven;
[0008] (3) In situ growth of conjugated microporous polymer to obtain fibrous catalytic membrane.
[0009] Preferably, in step (1), the molecular weight of polyacrylonitrile is 50000-150000, the mass concentration of polyacrylonitrile in N,N-dimethylformamide is 15wt% to 30wt%; the mass ratio of p-phenylenediamine to polyacrylonitrile is 1: (1 to 2); the stirring temperature is 20 to 60°C, and the time is 0.5 to 24 h.
[0010] Preferably, in step (2), the electrospinning rate is set to 0.2 ~ 2 mL h-1, the working voltage is 10 ~ 25 kV, the distance between the needle and the collector is 10 ~ 20 cm; the drying temperature is 20 ~ 100 ° C, and the drying time is 3 ~ 24h.
[0011] Preferably, the in-situ grown conjugated microporous polymer in step (3) is PTPA, and the preparation method is: in-situ growing the conjugated microporous polymer on the electrospun membrane obtained in step (2) by Buchwald-Hartwig coupling reaction of two monomers, tri(4-bromophenyl)amine and p-phenylenediamine, and vacuum drying after washing to obtain a polymer membrane; the molar ratio of the two monomers, tri(4-bromophenyl)amine and p-phenylenediamine, is 1:(1 ~ 2).
[0012] Preferably, the solvent used in the Buchwald-Hartwig coupling reaction is one or more of toluene and tetrahydrofuran; the palladium catalyst used is bis(dibenzylideneacetone)palladium; the ligand is 2-dicyclohexylphosphine-2', 4',6'-triisopropylbiphenyl; and the alkali used is sodium tert-butoxide.
[0013] Preferably, the coupling reaction system is placed in a Schlenk tube and reacted at 65 or 110°C under a nitrogen atmosphere for 24-48 hours; the washing is: washing with anhydrous methanol, chloroform, and deionized water in sequence until the filtrate is colorless and transparent; the vacuum drying temperature is 25 ~ 80°C, and the vacuum drying time is 12 ~ 48 hours.
[0014] The invention discloses a fiber catalytic membrane based on conjugated microporous polymer prepared by the method.
[0015] The invention discloses an application of a fiber catalytic membrane prepared by the method in continuous flow removal of organic pollutants.
[0016] Preferably, the specific method of the application is: the organic pollutant solution is stirred at 0.5 to 5 mL min -1The organic pollutant solution flows through the fiber catalytic membrane at a flow rate of , and the pH value of the organic pollutant solution is 2 to 11.
[0017] Preferably, the organic pollutant solution further contains one or more of peroxymonosulfate or peroxydisulfate; the concentration of peroxymonosulfate or peroxydisulfate in the organic pollutant solution is 1 ~ 10 mmol L -1 ; The organic pollutants are one or more of phenol, aniline, hydroquinone and bisphenol A. Beneficial Effects
[0018] (1) The present invention in situ grows a conjugated microporous polymer on an electrospun nanofiber membrane through a Buchwald-Hartwig coupling reaction. The staggered arrangement of the fiber skeleton can form a stable fiber network with a large specific surface area and fully exposed active sites. The polymer membrane has good stability and is easy to recycle and utilize.
[0019] (2) The present invention adopts a method that combines membrane separation with advanced oxidation technology. In this system, the diffusion distance of organic pollutant molecules to the active sites on the membrane surface is significantly reduced, which improves the mass transfer of the catalytic system. At the same time, it enhances the activation efficiency between the catalyst and the oxidant, thereby improving the efficient utilization of active oxygen species. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Macroscopic photographs and SEM images at 30 μm size of the PTPA / PAN membrane of the present invention.
[0021] Figure 2 The graph shows the changes in treatment flux and degradation rate of PTPA / PAN membrane and PAN membrane for bisphenol A-containing wastewater over time.
[0022] Figure 3 This is the electron paramagnetic resonance spectrum of PTPA. DETAILED DESCRIPTION
[0023] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally. Example 1
[0024] This example provides a method for preparing a fiber catalytic membrane based on a conjugated microporous polymer, comprising the following steps:
[0025] (1) Dissolve 1.5 g of polyacrylonitrile in 8.5 g of N,N-dimethylformamide solution, add 1.5 g of p-phenylenediamine, and stir for 3 h to form a uniformly dispersed electrospinning solution.
[0026] (2) Inject the spinning solution into the electrospinning equipment and adjust the electrospinning rate to 1 mL min -1 , the working voltage was 15 kV, the distance between the needle and the collector on the spinning equipment was 20 cm, and the spun products were collected and dried at 50 °C for 8 h to obtain the electrospun membrane, which was recorded as PDA / PAN membrane.
[0027] (3) Tri(4-bromophenyl)amine (241 mg, 0.5 mmol, TCI), p-phenylenediamine (35.64 mg, 0.33 mmol, Sinopharm) and PDA / PAN membrane were placed in a Schlenk tube (100 mL), and bis(dibenzylideneacetone)palladium (17.25 mg, 0.03 mmol, TCI), 2-dicyclohexylphosphino-2',4',6'-triisopropylbiphenyl (21.42 mg, 0.45 mmol, TCI), sodium tert-butoxide (336.4 mg, 3.5 mmol, Wokai) were added. 30 mL of tetrahydrofuran was added under nitrogen atmosphere, and the coupling reaction was carried out in an oil bath at 65 °C for 48 h. After the reaction was completed, the mixture was washed twice with anhydrous methanol, chloroform and deionized water at 60 °C for two hours each time to remove unreacted raw materials and oligomers. Finally, the fiber catalytic membrane (PTPA / PAN membrane) was obtained by drying in a vacuum oven at 40°C for 24 h. The SEM image of the membrane is shown in the figure. Figure 1 As shown, a is a macroscopic photograph of the PTPA / PAN membrane, and b is a SEM image of the PTPA / PAN membrane at a size of 30 μm. Example 2
[0028] This example provides a fiber catalytic membrane based on a conjugated microporous polymer, which is specifically similar to Example 1, except that the amount of polyacrylonitrile in step (1) is set to 2.25 g. Example 3
[0029] This example provides a fiber catalytic membrane based on a conjugated microporous polymer, which is specifically similar to Example 1, except that the amount of polyacrylonitrile in step (1) is set to 3 g.
[0030] Comparative Example 1
[0031] This embodiment provides a polyacrylonitrile fiber catalytic membrane, which is specifically similar to Example 1, except that there is no p-phenylenediamine and subsequent in-situ polymerization process, and the prepared membrane is named PAN membrane.
[0032] This example provides a catalytic filtration method for continuous flow removal of organic pollutants using a fiber catalytic membrane, as follows:
[0033] The polymer membrane was placed in a permeation reactor and the organic pollutant solution (containing 2 mg L -1 Organic pollutants, 5 mmol L -1 PMS, organic pollutant solution pH 6) at 2.5 mL min -1 The liquid passed through the polymer membrane at a flow rate of , and samples were taken at the outlet at different time points. The concentration of organic pollutants in the solution was determined by high performance liquid chromatography (the mobile phase was 70% methanol and 30% ultrapure water).
[0034] Taking bisphenol A as a model pollutant, samples were taken at the outlet at 5, 10, 15, 30, 45, 60, 90 and 120 minutes respectively to investigate the degradation effect of the polymer membrane on organic pollutants within 120 minutes. The experimental results are shown in the figure. In the catalytic filtration system, the degradation rate of bisphenol A by the polymer membrane remained above 95% within 60 minutes and remained above 90% within 120 minutes, indicating that the polymer membrane has a good degradation effect on organic pollutants, indicating that the PTPA / PAN membrane / PMS system has good practicality ( Figure 2 ).
[0035] This example provides a method for detecting active oxygen species in an activated PMS experiment using a fiber catalytic membrane, as follows:
[0036] The fiber catalytic membrane was placed in a penetration reactor, and the organic pollutant solution (containing 2 mg L -1 Organic pollutants, 5 mmol L -1 PMS, organic pollutant solution pH 6) at 2.5 mLmin -1 The flow rate of 1.5 mol / L was passed through the polymer membrane, and a sample was taken at the outlet at 5 min. 40 μL of the sample solution was added into a plastic tube containing 20 μL of active oxygen species scavenger (free radical scavenger: dimethylpyridine N-oxide (DMPO), singlet oxygen scavenger: 2,2,6,6-tetramethylpiperidine (TEMP)). After shaking evenly, the active oxygen species signal intensity was tested using an electron paramagnetic resonance spectrometer (EPR). The results are shown in Figure 2. Figure 3 As shown in the figure, a is TMEP capturing singlet oxygen, and b is DMPO capturing free radicals. It can be seen from the figure that when DMPO and TEMP are used as capture agents, obvious superoxide free radicals (O2 ●— ) and singlet oxygen ( 1O2), indicating that superoxide radicals and singlet oxygen are the main active oxygen species in the PTPA / PAN membrane / PMS system.
Claims
1. A method for preparing a fiber catalytic membrane based on a conjugated microporous polymer, Features The steps include: (1) Dissolve polyacrylonitrile in N,N-dimethylformamide solution, add a certain amount of p-phenylenediamine, stir for a period of time to prepare a spinning solution; (2) preparing an electrospinning membrane using an electrospinning apparatus, and then drying the electrospinning membrane in a vacuum drying oven; (3) In situ growth of conjugated microporous polymer to obtain fibrous catalytic membrane; The in-situ grown conjugated microporous polymer is PTPA, and the preparation method is as follows: the two monomers of tri(4-bromophenyl)amine and p-phenylenediamine are subjected to a Buchwald-Hartwig coupling reaction to in-situ grow the conjugated microporous polymer on the electrospinning membrane obtained in step (2), and the polymer membrane is obtained by vacuum drying after washing; the molar ratio of the two monomers of tri(4-bromophenyl)amine and p-phenylenediamine is 1:(1 ~ 2).
2. The preparation method according to claim 1, It is characterized in that In the step (1), the molecular weight of polyacrylonitrile is 50000-150000, the mass concentration of polyacrylonitrile in N,N-dimethylformamide is 15wt% to 30wt%; the mass ratio of p-phenylenediamine to polyacrylonitrile is 1: (1 to 2); the stirring temperature is 20 to 60°C, and the time is 0.5 to 24 h.
3. The preparation method according to claim 1, It is characterized in that The electrospinning rate in step (2) is set to 0.2 ~ 2 mL h -1 , the working voltage is 10 ~ 25 kV, the distance between the needle and the collector is 10 ~ 20 cm; the drying temperature is 20 ~ 100 ℃, and the drying time is 3 ~ 24 h.
4. The preparation method according to claim 1, It is characterized in that The solvent used in the Buchwald-Hartwig coupling reaction is one or more of toluene and tetrahydrofuran; the palladium catalyst used is bis(dibenzylideneacetone)palladium; the ligand is 2-dicyclohexylphosphine-2', 4',6'-triisopropylbiphenyl; and the alkali used is sodium tert-butoxide.
5. The preparation method according to claim 4, It is characterized in that The coupling reaction system is placed in a Schlenk tube and reacted at 65 or 110° C. under a nitrogen atmosphere for 24-48 h; the washing is: washing with anhydrous methanol, chloroform, and deionized water in sequence until the filtrate is colorless and transparent; the vacuum drying temperature is 25 to 80° C., and the vacuum drying time is 12 to 48 h.
6. A fiber catalytic membrane based on conjugated microporous polymer prepared by the method of claim 1.
7. Use of the fiber catalytic membrane according to claim 6 in continuous flow removal of organic pollutants.
8. The use according to claim 7, It is characterized in that The application process is: the organic pollutant solution is stirred at 0.5 ~ 5mL min -1 The flow rate flows through the fiber catalytic membrane; the pH value of the organic pollutant solution is 2 to 11.
9. The use according to claim 8, It is characterized in that The organic pollutant solution further contains one or more of peroxymonosulfate or peroxydisulfate; the concentration of peroxymonosulfate or peroxydisulfate in the organic pollutant solution is 1 to 10 mmol L -1 ; The organic pollutants are one or more of phenol, aniline, hydroquinone and bisphenol A.
Citation Information
Patent Citations
Microporous conjugated polyaniline adsorption material and preparation method thereof, and application of microporous conjugated polyaniline adsorption material in hexavalent chromium adsorption
CN111569846A