Composite negative electrode active materials, including their negative electrodes and lithium batteries

By forming a shell structure of metal oxides and carbonaceous materials on the surface of silicon-based anode active materials, the degradation problem caused by volume changes in silicon-based anode active materials in lithium batteries is solved, thereby improving the stability and cycle characteristics of high-capacity lithium batteries.

CN116190588BActive Publication Date: 2026-11-17SAMSUNG SDI CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211500546.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-26
Filing Date
2022-11-28
Publication Date
2026-11-17
Estimated Expiration
2042-11-28

AI Technical Summary

Technical Problem

Existing silicon-based anode active materials are prone to degradation in lithium batteries due to volume changes caused by charging and discharging, leading to increased internal resistance and decreased cycle performance.

Method used

The composite negative electrode active material is used, including a core and shell structure. The core contains silicon-based materials, and the shell is composed of specific metal oxides and carbonaceous materials, which are formed by chemical bonding. The shell material is located on the core surface in a conformal manner, which buffers volume changes and reduces interfacial resistance.

Benefits of technology

It effectively suppressed the volume change and internal resistance increase of lithium batteries, improved the cycle characteristics and stability of lithium batteries, and enhanced the high-capacity performance of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116190588B_ABST
    Figure CN116190588B_ABST
Patent Text Reader

Abstract

A composite negative electrode active material is provided, as well as a negative electrode and a lithium battery both comprising the composite negative electrode active material. The composite negative electrode active material includes a core and a shell located on the surface of the core and conforming to the surface of the core, wherein the core comprises a silicon-containing structure, a silicon-containing compound, or a combination thereof, and the shell comprises a structure made of M… a O b (0
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims the benefit of priority based on and entitled to Korean Patent Application No. 10-2021-0166115 filed with the Korean Intellectual Property Office on November 26, 2021, the entire disclosure of which is incorporated herein by reference. Technical Field

[0002] One or more embodiments relate to a composite negative active material, and a negative electrode and a lithium battery each including the composite negative active material. Background Art

[0003] To meet the miniaturization and high performance of various devices, lithium batteries are required to have high energy density in addition to miniaturization and weight reduction. That is, high-capacity lithium batteries are becoming increasingly important.

[0004] To realize lithium batteries suitable for these uses, negative active materials with high capacity are being researched.

[0005] Compared with carbonaceous negative active materials, silicon-based negative active materials in the related art are prone to deterioration due to volume changes caused by charging and discharging.

[0006] There is a need to develop a lithium battery that includes a silicon-based negative active material and provides excellent cycle characteristics. Disclosure of Invention

[0007] One or more embodiments include a novel composite negative active material that prevents deterioration of a lithium battery.

[0008] One or more embodiments provide a negative electrode including the composite negative active material.

[0009] One or more embodiments provide a lithium battery including the negative electrode.

[0010] Additional aspects will be set forth in part in the description which follows and, in part, will be apparent from the description, or may be learned by practice of the presented embodiments of the disclosure.

[0011] According to one or more embodiments, a composite negative active material includes a core; and a shell disposed on a surface of the core and conformal to the surface of the core, wherein the core includes a silicon-containing structure, a silicon-containing compound, or a combination thereof, and the shell includes a compound represented by formula M a O b (0<a≤3, 0<b<4, and when a is 1, 2, or 3, b is not an integer), at least one first metal oxide, and a first carbonaceous material, wherein the first metal oxide is disposed in the first carbonaceous material, and M is at least one metal selected from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements.

[0012] According to one or more embodiments, the negative electrode includes a composite negative active material.

[0013] According to one or more embodiments, the negative electrode includes: a dry composite negative active material, a dry conductive material, and a dry binder, wherein the dry composite negative active material includes: a core, and a shell disposed on a surface of the core and conformal with the surface of the core, the core includes a silicon-containing structure, a silicon-containing compound, or a combination thereof, and the shell includes a compound of formula M a O b (0<a≤3, 0<b<4, and when a is 1, 2, or 3, b is not an integer), at least one first metal oxide represented by the formula, and a first carbonaceous material, the first metal oxide is disposed in the first carbonaceous material, and M is at least one metal selected from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements.

[0014] According to one or more embodiments, a lithium battery includes the negative electrode. Brief Description of the Drawings

[0015] The above and other aspects, features, and advantages of certain embodiments of the present disclosure will become more apparent from the following description taken in conjunction with the accompanying drawings, in which:

[0016] Figure 1 is a schematic cross-sectional view of a composite negative active material according to an embodiment;

[0017] Figure 2A are X-ray photoelectron spectroscopy (XPS) spectra of the C1s orbital of the silicon composite structure prepared according to Preparation Example 3 and the composite negative active material prepared according to Example 1;

[0018] Figure 2B are XPS spectra of the O1s orbital of the silicon composite structure prepared according to Preparation Example 3 and the composite negative active material prepared according to Example 1;

[0019] Figure 2C are XPS spectra of the Si2p orbital of the silicon composite structure prepared according to Preparation Example 3 and the composite negative active material prepared according to Example 1;

[0020] Figure 2D are XPS spectra of the Al2p orbital of the silicon composite structure prepared according to Preparation Example 3 and the composite negative active material prepared according to Example 1;

[0021] Figure 3A are XPS spectra of the C1s orbital of the silicon composite structure prepared according to Comparative Example 5 and the composite negative active material prepared according to Example 8;

[0022] Figure 3BThe XPS spectra of the O1s orbitals of the silicon composite structure prepared according to Comparative Example 5 and the composite negative electrode active material prepared according to Example 8 are shown.

[0023] Figure 3C The XPS spectra of the Si2p orbitals of the silicon composite structure prepared according to Comparative Example 5 and the composite negative electrode active material prepared according to Example 8 are shown.

[0024] Figure 3D The XPS spectra of the Al2p orbitals of the silicon composite structure prepared according to Comparative Example 5 and the composite negative electrode active material prepared according to Example 8 are shown.

[0025] Figure 4A This is a scanning electron microscope (SEM) image of the composite negative electrode active material in Example 1;

[0026] Figure 4B This is a SEM-energy dispersive X-ray spectroscopy (EDS) image of the composite negative electrode active material in Example 1;

[0027] Figure 4C This is a SEM image of the composite negative electrode active material in Example 8;

[0028] Figure 4D This is the SEM-energy dispersive spectroscopy (EDS) image of the composite negative electrode active material in Example 8;

[0029] Figure 5 This is a cross-sectional schematic diagram of the composite negative electrode active material according to the embodiments;

[0030] Figure 6 This is a schematic diagram of a lithium battery according to an embodiment;

[0031] Figure 7 This is a schematic diagram of a lithium battery according to an embodiment; and

[0032] Figure 8 This is a schematic diagram of a lithium battery according to an embodiment. Detailed Implementation

[0033] Referring now to embodiments, examples of which are shown in the accompanying drawings, wherein the same reference numerals always refer to the same elements. In this respect, the given embodiments may have different forms and should not be construed as limited to the description set forth herein. Therefore, the embodiments are described below only by reference to the accompanying drawings to explain aspects of this specification. As used herein, the term “and / or” includes any and all combinations of one or more of the associated listed items. Expressions such as “at least one of…” modify the entire list of elements when following a list of elements, without modifying any individual element in that list.

[0034] Since the inventive concept described below can be modified and has various embodiments, specific embodiments are shown in the accompanying drawings and described in detail in the detailed description. However, this is not intended to limit the inventive concept to the specific embodiments, and it should be understood to include all modifications, equivalents, or substitutions included within the technical scope of the inventive concept.

[0035] The terminology used below is for describing specific embodiments only and is not intended to limit the inventive concept. Unless the context clearly indicates otherwise, singular expressions include plural expressions. It will also be understood below that when the terms “comprising,” “including,” or “having” are used in this specification, it indicates the presence of the stated features, integers, steps, operations, elements, and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups thereof. Depending on the context, the “ / ” used below may be interpreted as “and” or “or.”

[0036] In the accompanying drawings, thicknesses have been enlarged or reduced for clarity of the various layers and regions. Throughout the specification, the same reference numerals denote the same components. Throughout the specification, when references are made to an component such as a layer, film, region, or plate being placed "on" another component, it will be understood that the component may be directly on said other component, or another component may be placed therebetween. Throughout the specification, although the terms "first," "second," "third," etc., may be used herein to describe various elements, components, regions, and / or layers, these elements, components, regions, and / or layers should not be limited by these terms. These terms are used only to distinguish one component from another.

[0037] The term "particle size" as used herein refers to the average diameter when the particle is spherical, or the average major axis length when the particle is non-spherical. Particle size can be measured using a particle size analyzer (PSA). The "particle size" can be, for example, the average particle size. Unless otherwise explicitly stated, the average particle size is the median particle size (D50). The median particle size (D50) refers to the particle size corresponding to 50% of the cumulative value calculated from the side with the smallest particle size on a cumulative distribution curve of particle sizes, where particles accumulate in order of particle size from smallest to largest. The cumulative value can be, for example, the cumulative volume. The median particle size (D50) can be measured by, for example, laser diffraction.

[0038] The term “particle size D10” as used here refers to the particle size corresponding to 10% of the cumulative value calculated from the side with the smallest particle size on the cumulative distribution curve of particle size.

[0039] As used herein, the term "particle size D90" refers to the particle size corresponding to a cumulative value of 90% calculated from the side of particles having the smallest particle size on the cumulative distribution curve of particle sizes.

[0040] As used herein, the term "silicon suboxide" may have, for example, a single composition represented by SiO x (0<x<2). Alternatively, "silicon suboxide" may include, for example, at least one selected from Si and SiO₂ to have a SiO x (0<x<2) average composition. Alternatively, "silicon suboxide" may further include, for example, silicon suboxide-based materials. The silicon suboxide-based material is a material having properties similar to those of silicon suboxide, and may include, for example, at least one selected from Si and SiO₂ to have a SiO x (0<x<2) average composition.

[0041] Hereinafter, a composite negative active material according to an embodiment, a negative electrode including the composite negative active material, and a lithium battery including the negative electrode will be described in more detail.

[0042] The composite negative active material includes: a core; and a shell disposed on a surface of the core and conformal with the surface of the core, wherein the core may include a silicon-containing structure, a silicon-containing compound, or a combination thereof, and the shell includes at least one first metal oxide represented by Formula M a O b (0<a≤3, 0<b<4, and when a is 1, 2, or 3, b is not an integer) and a first carbonaceous material, the first metal oxide is disposed in the first carbonaceous material, and M is at least one metal selected from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements. Referring to Figure 1 , the composite negative active material 100 includes a core 10 and a shell 20 positioned continuously or discontinuously along the surface of the core 10. The shell 20 may cover all or part of the core 10. The core 10 may include a silicon-containing negative active material (such as a silicon-containing structure, a silicon-containing compound, or a combination thereof), and the shell 20 may include a first metal oxide 21 and a first carbonaceous material 22.

[0043] Hereinafter, the theoretical basis for providing the excellent effects of the composite negative active material according to the embodiment will be described, but this is to help understand the inventive concept, and is not intended to limit the inventive concept in any way.

[0044] The composite negative electrode active material includes a matrix of a first carbonaceous material, and by using a composite comprising a plurality of first metal oxides located inside the matrix, a uniform shell can be positioned on the core while preventing agglomeration of the first carbonaceous material. Accordingly, contact between the core and the electrolyte is effectively blocked, thereby effectively preventing side reactions caused by the contact between the core and the electrolyte. The first carbonaceous material may be, for example, a crystalline carbonaceous material. The first carbonaceous material may be, for example, a carbonaceous nanostructure. The first carbonaceous material may be, for example, a carbonaceous two-dimensional nanostructure. The first carbonaceous material may be, for example, a carbonaceous flake. The first carbonaceous material may be, for example, graphene. Since the shell comprising graphene and / or its matrix has flexibility, it can easily accommodate volume changes in the core during charging and discharging. Therefore, since cracks occurring on the surface and / or inside the composite negative electrode active material during charging and discharging can be suppressed, the formation of a solid electrolyte interphase (SEI) film on the surface and / or inside the composite negative electrode active material can be suppressed. As a result, deterioration of the lithium battery including the composite negative electrode active material is inhibited. In contrast, in the case of a silicon-based negative electrode active material in the related art, cracks generally occur on the surface and / or inside the silicon-based negative electrode active material due to volume changes during charging and discharging. New surfaces are generated inside and / or outside the silicon-based negative electrode active material through the cracks. On these new surfaces, a solid electrolyte interphase (SEI) film is formed through a side reaction between the silicon-based negative electrode active material and the electrolyte. As charging and discharging proceed, the continuous formation of the solid electrolyte interphase (SEI) film increases the internal resistance of the silicon-based negative electrode active material, thus degrading the performance of the lithium battery. In addition, the carbonaceous materials of the related art are prone to agglomeration during the coating process, making it difficult to uniformly coat the core.

[0045] The core of the composite negative electrode active material includes a silicon-containing negative electrode active material, such as a silicon-containing structure, a silicon-containing compound, or a combination thereof. The silicon-containing structure may include, for example, a silicon composite structure. The silicon composite structure may be, for example, a silicon-carbon composite. The silicon-carbon composite may be, for example, a silicon-carbon nanocomposite. The silicon-carbon nanocomposite refers to a composite in which at least one of silicon and carbon has a nanoscale size of less than 1 μm. For example, the silicon-carbon nanocomposite may be a composite in which silicon nanoparticles and carbon nanoparticles are composited. The silicon-containing compound may include, for example, silicon, a silicon alloy, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or a combination thereof. The silicon-containing compound may include, for example, SiO x (0<x<2).

[0046] The silicon composite structure may include, for example, porous silicon secondary particles and first carbon flakes located on the porous silicon secondary particles, wherein the porous silicon secondary particles are aggregates of a plurality of silicon composite primary particles, and the silicon composite primary particles include: silicon; silicon suboxide (SiO x , 0<x<2), located on the silicon; and second carbon flakes, located on the silicon suboxide.

[0047] The silicon composite structure may include porous silicon secondary particles which are aggregates comprising a plurality of silicon composite primary particles, and first carbon flakes disposed on the porous silicon secondary particles. In addition, the first carbon flakes on the porous silicon secondary particles may be positioned to cover at least a portion of the surfaces of the porous silicon secondary particles. The first carbon flakes may be directly deposited on the porous silicon secondary particles. The first carbon flakes may be directly grown on the silicon suboxide of the porous silicon secondary particles. The first carbon flakes may be directly grown on the surfaces of the porous silicon secondary particles to be directly located on the surfaces of the porous silicon secondary particles. The first carbon flakes may completely cover the surfaces of the porous silicon secondary particles, or may cover a portion thereof. Based on the total surface area of the porous silicon secondary particles, the coverage rate of the first carbon flakes may be, for example, 5% to 100%, 10% to 99%, 20% to 95%, or 40% to 90%. The carbon of the first carbon flakes exists on the surfaces of the porous silicon secondary particles, and effectively buffers the volume change of the porous silicon secondary particles. The size of the porous silicon secondary particles may be, for example, about 1 μm to about 20 μm, about 2 μm to about 18 μm, or about 3 μm to about 10 μm. The size of the first carbon flakes may be, for example, about 1 nm to about 200 nm, about 5 nm to about 150 nm, or about 10 nm to about 100 nm. The term "size" as used herein refers to the diameter or major axis length.

[0048] The silicon composite primary particles include silicon, silicon suboxide (SiO x , 0<x<2) disposed on at least a portion of the surface of the silicon, and second carbon flakes disposed on one side of the silicon suboxide. The silicon may be, for example, plate-shaped, needle-shaped, spherical, or a combination thereof. The shape of the silicon is not particularly limited, and may be, for example, in the shape of a sphere, nanowire, needle, rod, particle, nanotube, nanorod, wafer, and nanobelt, or a combination thereof. The average size of the silicon may be, for example, about 10 nm to about 1 μm, about 10 nm to about 500 nm, about 20 nm to about 150 nm, or 100 nm. Regarding the average size of the silicon, when the silicon is a spherical particle, the average size is the average particle diameter, and when the silicon is a non-spherical particle (for example, a plate-shaped particle or a needle-shaped particle), the average size is the major axis length, length, or thickness. The silicon suboxide (SiO on the silicon in the silicon composite primary particles x, 0<x<2) can cover at least a part of the surface of silicon. Silicon monoxide may be directly on silicon. Silicon monoxide may completely cover the surface of silicon or may cover a part of the surface of silicon. Based on the total surface area of silicon, the coverage rate of silicon monoxide may be, for example, from about 1% to about 100%, from about 5% to about 99%, from about 10% to about 95%, or from about 20% to about 90%. The second carbon flakes located on the silicon monoxide may be positioned to cover at least a part of the surface of the silicon monoxide. The second carbon flakes may be directly on the silicon monoxide. The second carbon flakes may grow directly from the surface of the silicon monoxide and be directly on the surface of the silicon monoxide. In an embodiment, the second carbon flakes may completely cover the surface of the silicon monoxide or may cover a part of the surface of the silicon monoxide. Based on the total surface area of the silicon monoxide, the coverage rate of the second carbon flakes may be, for example, about 10% to about 100%, about 10% to about 99%, about 20% to about 95%, or about 40% to about 90%. Carbon of the second carbon flakes is present on the surface of silicon and / or silicon monoxide, and can effectively buffer the volume change of the silicon composite primary particles. The size of the second carbon flakes may be, for example, about 1 nm to about 200 nm, about 5 nm to about 150 nm, or about 10 nm to about 100 nm. As used herein, the term "size" refers to the diameter or the length of the major axis.

[0049] The silicon composite structure includes porous silicon secondary particles and first carbon flakes located on the porous silicon secondary particles. The first carbon flakes may completely cover the porous silicon secondary particles or may cover a part of the porous silicon secondary particles. For example, the first carbon flakes may completely surround the porous silicon secondary particles or may surround a part of the porous silicon secondary particles. The silicon composite structure includes second carbon flakes located on the silicon composite primary particles included in the porous silicon secondary particles. During the volume expansion / contraction of the silicon composite structure, the silicon included in the porous silicon secondary particles may remain in contact with the first carbon flakes and / or the second carbon flakes. Since the porous silicon secondary particles include pores, the pores may serve as an internal buffer space during the volume expansion / contraction of the silicon composite structure. Therefore, unlike the silicon-based negative electrode active materials of the prior art, the silicon composite structure can suppress an increase in internal resistance while effectively accommodating the volume change of the silicon composite structure during charging and discharging.

[0050] The porosity of the silicon composite structure may be, for example, 60% or less, 30% to 60%. Alternatively, the silicon composite structure may be non-porous. The non-porous structure may have a porosity of, for example, 10% or less, or 5% or less. The non-porous structure may have a porosity of, for example, 0.01% to 5% or 0%. The porosity may be measured by a mercury intrusion method (porosimetry) or a nitrogen adsorption method.

[0051] Silicon composite structures can have, for example, non-spherical shapes. The circularity of a silicon composite structure can be, for example, 0.9 or less. The circularity of a silicon composite structure can be, for example, 0.7 to 0.9, 0.8 to 0.9, or 0.85 to 0.9. Circularity is, for example, 4πA / P. 2 (A is the area, P is the perimeter) Determine.

[0052] Silicon composite structures may include a first carbon sheet and a second carbon sheet. The first and second carbon sheets may be, for example, identical carbon sheets. The first and second carbon sheets may be any carbonaceous material having a sheet shape. The first and second carbon sheets may each independently be graphene, graphite, carbon fiber, graphitic carbon, graphene oxide, or mixtures thereof. Silicon composite structures may include, for example, a first graphene and a second graphene, respectively serving as the first and second carbon sheets. Both the first and second graphene may have structures such as nanosheets, films (or thin films), or sheets. Nanosheets refer to those irregularly formed on sub-silicon oxide or porous silicon secondary particles, having a thickness of about 1000 nm or less (e.g., 1 nm to 1000 nm). Films refer to those continuously and uniformly formed on sub-silicon oxide or porous silicon secondary particles.

[0053] The silicon-containing structure may also include a carbonaceous coating on the silicon composite structure. The carbonaceous coating can improve the physical stability of the silicon composite structure and more effectively prevent side reactions between silicon and the electrolyte during charging and discharging. The carbonaceous coating may include, for example, a first amorphous carbon. The carbonaceous coating may include a first amorphous carbon with a high density. The first amorphous carbon may include, for example, pitch carbon, soft carbon, hard carbon, mesophase pitch carbides, calcined coke, carbon fibers, or mixtures thereof. The carbonaceous coating may also include crystalline carbon. By further including crystalline carbon, the carbonaceous coating can more effectively act as a buffer against volume changes in the silicon composite structure. The crystalline carbon may be, for example, natural graphite, artificial graphite, graphene, fullerene, carbon nanotubes, or mixtures thereof. The thickness of the carbonaceous coating may be, for example, about 1 nm to about 5000 nm, about 10 nm to about 2000 nm, or about 5 nm to about 2500 nm.

[0054] The silicon-containing structure may also include, for example, a second amorphous carbon located within the silicon composite structure. For instance, the silicon composite structure may include porous silicon secondary particles, and the second amorphous carbon may be located within the pores of the porous silicon secondary particles. The second amorphous carbon may be located between multiple silicon composite primary particles constituting the porous silicon secondary particles. The silicon composite primary particles may include, for example, silicon, or silicon suboxide (SiO2) located on silicon. x, 0<x<2), a second carbon flake disposed on the silicon monoxide, and a second amorphous carbon disposed on the second carbon flake. Since pores are filled with the dense second amorphous carbon in the silicon composite structure, the silicon composite structure may have a dense structure that is a pore-free structure. As the silicon composite structure has such a pore-free structure, side reactions with an electrolyte during charging and discharging may be further reduced, and volume change of the silicon composite structure may be more effectively reduced. The second amorphous carbon may include, for example, pitch carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, carbon fiber, or a mixture thereof.

[0055] In the silicon composite structure, a mixing ratio of the total weight of the first carbon, which is the sum of the carbon of the first carbon flake and the carbon of the second carbon flake, to the weight of the second carbon, which is the carbon of the carbonaceous coating, may be, for example, 30:1 to 1:3, 20:1 to 1:1, or 10:1 to 1:0.9. When the first carbon and the second carbon have a mixing ratio within these ranges, a lithium battery having improved cycle characteristics may be provided. The mixing ratio of the first carbon to the second carbon may be confirmed by thermogravimetric analysis. The first carbon is related to a peak appearing in a region of 700°C to 750°C, and the second carbon is related to a peak appearing in a region of 600°C to 650°C. The thermogravimetric analysis may be performed under conditions including, for example, a heating rate of about 10°C / min and an air atmosphere from 25°C to 1000°C. The first carbon may be, for example, crystalline carbon, and the second carbon may be, for example, amorphous carbon. The mixing ratio of the total weight of the carbon of the first carbon flake and the carbon of the second carbon flake to the total weight of the first amorphous carbon and the second amorphous carbon may be, for example, 1:99 to 99:1, 1:20 to 80:1, or 1:1 to 1:10.

[0056] The core is a negative active material including silicon, and may include the silicon-including compound SiO x (0<x<2). SiO x The average particle diameter of (0<x<2) may be, for example, 1 μm or greater, 3 μm or greater, or 5 μm or greater. SiO x The average particle diameter of (0<x<2) may be, for example, about 1 μm to about 30 μm, about 3 μm to about 20 μm, or about 5 μm to about 15 μm.

[0057] The shell may include a first metal oxide and a first carbonaceous material.

[0058] Because the first carbonaceous material (e.g., graphene) has high electronic conductivity, the interfacial resistance between the composite negative electrode active material and the electrolyte can be reduced. Therefore, despite the introduction of a shell including the first carbonaceous material, the increase in the internal resistance of the lithium battery is suppressed. Since the first carbonaceous material included in the shell of the composite negative electrode active material is derived from a graphene matrix, it has a relatively low density and high porosity compared to carbonaceous materials derived from graphite-based materials in related technologies. The d002 interplanar spacing of the first carbonaceous material included in the shell of the composite negative electrode active material can be, for example... or larger or larger or larger or larger or larger or larger or Or larger. The d002 interplanar spacing of the first carbonaceous material included in the shell of the composite negative electrode active material can be, for example, approximately to approximately about to approximately about to approximately about to approximately or about to approximately On the other hand, the d002 interplanar spacing of the related technology derived from graphite-based carbonaceous materials can be, for example... or smaller or to Because the first metal oxide has voltage resistance, core degradation can be prevented during charging and discharging at high voltages. The casing may include, for example, one first metal oxide or two or more different first metal oxides. As a result, the cycle characteristics of lithium batteries including composite negative electrode active materials are improved, and their volume changes can be suppressed.

[0059] The amount of the shell can be from about 0.1 wt% to about 5 wt%, from about 0.1 wt% to about 4 wt%, from about 0.1 wt% to about 3 wt%, or from about 0.1 wt% to about 2 wt% of the total weight of the composite negative electrode active material. The amount of the first metal oxide can be, for example, from about 0.06 wt% to about 3 wt%, from about 0.06 wt% to about 2.4 wt%, from about 0.06 wt% to about 1.8 wt%, or from about 0.06 wt% to about 1.2 wt% of the total weight of the composite negative electrode active material. Since the composite negative electrode active material includes the shell and the first metal oxide in these ranges, the cycle characteristics of the lithium battery are further improved.

[0060] The shell includes a first metal, and based on the total number of atoms in the shell, the amount of the first metal can be, for example, from about 0.1 at% to about 10 at%, from about 0.5 at% to about 7 at%, or from about 1 at% to about 5 at%. When the shell includes a first metal in these ranges, the cycle characteristics of the lithium battery including the composite negative electrode active material can be further improved. The amount of the first metal element included in the shell can be obtained, for example, by measuring peaks in the XPS spectrum of the surface of the composite negative electrode active material. The first metal can be a metal included in a first metal oxide.

[0061] The shell may include oxygen (O), and based on the total number of atoms in the shell, the amount of oxygen (O) may be, for example, about 6 at% to about 20 at%, about 7 at% to about 15 at%, about 8 at% to about 15 at%, or about 10 at% to about 15 at%. When the shell includes oxygen in these ranges, the cycle characteristics of the lithium battery including the composite negative electrode active material can be further improved. The amount of oxygen (O) included in the shell can be obtained, for example, by measuring peaks in the XPS spectrum of the surface of the composite negative electrode active material.

[0062] The casing may include aluminum (Al) as a first metal, and the amount of aluminum (Al) may be, for example, about 0.1 at% to about 10 at%, about 0.5 at% to about 10 at%, about 1 at% to about 9 at%, about 1 at% to about 7 at%, or about 1 at% to about 5 at%, depending on the total number of atoms in the casing. When the casing includes aluminum in these ranges, the cycle characteristics of the lithium battery including the composite negative electrode active material can be further improved. The amount of aluminum (Al) included in the casing can be obtained, for example, by measuring peaks in the XPS spectrum of the surface of the composite negative electrode active material.

[0063] The shell comprises carbon (C), and based on the total number of atoms in the shell, the amount of carbon (C) can be, for example, about 70 at% to about 95 at%, about 70 at% to about 90 at%, about 75 at% to about 90 at%, about 80 at% to about 90 at%, about 80 at% to about 87 at%, or about 80 at% to about 85 at%. When the shell comprises carbon in these ranges, the cycle characteristics of the lithium battery comprising the composite negative electrode active material can be further improved. The amount of carbon included in the shell can be obtained, for example, by measuring peaks in the XPS spectrum of the surface of the composite negative electrode active material.

[0064] The first metal oxide may include a first metal, and the first metal may be at least one selected from, for example, Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide may be, for example, selected from Al₂O₃. z (0 <z<3)、NbO x(0<x<2.5), MgO x (0<x<1), Sc2O z (0<z<3), TiO y (0<y<2), ZrO y (0<y<2), V2O z (0<z<3), WO y (0<y<2), MnO y (0<y<2), Fe2O z (0<z<3), Co3O w (0<w<4), PdO x (0<x<1), CuO x (0<x<1), AgO x (0<x<1), ZnO x (0<x<1), Sb2O z (0<z<3) and SeO y at least one of (0<y<2). Since such a first metal oxide is disposed in the matrix of the carbonaceous material, the uniformity of the shell disposed on the core is improved, and the voltage resistance of the composite negative active material can be further improved. For example, the shell comprises Al2O x (0<x<3) as the first metal oxide.

[0065] The shell may further comprise at least one second metal oxide represented by M a O c (0<a≤3, 0<c≤4, when a is 1, 2 or 3, c is an integer). M is at least one metal selected from Groups 2 to 13, Group 15 and Group 16 of the Periodic Table of the Elements. For example, the second metal oxide includes the same metal as the metal of the first metal oxide, and the ratio c / a of c to a in the second metal oxide is greater than the ratio b / a of b to a in the first metal oxide. For example, c / a>b / a. The second metal oxide is selected from Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3 and SeO2. The first metal oxide may be, for example, a reduction product of the second metal oxide. The first metal oxide is obtained by reducing part or all of the second metal oxide. Therefore, compared with the second metal oxide, the first metal oxide has a lower oxygen content and a lower metal oxidation number. For example, the shell comprises Al2O as the first metal oxide x (0<x<3) and Al2O3 as the second metal oxide.

[0066] The shell may include at least one selected from a first metal oxide and a second metal oxide. The particle size of one or more of the first and second metal oxides may be, for example, about 1 nm to about 100 nm, about 1 nm to about 50 nm, about 1 nm to about 30 nm, about 5 nm to about 30 nm, or about 10 nm to about 30 nm. Within these nanometer-range particle sizes, the first metal oxide and / or the second metal oxide can be more uniformly distributed in the matrix of the first carbonaceous material of the shell. When the particle size of at least one of the first and second metal oxides increases excessively, the internal resistance of the composite negative electrode active material increases due to the increase in shell thickness. When the particle size of at least one of the first and second metal oxides decreases excessively, uniform dispersion becomes difficult.

[0067] The shell may include a first metal oxide and / or a second metal oxide, and may include a first carbonaceous material. The first carbonaceous material may be located in a direction protruding from the surface of the first metal oxide and / or the second metal oxide. Since the first carbonaceous material grows directly from the surface of the first metal oxide and / or the second metal oxide, it can be located in a direction protruding from the surface of the first metal oxide and / or the second metal oxide. The first carbonaceous material located in the direction protruding from the surface of the first metal oxide and / or the second metal oxide may be, for example, a two-dimensional carbonaceous nanostructure, a carbonaceous sheet, or graphene.

[0068] The shell may include, for example, a first carbonaceous material, and the core may include, for example, a silicon-containing structure and / or a silicon-containing compound as a silicon-containing negative electrode active material. For example, the first carbonaceous material can be formed into a composite through a mechanochemical reaction with a silicon-containing structure and / or a silicon-containing compound. The first carbonaceous material can be chemically bonded to, for example, a silicon-containing structure and / or a silicon-containing compound. The core and shell can be formed into a composite by chemically bonding the first carbonaceous material in the shell to the silicon-containing structure and / or a silicon-containing compound in the core. Therefore, the composite negative electrode active material is different from a simple physical mixture of the first carbonaceous material and a silicon-containing structure and / or a silicon-containing compound. The first metal oxide and the first carbonaceous material included in the shell can also be chemically bonded to each other. Here, the chemical bond can be, for example, a covalent bond or an ionic bond.

[0069] The shell thickness can be, for example, from about 1 nm to about 5 μm, from about 1 nm to about 1 μm, from about 1 nm to about 500 nm, from about 1 nm to about 200 nm, from about 1 nm to about 100 nm, from about 1 nm to about 50 nm, from about 1 nm to about 30 nm, or from about 1 nm to about 20 nm. When the shell has a thickness within these ranges, the electronic conductivity of the negative electrode, including the composite negative electrode active material, can be further improved.

[0070] The shell, located on and conforming to the surface of the core, may comprise at least one of the following materials: a composite comprising a first metal oxide and a first carbonaceous material (e.g., graphene); and the result of grinding the composite. The first metal oxide may be located within a matrix of the first carbonaceous material (e.g., a graphene matrix). The shell may be made from, for example, a composite comprising a first metal oxide and a first carbonaceous material (e.g., graphene). In addition to the first metal oxide, the composite may also comprise a second metal oxide. The composite may comprise, for example, two or more first metal oxides. The composite may comprise, for example, two or more first metal oxides and two or more second metal oxides.

[0071] The amount of at least one of the composite and its milled derivatives may be 5 wt% or less, 3 wt% or less, 2 wt% or less, 1 wt% or less, or 0.5 wt% or less of the total weight of the composite negative electrode active material. The amount of at least one of the composite and its milled derivatives included in the composite negative electrode active material may be, for example, about 0.1 wt% to about 5 wt%, about 0.1 wt% to about 4 wt%, about 0.1 wt% to about 3 wt%, or about 0.1 wt% to about 2 wt% of the total weight of the composite negative electrode active material. When the composite negative electrode active material includes at least one of the composite and its milled derivatives within these ranges, the cycle characteristics of the lithium battery including the composite negative electrode active material can be further improved.

[0072] The composite may include at least one selected from a first metal oxide and a second metal oxide. The particle size of one or more of the first and second metal oxides may be, for example, about 1 nm to about 100 nm, about 1 nm to about 50 nm, about 1 nm to about 30 nm, about 5 nm to about 30 nm, or about 10 nm to about 30 nm. Within these nanometer-range particle sizes, the first metal oxide and / or the second metal oxide can be more uniformly distributed in the matrix of the first carbonaceous material of the composite. Therefore, such a composite can be uniformly applied to the core to form a shell. Furthermore, because the first metal oxide and / or the second metal oxide have particle sizes within these nanometer ranges, they can be more uniformly located on the core. Therefore, the first metal oxide and / or the second metal oxide can be uniformly located on the core, thereby more effectively exhibiting voltage withstand properties. The average particle size of the first and second metal oxides is measured using a measuring device employing a laser diffraction method or a dynamic light scattering method. The particle sizes of the first and second metal oxides are measured using a scattering particle size analyzer (e.g., Horiba LA-920), and are the median particle size (D50) values ​​when the metal oxide particles accumulate to 50% in volume conversion from the smaller particles. The uniformity deviation of at least one of the first and second metal oxides can be 3% or less, 2% or less, or 1% or less. Uniformity can be obtained, for example, by XPS. Therefore, at least one of the first and second metal oxides can have a uniformity deviation of 3% or less, 2% or less, or 1% or less, and can be uniformly distributed in the composite.

[0073] The composite may include a first carbonaceous material. The first carbonaceous material may have, for example, a branched structure, and at least one metal oxide selected from a first metal oxide and a second metal oxide may be distributed within the branched structure of the first carbonaceous material. The branched structure of the first carbonaceous material includes, for example, multiple particles of the first carbonaceous material in contact with each other. Because the first carbonaceous material has a branched structure, various conductive paths can be provided. The first carbonaceous material may be, for example, graphene. Graphene may have, for example, a branched structure, and at least one metal oxide selected from a first metal oxide and a second metal oxide may be distributed within the branched structure of the graphene. The branched structure of the graphene includes multiple graphene particles in contact with each other. Because the graphene has a branched structure, various conductive paths can be provided.

[0074] The first carbonaceous material may have, for example, a spherical structure, and at least one metal oxide selected from a first metal oxide and a second metal oxide may be distributed within the spherical structure of the first carbonaceous material. The size of the spherical structure of the first carbonaceous material may be from about 50 nm to about 300 nm. Multiple first carbonaceous materials with spherical structures may be present. Because the first carbonaceous material has a spherical structure, the composite may have a rigid structure. The first carbonaceous material may be, for example, graphene. Graphene may have, for example, a spherical structure, and at least one metal oxide selected from a first metal oxide and a second metal oxide may be distributed within the spherical structure of the graphene. The spherical structure of the graphene may have a size from about 50 nm to 300 nm. Multiple graphenes with spherical structures may be provided. Because graphene has a spherical structure, the composite may have a robust structure.

[0075] The first carbonaceous material can have a helical structure with multiple spherical structures interconnected, and at least one metal oxide selected from a first metal oxide and a second metal oxide can be distributed within the spherical structures of the helical structure. The size of the helical structure of the first carbonaceous material can be from about 500 nm to about 100 μm. Because the first carbonaceous material has a helical structure, the composite can have a rigid structure. The first carbonaceous material can be, for example, graphene. Graphene can have a helical structure with multiple spherical structures interconnected, and at least one metal oxide selected from a first metal oxide and a second metal oxide can be distributed within the spherical structures of the helical structure. The helical structure of graphene can have a size from about 500 nm to 100 μm. Because graphene has a helical structure, the composite can have a robust structure.

[0076] The first carbonaceous material can have a cluster structure of multiple spherical structures, and at least one metal oxide selected from a first metal oxide and a second metal oxide can be distributed within the spherical structures of the cluster structure. The size of the cluster structure of the first carbonaceous material can be from about 0.5 mm to about 10 mm. Because the first carbonaceous material has a cluster structure, the composite can have a rigid structure. The first carbonaceous material can be, for example, graphene. Graphene can have a cluster structure of multiple spherical structures, and at least one metal oxide selected from a first metal oxide and a second metal oxide can be distributed within the spherical structures of the cluster structure. The cluster structure of graphene can have a size of about 0.5 mm to 10 mm. Because graphene has a cluster structure, the composite can have a robust structure.

[0077] The composite can be a wrinkled faceted-ball structure, and at least one of a first metal oxide and a second metal oxide can be distributed within or on the surface of the structure. Because the composite is such a faceted-ball structure, it can be readily applied to the irregular surface of the core.

[0078] The complex can be, for example, a planar structure, and at least one selected from a first metal oxide and a second metal oxide can be distributed within or on the surface of the planar structure. Because the complex is such a two-dimensional planar structure, it can be readily applied to the irregular surface of the core.

[0079] The first carbonaceous material may extend from the first metal oxide by a distance of 10 nm or less, and may comprise at least one to 20 layers of the first carbonaceous material. For example, due to the stacking of multiple layers of the first carbonaceous material, a first carbonaceous material having a total thickness of 12 nm or less may be located on the first metal oxide. For example, the total thickness of the carbonaceous material may be from about 0.6 nm to about 12 nm. The first carbonaceous material may be, for example, graphene. Graphene may extend from the first metal oxide by a distance of 10 nm or less, and may comprise at least one to 20 graphene layers. For example, due to the stacking of multiple graphene layers, graphene having a total thickness of 12 nm or less may be disposed on the first metal oxide. For example, the total thickness of the graphene may be from about 0.6 nm to about 12 nm.

[0080] The shell may also include a second carbonaceous material, which is fibrous carbon. The second carbonaceous material may include fibrous carbon.

[0081] When the shell also includes a second carbonaceous material, which is fibrous carbon, the conductive path of the composite negative electrode active material can be further extended. The second carbonaceous material can form a three-dimensional conductive network among multiple composite negative electrode active materials, thereby reducing the internal resistance of the negative electrode including the composite negative electrode active materials. Since the fibrous carbon is fixed on the composite negative electrode active material, a uniform and stable three-dimensional conductive network can be formed among multiple composite negative electrode active materials. Therefore, the high-rate characteristics of lithium batteries including composite negative electrode active materials containing the second carbonaceous material can be improved. (Refer to...) Figure 5The composite negative electrode active material 100 includes a core 10 and a shell 20 located on and conformally to the surface of the core 10. The core 10 may include a silicon-containing structure, a silicon-containing compound, or a combination thereof, and the shell 20 may include a first metal oxide 21, a first carbonaceous material 22, and a second carbonaceous material 23. The second carbonaceous material 23 may include, for example, fibrous carbon having an aspect ratio of 10 or greater. Conversely, in the case of a simple mixture of core and fibrous carbon, it is difficult to form a uniform three-dimensional conductive network between multiple core particles due to the aggregation of fibrous carbon, etc. Since the second carbonaceous material 23 is located within the matrix of the first carbonaceous material 22, the second carbonaceous material 23 can be easily coated onto the core 10. The matrix of the first carbonaceous material 22 can act as a binder for bonding the core 10 and the second carbonaceous material 23. Therefore, when the first carbonaceous material 22 is absent, the second carbonaceous material 23 is difficult to easily adhere to the core 10 or will easily detach from the core 10 during the slurry manufacturing process. When a binder is added to bond the core 10 and the second carbonaceous material 23, the internal resistance of the composite negative electrode active material 100 increases because the core 10 is covered by the insulating binder. When the second carbonaceous material 23 and the binder-coated core 10 undergo high-temperature heat treatment to carbonize the binder, the core 10 and the second carbonaceous material 23 will deteriorate during the heat treatment process.

[0082] The aspect ratio of the second carbonaceous material can be 10 or greater, or 20 or greater. The aspect ratio of the second carbonaceous material can be, for example, about 10 to about 100,000, about 10 to about 80,000, about 10 to about 50,000, about 10 to about 10,000, about 10 to about 5,000, about 10 to about 1,000, about 10 to about 500, about 10 to about 100, or about 10 to about 50. The aspect ratio of the second carbonaceous material can be, for example, the ratio of the length of the major axis passing through the center of the second carbonaceous material to the length of the minor axis passing through the center of the second carbonaceous material and perpendicular to the major axis (i.e., the diameter of the second carbonaceous material).

[0083] The diameter of the second carbonaceous material can be, for example, 50 nm or less, 30 nm or less, 20 nm or less, or 10 nm or less. The diameter of the second carbonaceous material can also range from, for example, about 1 nm to about 50 nm, from about 1 nm to about 30 nm, or from about 1 nm to about 10 nm. When the diameter of the second carbonaceous material is too large, the absolute number of chains per volume decreases, thus the effect of reducing internal resistance is not significant. When the diameter of the second carbonaceous material is too small, it becomes difficult to disperse uniformly.

[0084] The length of the second carbonaceous material can be, for example, 1000 μm or less, 100 μm or less, 50 μm or less, 10 μm or less, 5 μm or less, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the second carbonaceous material can also be, for example, about 100 nm to about 1000 μm, about 100 nm to about 500 μm, about 100 nm to about 100 μm, about 100 nm to about 50 μm, about 100 nm to about 10 μm, about 100 nm to about 5 μm, about 100 nm to about 2 μm, about 100 nm to about 1 μm, about 100 nm to about 500 nm, or about 100 nm to about 300 nm. The length of the second carbonaceous material can be, for example, about 500 nm to about 1000 μm, about 500 nm to about 500 μm, about 500 nm to about 100 μm, about 500 nm to about 50 μm, about 500 nm to about 10 μm, about 500 nm to about 5 μm, or about 500 nm to about 2 μm. As the length of the second carbonaceous material increases, the internal resistance of the electrode can decrease. When the length of the second carbonaceous material is too short, it will be difficult to provide an effective conductive path.

[0085] The second carbonaceous material may include, for example, carbon nanofibers, carbon nanotubes, or combinations thereof.

[0086] Carbon nanotubes can include, for example, primary carbon nanotube structures, secondary carbon nanotube structures formed by the aggregation of multiple primary carbon nanotube structures, or combinations thereof.

[0087] The primary structure of a carbon nanotube is a single carbon nanotube unit. This unit is a cylindrical graphite sheet with a diameter of nanometers and an sp2 bond structure. Depending on the curvature and structure of the graphite surface, it can exhibit conductive or semiconductor properties. Based on the number of bonds forming the walls, carbon nanotube units can be classified as single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWCNTs), and multi-walled carbon nanotubes (MWCNs). The thinner the wall thickness of the carbon nanotube unit, the lower its electrical resistance.

[0088] Carbon nanotube units can be classified as single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWCNTs), multi-walled carbon nanotubes (MWCNs), or combinations thereof. The diameter of the primary structure of a carbon nanotube can be, for example, 1 nm or greater, or 2 nm or greater. The diameter of the primary structure of a carbon nanotube can be, for example, 20 nm or less, or 10 nm or less. The diameter of the primary structure of a carbon nanotube can be, for example, about 1 nm to about 20 nm, about 1 nm to about 15 nm, or about 2 nm to about 10 nm. The length of the primary structure of a carbon nanotube can be, for example, 100 nm or greater, or 200 nm or greater. The length of the primary structure of a carbon nanotube can be, for example, 2 μm or less, 1 μm or less, 500 nm or less, or 300 nm or less. The length of the primary structure of a carbon nanotube can be, for example, about 100 nm to about 2 μm, about 100 nm to about 1 μm, about 100 nm to about 500 nm, about 100 nm to about 400 nm, about 100 nm to about 300 nm, or about 200 nm to about 300 nm. The diameter and length of the primary structure of carbon nanotubes can be measured from scanning electron microscopy (SEM) images. Alternatively, the diameter and / or length of the primary structure of carbon nanotubes can be measured by laser diffraction.

[0089] Carbon nanotube secondary structures are structures formed by assembling primary carbon nanotube structures to integrally or partially form bundle-type or rope-type carbon nanotubes. Carbon nanotube secondary structures can include, for example, bundle-type carbon nanotubes, rope-type carbon nanotubes, or combinations thereof. The diameter of the carbon nanotube secondary structure can be, for example, 2 nm or greater, or 3 nm or greater. The diameter of the carbon nanotube secondary structure can be, for example, 50 nm or less, 30 nm or less, or 10 nm or less. The diameter of the carbon nanotube secondary structure can be, for example, about 2 nm to about 50 nm, about 2 nm to about 30 nm, or about 2 nm to about 20 nm. The length of the carbon nanotube secondary structure can be, for example, 500 nm or greater, 700 nm or greater, 1 μm or greater, or 10 μm or greater. The length of the carbon nanotube secondary structure can be, for example, 1000 μm or less, 500 μm or less, or 100 μm or less. The length of the carbon nanotube secondary structure can be, for example, about 500 nm to about 1000 μm, about 500 nm to about 500 μm, about 500 nm to about 200 μm, about 500 nm to about 100 μm, or about 500 nm to about 50 μm. The diameter and length of the carbon nanotube secondary structure can be measured from SEM images or optical microscope images. Optionally, the diameter and / or length of the carbon nanotube secondary structure can be measured by laser diffraction. In the embodiments, the carbon nanotube secondary structure can be used to prepare composite anode active materials after being converted into a carbon nanotube primary structure by dispersion in a solvent or the like.

[0090] Based on the total weight of the first and second carbonaceous materials, the amount of the second carbonaceous material can be, for example, from about 0.1 wt% to about 50 wt%, from about 1 wt% to about 40 wt%, or from about 5 wt% to about 30 wt%. Since the composite negative electrode active material includes these ranges of first and second carbonaceous materials, a conductive path is more effectively ensured within the composite negative electrode active material, allowing for a further reduction in the internal resistance of the composite negative electrode active material. As a result, the cycle characteristics of the lithium battery including the composite negative electrode active material can be further improved. Based on the total weight of the composite negative electrode active material, the amount of the second carbonaceous material can be, for example, from about 0.001 wt% to about 5 wt%, from about 0.01 wt% to about 3 wt%, or from about 0.01 wt% to about 1 wt%. Since the composite negative electrode active material includes these ranges of second carbonaceous material, a conductive path is ensured within the composite negative electrode active material, allowing for a further reduction in the internal resistance of the composite negative electrode active material. As a result, the cycle characteristics of the lithium battery including the composite negative electrode active material can be further improved.

[0091] The specific surface area of ​​the composite negative electrode active material can be, for example, about 1 m². 2 / g to approximately 100m 2 / g, approximately 1m 2 / g to approximately 50m 2 / g or approximately 1m 2 / g to approximately 30m 2 / g. Because the composite negative electrode active material has a specific surface area within these ranges, the cycle characteristics of lithium batteries using the composite negative electrode active material can be further improved. The average particle size (D50) of the composite negative electrode active material can be, for example, about 1 μm to about 30 μm, about 3 μm to about 20 μm, or about 5 μm to about 15 μm. The particle size (D10) of the composite negative electrode active material can be, for example, about 0.1 μm to about 10 μm, about 0.5 μm to about 10 μm, or about 1 μm to about 10 μm. The particle size (D90) of the composite negative electrode active material can be, for example, about 10 μm to about 50 μm, about 10 μm to about 30 μm, or about 10 μm to about 25 μm. When the composite negative electrode active material has an average particle size (D50), particle size (D10), and / or particle size (D90) within these ranges, the cycle characteristics of lithium batteries including the composite negative electrode active material can be further improved.

[0092] The negative electrode according to an embodiment includes a composite negative electrode active material. When the negative electrode includes a composite negative electrode active material, improved cycle characteristics and reduced volume change can be provided.

[0093] The negative electrode can be prepared using, for example, a wet process. The negative electrode is manufactured by the following example method, but the disclosure is not limited to this method and can be adjusted according to the desired conditions.

[0094] First, a negative electrode active material composition is prepared by mixing a composite negative electrode active material, a conductive material, a binder, and a solvent. The prepared negative electrode active material composition is then directly coated onto a copper current collector and dried to prepare a negative electrode plate with a negative electrode active material layer. Alternatively, a film layer obtained by casting the negative electrode active material composition onto a separate carrier and then peeling the composition off the carrier is laminated onto the copper current collector to form a negative electrode plate including a negative electrode active material layer.

[0095] As conductive materials, the following can be used: carbon black; fine graphite particles; natural graphite; artificial graphite; acetylene black; Ketjen black; carbon fiber; carbon nanotubes; metal powders, metal fibers, or metal tubes such as copper, nickel, aluminum, or silver; or conductive polymers such as polyphenylene derivatives, but the disclosure is not limited thereto. Any conductive material can be used, provided it is suitable for use in the art.

[0096] As an adhesive, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of these polymers, styrene-butadiene rubber polymers, polyacrylic acid, lithium-substituted polyacrylic acid, polyamide-imide, polyimide, etc., but not limited thereto, can be used, and any adhesive used in the art can be used.

[0097] As solvents, N-methylpyrrolidone (NMP), acetone, water, etc. are used, but not limited to these, and any solvent used in the art can be used.

[0098] Plasticizers and / or pore-forming agents can be further added to the negative electrode active material composition to form pores inside the electrode plate.

[0099] The amounts of composite negative electrode active material, conductive material, binder, and solvent used in the negative electrode can be at the levels typically used in lithium batteries. Depending on the application and construction of the lithium battery, one or more of the conductive material, binder, and solvent may be omitted.

[0100] Based on the total weight of the negative electrode active material layer, the amount of binder included in the negative electrode can be from about 0.1 wt% to about 10 wt% or from about 0.1 wt% to about 5 wt%. Based on the total weight of the negative electrode active material layer, the amount of composite negative electrode active material included in the negative electrode can be from about 0.1 wt% to about 99 wt%, from about 0.1 wt% to about 90 wt%, from about 0.1 wt% to about 50 wt%, from about 0.1 wt% to about 30 wt%, from about 0.1 wt% to about 20 wt%, or from about 0.1 wt% to about 10 wt%.

[0101] In addition to composite negative electrode active materials, the negative electrode may also include negative electrode active materials based on related technologies.

[0102] The negative electrode active material of the related technology includes, but is not limited to, at least one selected from lithium metal, lithium alloyable metals, transition metal oxides, non-transition metal oxides, and carbonaceous materials. Any material can be used here, as long as it is used in the art as a negative electrode active material for lithium batteries.

[0103] Examples of lithium alloyable metals include Si, Sn, Al, Ge, Pb, Bi, Sb, Si-X alloys (where X is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, transition metal, rare earth element, or a combination thereof, and not Si) and Sn-X alloys (where X is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, transition metal, rare earth element, or a combination thereof, and not Sn). Element X can be, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof.

[0104] Transition metal oxides can be, for example, lithium titanium oxide, vanadium oxide, lithium vanadium oxide, etc.

[0105] Non-transition metal oxides can be, for example, SnO2.

[0106] Carbonaceous materials are, for example, crystalline carbon, amorphous carbon, or mixtures thereof. Crystalline carbon is, for example, graphite (such as amorphous, tabular, flake, spherical, or fibrous natural or artificial graphite). Amorphous carbon is, for example, soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbides, or calcined coke.

[0107] Based on the total weight of the negative electrode active material layer, the total amount of composite negative electrode active material and negative electrode active material of related technologies included in the negative electrode can be about 80 wt% to about 99 wt%, about 90 wt% to about 99 wt%, or about 90 wt% to about 95 wt%.

[0108] In this embodiment, the negative electrode may be a dry negative electrode prepared by a dry process.

[0109] The dry negative electrode may include a dry composite negative electrode active material, a dry conductive material, and a dry binder. The dry composite negative electrode active material includes a core and a shell located on the surface of the core and conforming to the surface of the core. The core may include a silicon-containing structure, a silicon-containing compound, or a combination thereof. The shell includes a structure of formula M... a O bat least one first metal oxide represented by (0<a≤3, 0<b<4, and when a is 1, 2 or 3, b is not an integer) and a first carbonaceous material, wherein the first metal oxide is disposed in the first carbonaceous material, and M is at least one metal selected from Groups 2 to 13, Group 15 and Group 16 of the Periodic Table of the Elements.

[0110] In an embodiment, the method of preparing a dry negative electrode may comprise: preparing a dry mixture by dry-mixing a dry composite negative active material, a dry conductive material and a dry binder; providing a negative electrode current collector; disposing an intermediate layer on one side of the negative electrode current collector; and placing the dry mixture on the intermediate layer and rolling the same, so as to arrange a negative active material layer on one surface of the negative electrode current collector.

[0111] First, a dry mixture is prepared by dry-mixing a dry composite negative active material, a dry conductive material and a dry binder. Dry-mixing refers to mixing performed without including a process solvent. The process solvent may be, for example, a solvent used in the preparation of an electrode slurry. The process solvent may be, for example, water, NMP and the like, but is not limited thereto, and any process solvent used in the preparation of an electrode slurry may be used herein. Dry-mixing may be performed using a stirrer at a temperature of, for example, 25°C to 65°C. Dry-mixing may be performed using a stirrer at a rotation speed of, for example, about 10 rpm to about 10000 rpm, or about 100 rpm to about 10000 rpm. Dry-mixing may be performed using a stirrer for, for example, about 1 minute to about 200 minutes, or about 1 minute to about 150 minutes. The composite negative active material may be a dry composite negative active material.

[0112] Dry-mixing may be performed, for example, once or more times. First, a first mixture may be prepared by subjecting the dry composite negative active material, the dry conductive material and the dry binder to a first dry-mixing. The first dry-mixing may be performed, for example, at a temperature of 25°C to 65°C at a rotation speed of 2000 rpm or lower for 15 minutes or less. The first dry-mixing may be performed, for example, at a temperature of about 25°C to about 65°C at a rotation speed of about 500 rpm to about 2000 rpm for about 5 minutes to about 15 minutes. The dry composite negative active material, the dry conductive material and the dry binder may be uniformly mixed through the first dry-mixing. Subsequently, a second mixture may be prepared by subjecting the dry composite negative active material, the dry conductive material and the dry binder to a second dry-mixing. The second dry-mixing may be performed, for example, at a temperature of 25°C to 65°C at a rotation speed of 4000 rpm or higher for 10 minutes or longer. The second dry-mixing may be performed, for example, at a temperature of 25°C to 65°C at a rotation speed of about 4000 rpm to about 9000 rpm for 10 minutes to 60 minutes. A dry mixture comprising a fibrillated dry binder may be obtained through the second dry-mixing.

[0113] The mixer can be, for example, a kneader. The mixer may include, for example, a chamber; one or more rotating shafts located inside the chamber and rotating therein; and blades rotatably coupled to the rotating shafts and located in the longitudinal direction of the rotating shafts. The blades can be, for example, one or more selected from ribbon blades, Sigma blades, jet (Z) blades, dispersing blades, and helical blades. By including blades, a dough-like dry mixture can be prepared by efficiently mixing dry negative electrode composite active material, dry conductive material, and dry binder without solvents.

[0114] The prepared dry mixture can be introduced into an extrusion apparatus and extruded in sheet form. The extrusion pressure can be, for example, from about 4 MPa to about 100 MPa or from about 10 MPa to about 90 MPa. The resulting extrudate in sheet form can be a sheet for use as a negative electrode active material layer.

[0115] As dry conductive materials, the following can be used: carbon black; fine graphite particles; natural graphite; artificial graphite; acetylene black; Ketjen black; carbon fiber; carbon nanotubes; metal powders, fibers, or tubes such as copper, nickel, aluminum, or silver; or conductive polymers such as polyphenylene derivatives, but the disclosure is not limited thereto. Any conductive material can be used, provided it is suitable for use in the art. The conductive material can be, for example, a carbonaceous conductive material. The dry conductive material can be a conductive material that has not yet been in contact with the process solvent.

[0116] Examples of dry binders include vinylidene fluoride / hexafluoropropylene copolymers, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), mixtures of these polymers, and styrene-butadiene rubber polymers, but are not limited thereto; any material used in the art may be used. A dry binder may be, for example, polytetrafluoroethylene (PTFE). A dry binder may be a binder that has not yet been contacted with the process solvent.

[0117] Plasticizers and / or pore-forming agents can be further added to the dry mixture to form pores inside the negative electrode active material layer.

[0118] The amounts of dry composite negative electrode active material, dry conductive material, and dry binder used in the negative electrode active material layer are within the same range as those used in the wet negative electrode.

[0119] Next, a negative current collector is provided. The negative current collector can be, for example, aluminum foil.

[0120] Then, an intermediate layer is disposed on at least one surface of the negative electrode current collector. The intermediate layer may include a carbonaceous conductive material and a binder. The intermediate layer may be omitted.

[0121] Then, the prepared negative electrode active material layer sheet is arranged on the intermediate layer and rolled to deposit the negative electrode active material layer on one surface of the negative electrode current collector, thereby completing the preparation of the negative electrode. The intermediate layer can be located between the negative electrode current collector and the negative electrode active material layer. Rolling can be, for example, rolling, flat rolling, etc., but is not limited to these. The rolling pressure can be, for example, about 0.1 tons / cm². 2 From approximately 10.0 tons / cm 2 However, this is not the only possibility. Excessive pressure during rolling can cause the negative electrode current collector to rupture. Conversely, insufficient pressure during rolling can reduce the adhesion between the negative electrode current collector and the negative electrode active material layer.

[0122] The lithium battery according to an embodiment includes a negative electrode, which includes a composite negative electrode active material.

[0123] Because of the inclusion of a negative electrode containing composite negative electrode active materials, lithium batteries can provide improved cycle characteristics and reduced volume change.

[0124] Lithium batteries are manufactured, for example, by the following exemplary method, but the disclosure is not limited to this method and may be adapted to the required conditions.

[0125] First, the negative electrode is manufactured according to the method used to manufacture the negative electrode.

[0126] Next, a positive electrode active material composition is prepared, comprising a mixture of positive electrode active material, conductive material, binder, and solvent. The positive electrode active material composition is directly coated onto an aluminum current collector and then dried to prepare a positive electrode plate. Alternatively, the positive electrode active material composition can be cast onto a separate carrier, and then a film layer peeled from the carrier can be laminated onto the aluminum current collector to manufacture a positive electrode plate.

[0127] As the positive electrode active material, any lithium-containing metal oxide can be used without limitation, provided it is suitable for use in the art. The positive electrode active material may include, for example, lithium and one or more types of composite oxides of metals selected from cobalt, manganese, nickel, and combinations thereof. The positive electrode active material may include, for example, at least one selected from the group consisting of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, and lithium manganese oxide, but is not necessarily limited thereto. Any material used as a positive electrode active material for lithium batteries can be used here.

[0128] The positive electrode active material can be a compound represented by, for example, one of the following formulas: Li a A 1-b B b D2 (where 0.90≤a≤1.8 and 0≤b≤0.5); Li a E 1-b B b O 2-c Dc (Where, 0.90≤a≤1.8, 0≤b≤0.5 and 0≤c≤0.05); LiE 2-b B b O 4-c D c (Where, 0 ≤ b ≤ 0.5 and 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b B c D α (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Co b B c O 2-α F α (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Co b B c O 2-α F2 (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Mn b B c D α (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2); Li a Ni 1-b-c Mn b B c O 2-α F α (Where, 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F2 (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2); Li a Ni b E c G d O2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5 and 0.001≤d≤0.1); Li a Ni b Co c Mn dGeO2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5 and 0.001≤e≤0.1); Li a NiG b O2 (where 0.9 ≤ a ≤ 1.8 and 0.001 ≤ b ≤ 0.1); Li a CoG b O2 (where 0.90 ≤ a ≤ 1.8 and 0.001 ≤ b ≤ 0.1); Li a MnG b O2 (where 0.90 ≤ a ≤ 1.8 and 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiIO2; LiNiVO4; Li (3-f) J2(PO4)3 (0≤f≤2); Li (3-f) Fe2(PO4)3 (0≤f≤2); and LiFePO4.

[0129] In the above formula, A can be Ni, Co, Mn or a combination thereof; B can be Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, rare earth elements or a combination thereof; D can be O, F, S, P or a combination thereof; E can be Co, Mn or a combination thereof; F can be F, S, P or a combination thereof; G can be Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q can be Ti, Mo, Mn or a combination thereof; I can be Cr, V, Fe, Sc, Y or a combination thereof; and J can be V, Cr, Mn, Co, Ni, Cu or a combination thereof.

[0130] Compounds in which the coating is applied to the surface of the aforementioned compounds can be used, as well as mixtures of the aforementioned compounds and coated compounds. The coating applied to the surface of the aforementioned compounds may include a coating element compound, such as an oxide of the coating element, a hydroxide of the coating element, a hydroxy oxide of the coating element, an oxycarbonate of the coating element, or a hydroxycarbonate of the coating element. The compound constituting the coating may be amorphous or crystalline. The coating element included in the coating may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The method of forming the coating is selected within a range that does not adversely affect the physical properties of the positive electrode active material. The coating method may be, for example, a spraying method, an impregnation method, etc. A detailed description of the coating method will be omitted, as it will be well understood by those skilled in the art.

[0131] The positive active material may be, for example, LiNiO2, LiCoO2, LiMn x O 2x (x=1, 2), LiNi 1-x Mn x O2(0<x<1), LiNi 1-x-y Co x Mn y O2(0≤x≤0.5, 0≤y≤0.5), LiFeO2, V2O5, TiS, MoS and the like.

[0132] The positive active material may be, for example, Li a Ni x Co y M z O 2-b A b (1.0≤a≤1.2, 0≤b≤0.2, 0.8≤x<1, 0≤y≤0.3, 0<z≤0.3, x+y+z=1, M is at least one selected from the group consisting of manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al) and boron (B), and A may be F, S, Cl, Br or a combination thereof), LiNi x Co y Mn z O2(0.8≤x≤0.95, 0≤y≤0.2, 0<z≤0.2, and x+y+z=1), LiNi x Co y Al z O2(0.8≤x≤0.95, 0≤y≤0.2, 0<z≤0.2, and x+y+z=1), LiNi x Co y Al v Mn w O2(0.8≤x≤0.95, 0≤y≤0.2, 0<v≤0.2, 0<w≤0.2, and x+y+z=1) or LiNi x Mn y M' z O 2-b A b(1.0≤a≤1.2, 0≤b≤0.2, 0<x≤0.3, 0.5≤y<1, 0<z≤0.3 and x+y+z=1, M' may be cobalt (Co), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), boron (B) or a combination thereof, and A may be F, S, Cl, Br or a combination thereof).

[0133] Regarding the positive active material composition, a conductive material, a binder, and a solvent for a negative active material may be used herein. Meanwhile, by further adding a plasticizer and / or a pore-forming agent to the positive active material composition and / or the negative active material composition, pores can be formed in the electrode plate.

[0134] The amounts of the positive active material, the conductive material, the binder, and the solvent are at levels commonly used in lithium batteries. Depending on the use and configuration of the lithium battery, at least one of the conductive material, the binder, and the solvent may be omitted.

[0135] Based on the total weight of the positive active material layer, the amount of the binder included in the positive electrode may be, for example, about 0.1 wt% to about 10 wt% or about 0.1 wt% to about 5 wt%. Based on the total weight of the positive active material layer, the amount of the positive active material included in the positive electrode may be, for example, about 70 wt% to about 99 wt%, about 90 wt% to about 99 wt%, or about 95 wt% to about 99 wt%.

[0136] Next, a separator to be interposed between the positive electrode and the negative electrode is prepared.

[0137] Any separator may be used as long as it is commonly used in lithium batteries. As the separator, for example, a separator having low resistance to ion movement of an electrolyte and excellent electrolyte moisturizing ability is used. The separator is a non-woven fabric or woven fabric comprising at least one selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE), and combinations thereof. For lithium ion batteries, for example, a rollable separator comprising polyethylene, polypropylene and the like is used, and for lithium ion polymer batteries, a separator having excellent organic electrolyte impregnation ability is used.

[0138] The separator is manufactured by the following exemplary method, but the disclosure is not necessarily limited to this method, and may be adjusted according to required conditions.

[0139] First, a polymer resin, a filler, and a solvent are mixed to prepare a separator composition. The separator composition is directly applied onto an electrode and dried to form a separator. Alternatively, a film obtained by casting the separator composition on a carrier, drying the composition, and then separating the composition from the carrier is laminated on the electrode to form a separator.

[0140] The polymer used to manufacture the diaphragm is not particularly limited, and any polymer can be used as long as it serves as the binder for the electrode plates. For example, as polymers, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or mixtures thereof can be used.

[0141] Next, the electrolyte is prepared.

[0142] Electrolytes are, for example, organic electrolytes. Organic electrolytes are prepared, for instance, by dissolving lithium salts in an organic solvent.

[0143] As an organic solvent, any organic solvent can be used, as long as it is applicable in the art. Organic solvents can be, for example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butyl carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, isopropyl methyl carbonate, dipropyl carbonate, dibutyl carbonate, benzyl nitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, sulfolane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or mixtures thereof.

[0144] As the lithium salt, any lithium salt can be used, as long as it is suitable for use in the art. Examples of lithium salts include, for instance, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, and LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2 (1≤x≤20, 1≤y≤20), LiCl, LiI or mixtures thereof.

[0145] Alternatively, the electrolyte can be a solid electrolyte. Solid electrolytes are, for example, boron oxide or lithium oxynitride, but are not limited to these. Any solid electrolyte can be used, as long as it is suitable for use in the art. The solid electrolyte can be formed on the negative electrode by methods such as sputtering, or by stacking separate solid electrolyte sheets on the negative electrode.

[0146] Solid electrolytes can be, for example, oxide-based solid electrolytes or sulfide-based solid electrolytes.

[0147] Solid electrolytes can be, for example, oxide-based solid electrolytes. Oxide-based solid electrolytes can be selected from Li... 1+x+y Al x Ti2-x Si y P 3-y O 12 (0≤x≤2 and 0≤y≤3), BaTiO3, Pb(Zr,Ti)O3 (PZT), Pb 1-x La x Zr 1- y Ti y O3 (PLZT) (0≤x≤1, 0≤y≤1), Pb(Mg3Nb 2 / 3 )O3-PbTiO3 (PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, Li3PO4, Li x Ti y (PO4)3 (0<x<2 and 0<y<3), Li x Al y Ti z (PO4)3 (0<x<2, 0<y<1 and 0<z<3), Li 1+x+y (Al,Ga) x (Ti,Ge) 2-x Si y P 3-y O 12 (0≤x≤1 and 0≤y≤1), Li x La y TiO3 (0<x<2 and 0<y<3), Li2O, LiOH, Li2CO3, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2, Li 3+x La3M2O 12 (M is Te, Nb, or Zr, and x is an integer from 1 to 10) one or more of them. The solid electrolyte is manufactured by sintering. For example, the oxide-based solid electrolyte may be a garnet-type solid electrolyte selected from Li7La3Zr2O 12 (LLZO) and Li 3+x La3Zr 2-a M a O 12 (M-doped LLZO, M is Ga, W, Nb, Ta or Al, and x is an integer from 1 to 10).

[0148] The sulfide-based solid electrolyte may include, for example, lithium sulfide, silicon sulfide, phosphorus sulfide, boron sulfide, or a combination thereof. The sulfide-based solid electrolyte particles may include Li2S, P2S5, SiS2, GeS2, B2S3, or a combination thereof. The sulfide-based solid electrolyte particles may be Li2S or P2S5. It is known that the sulfide-based solid electrolyte particles have a higher lithium ion conductivity than the lithium ion conductivity of other inorganic compounds. For example, the sulfide-based solid electrolyte includes Li2S and P2S5. When the sulfide solid electrolyte material constituting the sulfide-based solid electrolyte includes Li2S-P2S5, the mixing molar ratio of Li2S to P2S5 may be, for example, in the range of about 50:50 to about 90:10. In an embodiment, by adding Li3PO4, a halogen, a halogen compound, Li 2+2x Zn 1-x GeO4 ("LiSiCON", 0≤x<1), Li 3+y PO 4-x N x ("LiPON", 0<x<4, 0<y<3), Li 3.25 Ge 0.25 P 0.75 S4 ("ThioLISICON"), Li2O-Al2O3-TiO2-P2O5 ("LATP") to an inorganic solid electrolyte of Li2S-P2S5, SiS2, GeS2, B2S3, or a combination thereof, the prepared inorganic solid electrolyte may be used as the sulfide solid electrolyte. Non-limiting examples of the sulfide solid electrolyte material include: Li2S-P2S5; Li2S-P2S5-LiX (X=halogen element); Li2S-P2S5-Li2O; Li2S-P2S5-Li2O-LiI; Li2S-SiS2; Li2S-SiS2-LiI; Li2S-SiS2-LiBr; Li2S-SiS2-LiCl; Li2S-SiS2-B2S3-LiI; Li2S-SiS2-P2S5-LiI; Li2S-B2S3; Li2S-P2S5-Z m S n (0<m<10, 0<n<10, Z is Ge, Zn or Ga); Li2S-GeS2; Li2S-SiS2-Li3PO4; and Li2S-SiS2-LiPMO q (0<p<10, 0<q<10, M is P, Si, Ge, B, Al, Ga or In). In this regard, the sulfide solid electrolyte material may be prepared by treating raw materials of the sulfide solid electrolyte material (e.g., Li2S, P2S5, etc.) through a melt quenching method, a mechanical milling method, or the like. In addition, a calcination process may be performed after the treatment. The sulfide-based solid electrolyte may be amorphous, crystalline, or a mixture thereof.

[0149] Reference Figure 6 The lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, the negative electrode 2, and the separator 4 can be wound or folded to form a battery structure 7 (see...). Figure 7 The battery structure 7 is housed within the battery casing 5. An organic electrolyte is injected into the battery casing 5, and the battery casing 5 is sealed with a cover assembly 6 to complete the lithium battery 1. The battery casing 5 is cylindrical, but is not limited to this shape; for example, its shape can be square, thin film, etc.

[0150] Reference Figure 7 According to an embodiment, the lithium battery 1 includes a positive electrode 3, a negative electrode 2, and a separator 4. The separator 4 may be located between the positive electrode 3 and the negative electrode 2, and the positive electrode 3, negative electrode 2, and separator 4 may be wound or folded to form a battery structure 7. The battery structure 7 is housed in a battery casing 5. Electrode terminals 8 may be included as electrical paths for guiding current formed in the battery structure 7 to the outside. An organic electrolyte is injected into the battery casing 5 and sealed to complete the manufacture of the lithium battery 1. The battery casing 5 may have a rectangular shape, but is not limited to this shape, and may have, for example, a cylindrical shape, a thin-film type, etc.

[0151] Reference Figure 8 The lithium battery 1 according to an embodiment includes a positive electrode 3, a negative electrode 2, and a separator 4. The separator 4 is located between the positive electrode 3 and the negative electrode 2 to form a battery structure. The battery structure 7 is stacked in a dual-cell structure and then housed in a battery casing 5. Electrode terminals 8 may be included as electrical paths for guiding current formed in the battery structure 7 to the outside. An organic electrolyte is injected into the battery casing 5 and sealed to complete the manufacture of the lithium battery 1. The battery casing 5 may have a rectangular shape, but is not limited to this shape, and may have, for example, a cylindrical shape, a thin-film type, etc.

[0152] Pouch-type lithium batteries and using pouches as batteries Figures 6 to 8 Each lithium battery corresponds to a specific battery casing. A pouch-type lithium battery includes at least one battery structure. A separator is positioned between the positive and negative electrodes to form the battery structure. After stacking the battery structures in a dual-cell structure, they are impregnated with an organic electrolyte and housed and sealed in a pouch to complete the pouch-type lithium battery. For example, although not shown in the figures, the positive, negative, and separator can simply be stacked and housed in a pouch as an electrode assembly. In embodiments, the positive, negative, and separator can be wound or folded into an electrode assembly in the form of a jelly roll and then housed in a pouch. An organic electrolyte is then injected into the pouch, and the pouch is sealed to complete the manufacture of the lithium battery.

[0153] Lithium batteries are used in electric vehicles (EVs) due to their excellent cycle life characteristics and high-rate characteristics. For example, lithium batteries are used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). In addition, lithium batteries are used in fields requiring large amounts of electric power storage. For example, lithium batteries are used in electric bicycles, electric power tools, and the like.

[0154] A plurality of lithium batteries are stacked to form a battery module, and a plurality of battery modules may form a battery pack. Such a battery pack can be used in any device that requires high capacity and high output. For example, the battery pack can be used in notebook computers, smartphones, electric vehicles, and the like. The battery module may include, for example, a plurality of batteries and a frame for holding the plurality of batteries. The battery pack may include, for example, a plurality of battery modules and bus bars connecting the plurality of battery modules. The battery module and / or the battery pack may further include a cooling device. The plurality of battery packs may be controlled by a battery management system. The battery management system may include the battery packs and a battery control device connected to the battery packs.

[0155] A method of preparing a composite negative active material according to an embodiment includes: providing a silicon-containing negative active material, such as a silicon-containing structure, a silicon-containing compound, or a combination thereof; providing a composite; and subjecting the silicon-containing structure, the silicon-containing compound, or the combination thereof and the composite to mechanical milling, wherein the composite includes a compound represented by the formula M a O b (0<a≤3, 0<b<4, and when a is 1, 2, or 3, b is not an integer) at least one first metal oxide and a first carbonaceous material, and the first metal oxide is disposed within a matrix of the first carbonaceous material, and M is at least one metal selected from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements.

[0156] A silicon-containing negative active material is provided. The silicon-containing negative active material may be, for example, a silicon-containing structure, a silicon-containing compound, or a combination thereof. The silicon-containing structure may include, for example, the aforementioned silicon composite structure. The silicon-containing compound may include, for example, SiO x (0<x<2).

[0157] Providing the composite includes, for example, supplying a reaction gas including a carbon source gas to a second metal oxide represented by the formula M a O c (0<a≤3, 0<c≤4, and when a is 1, 2, or 3, c is an integer), and performing a heat treatment thereon to form the composite, wherein M is at least one metal selected from Groups 2 to 13, Group 15, and Group 16 of the Periodic Table of the Elements.

[0158] The carbon source gas may be the compound represented by Formula 1, or may be a mixed gas of at least one selected from the group consisting of the compound represented by Formula 1, the compound represented by Formula 2, and the oxygen-containing gas represented by Formula 3.

[0159] <Formula 1>

[0160] C n H (2n+2-a) [OH] a

[0161] In Formula 1, n is 1 to 20 and a is 0 or 1;

[0162] <Formula 2>

[0163] C n H 2n

[0164] In Formula 2, n is 2 to 6; and

[0165] <Formula 3>

[0166] C x H y O z

[0167] In Formula 3, x is 0 or an integer of 1 to 20, y is 0 or an integer of 1 to 20, and z is 1 or 2.

[0168] Each of the compound represented by Formula 1 and the compound represented by Formula 2 may be at least one selected from methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by Formula 3 may include, for example, carbon dioxide (CO2), carbon monoxide (CO), water vapor (H2O), or a mixture thereof.

[0169] After supplying the reaction gas including the carbon source gas to the second metal oxide represented by M a O c (0<a≤3, 0<c≤4, when a is 1, 2 or 3, c is an integer) and performing heat treatment, a cooling process using at least one inert gas selected from nitrogen, helium and argon may be further performed. The cooling process refers to a process of adjusting the temperature to room temperature (about 20°C to about 25°C). The carbon source gas may include at least one inert gas selected from nitrogen, helium and argon.

[0170] In the method of manufacturing the composite, the process of growing a carbonaceous material (for example, graphene) may be performed under various conditions according to a gas phase reaction.

[0171] According to a first condition, for example, first, methane is supplied to the M provided with a O creactor provided with the second metal oxide represented by (0<a≤3, 0<c≤4, when a is 1, 2 or 3, c is an integer), and the reactor is heated to a heat treatment temperature (T). The heating time for reaching the heat treatment temperature (T) is from about 10 minutes to about 4 hours, and the heat treatment temperature (T) is from about 700°C to about 1100°C. The heat treatment is performed for a reaction time at the heat treatment temperature (T). The reaction time is, for example, from about 4 hours to about 8 hours. The product obtained by the heat treatment is cooled to room temperature to prepare a composite. The time taken to perform the process of cooling the obtained product from the heat treatment temperature to room temperature is, for example, about 1 hour to 5 hours.

[0172] According to the second condition, for example, first, hydrogen is supplied to the reactor provided with the second metal oxide represented by M a O c (0<a≤3, 0<c≤4, when a is 1, 2 or 3, c is an integer), and the reactor is heated to a heat treatment temperature (T). The heating time for reaching the heat treatment temperature (T) is from about 10 minutes to about 4 hours, and the heat treatment temperature (T) is from about 700°C to about 1100°C. After performing the heat treatment for a predetermined reaction time at the heat treatment temperature (T), methane gas is supplied, and the heat treatment is performed for the remaining reaction time. The total reaction time is, for example, from about 4 hours to about 8 hours. The product obtained by the heat treatment is cooled to room temperature to prepare a composite. Nitrogen is supplied during the process of cooling the obtained product. The time taken to perform the process of cooling the obtained product from the heat treatment temperature to room temperature is, for example, about 1 hour to 5 hours.

[0173] According to the third condition, for example, first, hydrogen is supplied to the reactor provided with the second metal oxide represented by M a O c (0<a≤3, 0<c≤4, when a is 1, 2 or 3, c is an integer), and the reactor is heated to a heat treatment temperature (T). The heating time for reaching the heat treatment temperature (T) is from about 10 minutes to about 4 hours, and the heat treatment temperature (T) is from about 700°C to about 1100°C. After performing the heat treatment for a predetermined reaction time at the heat treatment temperature (T), a mixed gas of methane and hydrogen is supplied, and the heat treatment is performed for the remaining reaction time. The total reaction time is, for example, from about 4 hours to about 8 hours. The product obtained by the heat treatment is cooled to room temperature to prepare a composite. Nitrogen is supplied during the process of cooling the obtained product. The time taken to perform the process of cooling the obtained product from the heat treatment temperature to room temperature is, for example, about 1 hour to 5 hours.

[0174] In the process of preparing the composite, when the carbon source gas includes water vapor, a composite with very excellent electrical conductivity can be obtained. The amount of water vapor in the gas mixture is not limited, and is, for example, from about 0.01 vol% to about 10 vol% based on 100 vol% of the total carbon source gas. The carbon source gas can be, for example: methane; a mixture of methane and an inert gas; or a mixture of methane and a gas containing oxygen.

[0175] The carbon source gas can be, for example, methane; a mixture of methane and carbon dioxide; or a mixture of methane, carbon dioxide, and water vapor. The molar ratio of methane to carbon dioxide in a mixture of methane and carbon dioxide can be from about 1:0.20 to about 1:0.50, from about 1:0.25 to about 1:0.45, or from about 1:0.30 to about 1:0.40. In a gaseous mixture of methane, carbon dioxide, and water vapor, the molar ratio of methane, carbon dioxide, and water vapor can be from about 1:0.20 to 0.50:0.01 to 1.45, from about 1:0.25 to 0.45:0.10 to 1.35, or from about 1:0.30 to 0.40:0.50 to 1.0.

[0176] The carbon source gas can be, for example, carbon monoxide or carbon dioxide. The carbon source gas is, for example, a mixture of methane and nitrogen. In the mixture of methane and nitrogen, the molar ratio of methane to nitrogen can be about 1:0.20 to 1:0.50, about 1:0.25 to 1:0.45, and about 1:0.30 to 1:0.40. The carbon source gas may not include inert gases such as nitrogen.

[0177] The heat treatment pressure can be selected by taking into account the heat treatment temperature, the composition of the gas mixture, and the desired carbon coating amount. The heat treatment pressure can be controlled by adjusting the amount of gas mixture flowing into and out of the gas mixture. For example, heat treatment pressures are 0.5 atm or higher, 1 atm or higher, 2 atm or higher, 3 atm or higher, 4 atm or higher, or 5 atm or higher.

[0178] The heat treatment time can be selected taking into account the heat treatment temperature, heat treatment pressure, composition of the gas mixture, and desired carbon coating amount. For example, the reaction time at the heat treatment temperature can be, for example, about 10 minutes to about 100 hours, about 30 minutes to about 90 hours, or about 50 minutes to about 40 hours. For example, as the heat treatment time increases, the amount of deposited carbon (e.g., graphene) increases, thus improving the electrical properties of the composite. However, this trend does not necessarily have to be proportional to time. For example, after a predetermined time, carbon deposition (e.g., graphene deposition) may no longer occur, or the deposition rate may be low.

[0179] Through the gas phase reaction of a carbon source gas, even at low temperatures, a composite can be obtained by coating a uniform carbonaceous material (e.g., graphene) on at least one selected from the group consisting of M a O c a second metal oxide represented by (0<a≤3, 0<c≤4, and when a is 1, 2 or 3, c is an integer) and a reduction product thereof (that is, a first metal oxide represented by M a O b (0<a≤3, 0<b<4, a is 1, 2 or 3, and b is not an integer)).

[0180] The composite includes: a carbonaceous material matrix (e.g., a graphene matrix) having at least one structure selected from a spherical structure, a spiral structure in which a plurality of spherical structures are connected to each other, a cluster structure in which a plurality of spherical structures are aggregated with each other, and a sponge structure; and at least one selected from the group consisting of a first metal oxide represented by M a O b (0<a≤3, 0<b<4, a is 1, 2 or 3, and b is not an integer) and a second metal oxide represented by M a O c (0<a≤3, 0<c≤4, and when a is 1, 2 or 3, c is an integer), disposed in the carbonaceous material matrix.

[0181] Next, the silicon-containing structure, the silicon-containing compound or a combination thereof, and the composite are subjected to mechanical grinding. In the mechanical grinding, the grinding method is not particularly limited, and any method in the related art that brings the silicon-containing structure, the silicon-containing compound or a combination thereof into contact with the composite and presses the resulting product can be used here. A Nobilta mixer can be used in the grinding. The number of revolutions of the mixer during grinding may be, for example, 2000 rpm or higher, or 3000 rpm or higher. The number of revolutions of the mixer during grinding may be, for example, 4000 rpm or lower. The number of revolutions of the mixer during grinding may be, for example, from about 2000 rpm to about 4000 rpm, or from about 3000 rpm to about 4000 rpm.

[0182] When the milling speed is too low, the shear force applied to the silicon-containing structure, silicon-containing compound, or combination thereof and composite is weak, making it difficult to prepare the silicon-containing structure, silicon-containing compound, or combination thereof and composite in composite form. When the milling speed is too high, the composite forms in too short a time, making it difficult to uniformly coat the composite onto the silicon-containing structure and / or silicon-containing compound to form a uniform and continuous shell. Milling time can be, for example, about 5 minutes to about 100 minutes, about 5 minutes to about 60 minutes, or about 5 minutes to about 30 minutes. When the milling time is too short, it is difficult to uniformly coat the composite onto the silicon-containing structure and / or silicon-containing compound to form a uniform and continuous shell. When the milling time is too long, production efficiency decreases. Based on the total weight of the silicon-containing anode active material and the composite, the amount of the composite can be 5 wt% or less, 4 wt% or less, 3 wt% or less, 2 wt% or less, or 1 wt% or less. Based on the total weight of the silicon-containing anode active material and the composite, the amount of the composite can be, for example, from about 0.01 wt% to about 5 wt%, from about 0.01 wt% to about 4 wt%, from about 0.01 wt% to about 3 wt%, from about 0.1 wt% to about 2 wt%, or from about 0.1 wt% to about 1 wt%. For example, based on the total weight of the silicon-containing anode active material and the composite, the amount of the composite can be from about 0.01 parts by weight to about 5 parts by weight, from about 0.01 parts by weight to about 4 parts by weight, from about 0.01 parts by weight to about 3 parts by weight, from about 0.1 parts by weight to about 3 parts by weight, from about 0.1 parts by weight to about 2 parts by weight, or from about 0.1 parts by weight to about 1 part by weight. The average particle size (D50) of the composite used for mechanically milling the silicon-containing anode active material and the composite can be, for example, from about 50 nm to about 200 nm, from about 100 nm to about 300 nm, or from about 200 nm to about 500 nm.

[0183] The disclosure will be described in more detail through the following examples and comparative examples. However, these examples are for illustrative purposes only, and the scope of the disclosure is not limited thereto.

[0184] (Preparation of the complex)

[0185] Preparation Example 1: A l 2O3@Gr complex

[0186] Al2O3 particles (average particle size: about 20 nm) were placed in a reactor, and CH4 was then supplied to the reactor at about 300 sccm and 1 atm for about 30 minutes. The temperature inside the reactor was then raised to 1000 °C at a heating rate of about 23 °C / min.

[0187] Then, heat treatment is performed by maintaining this temperature for 7 hours. Then, the supply of CH4 is stopped and the temperature inside the reactor is adjusted to room temperature (25°C), to obtain Al2O3 particles and Al2O as a reduction product thereof z (0<z<3) A composite in which particles are embedded in graphene.

[0188] The amount of alumina contained in the composite is 60 wt%.

[0189] Preparation Example 2: Al2O3@Gr Complex

[0190] A composite was prepared in the same manner as in Preparation Example 1, except that Al2O3 particles (average particle diameter: about 200 nm) were used instead of Al2O3 particles (average particle diameter: about 20 nm).

[0191] Comparative preparation example 1: SiO2@Gr composite

[0192] SiO2 particles (average particle diameter: about 15 nm) were placed in a reactor, then CH4 was supplied into the reactor at about 300 sccm and 1 atm for about 30 minutes, and the temperature inside the reactor was raised to 1000°C at a heating rate of about 23°C / min.

[0193] Then, heat treatment is performed by maintaining this temperature for 7 hours. Then, the supply of CH4 is stopped and the temperature inside the reactor is adjusted to room temperature (25°C), to obtain SiO2 particles and SiO as a reduction product thereof y (0<y<2) A composite in which particles are embedded in graphene.

[0194] (Production of silicon-containing negative active material)

[0195] Preparation Example 3: Silicon Composite Structure

[0196] Acicular silicon is pulverized to obtain plate-like and acicular silicon particles having a length of about 125 nm and a thickness of about 40 nm, and the silicon particles have a surface on which silicon oxide (SiO x , 0<x<2) with a thickness of about 0.1 nm is formed.

[0197] A composition including 30 parts by weight of the plate-like and acicular silicon particles, 10 parts by weight of stearic acid, and 60 parts by weight of isopropanol is prepared. The prepared composition is spray-dried and dried to obtain porous silicon secondary particles having an average particle diameter of about 5 μm.

[0198] Spray drying was performed using a spray dryer (Mini Spray Dryer, Fujisaki Electric). In a nitrogen atmosphere, the nozzle size was about 5 μm, the pressure during spray drying was about 0.4 MPa, and the temperature of the powder spray atmosphere was about 200°C. The prepared composition was sprayed under these spray drying conditions to remove isopropanol, thereby obtaining porous silicon secondary particles.

[0199] The prepared porous silicon secondary particles were placed in a reactor. Under the condition that CH4 was supplied into the reactor at about 300 sccm and 1 atm, the temperature inside the reactor was raised to 1000°C at a heating rate of about 23°C / min.

[0200] Then, heat treatment was performed by maintaining this temperature for 5 hours. Thereafter, the supply of CH4 was stopped and the internal temperature of the reactor was adjusted to room temperature (25°C) to obtain a porous silicon composite structure.

[0201] The porous silicon composite structure includes porous silicon secondary particles and highly crystalline first graphene sheets disposed on the porous silicon secondary particles, wherein the porous silicon secondary particles comprise an aggregate of two or more silicon composite primary particles, and the silicon composite primary particles include silicon and silicon suboxide (SiO x , 0<x<2) disposed on the silicon, and second graphene sheets disposed on the silicon suboxide.

[0202] Based on 100 parts by weight of the total weight of the porous silicon composite structure, the amount of the first graphene sheets and the second graphene sheets in the silicon composite structure is about 25 parts by weight. The silicon composite structure is porous.

[0203] Preparation Example 4: Silicon Composite Structure + Amorphous Carbon Coating

[0204] 60 parts by weight of the silicon composite structure prepared according to Preparation Example 3, 40 parts by weight of coal tar pitch, and 10 parts by weight of N-methylpyrrolidone were added to a planetary mixer, and a mixing process was performed.

[0205] The coal tar pitch was infiltrated between the pores of the porous silicon secondary particles included in the silicon composite structure through the mixing process. The mixing process for infiltrating the coal tar pitch was carried out for 5 minutes each in the sequence of stirring-defoaming-stirring, for a total of 15 minutes, and the cycle of stirring-defoaming-stirring was defined as one cycle, and a total of 4 cycles were performed. During stirring, the revolution speed was 1000 rpm and the rotation speed was 1000 rpm, and during defoaming, the revolution speed was 2000 rpm and the rotation speed was 64 rpm. 40 parts by weight of coal tar pitch was divided into 4 portions, and each portion was added in each cycle. The mixing temperature was controlled at about 70°C. The mixed product was heat-treated at about 1000°C for 4 hours in a nitrogen atmosphere.

[0206] As a result, a silicon composite structure was prepared in which a carbonaceous coating film containing first amorphous carbon was disposed on the surface of the silicon composite structure, and second amorphous carbon was disposed inside the silicon composite structure. The second amorphous carbon is located in the pores of porous silicon secondary particles included in the silicon composite structure. The weight ratio of first amorphous carbon to second amorphous carbon is 1:2. In the prepared silicon composite structure, the weight ratio of carbon to amorphous carbon in the graphene sheet is 2:8. The graphene sheet is a combination of both the first graphene sheet and the second graphene sheet. The amorphous carbon is a combination of both the first amorphous carbon and the second amorphous carbon.

[0207] (Manufacturing of composite negative electrode active materials)

[0208] Example 1: 1 wt% Al2O3@Gr composite (0.6 wt% alumina) Coating silicon composite structure

[0209] The silicon composite structure prepared according to Preparation Example 3 and the composite prepared according to Preparation Example 1 were milled using a Nobilta mixer (Nobilta mixer, Hosokawa, Japan) at a rotation speed of approximately 2000 rpm to approximately 4000 rpm for approximately 5 to 30 minutes to obtain a composite negative electrode active material. The composite negative electrode active material has a structure in which a shell comprising the composite and / or the milling result thereof is coated on a silicon-containing negative electrode active material core.

[0210] The silicon composite structure obtained according to Preparation Example 3 is mixed in a weight ratio of 99:1 with the composite obtained according to Preparation Example 1.

[0211] Example 2: 0.1 wt% Al2O3@Gr complex Coating silicon composite structure

[0212] Except that the weight ratio of the silicon composite structure obtained according to Preparation Example 3 to the composite obtained according to Preparation Example 1 is changed to 99.9:0.1, the composite negative electrode active material is prepared in the same manner as in Example 1.

[0213] Example 3: 0.5 wt% Al2O3@Gr complex Coating silicon composite structure

[0214] Except that the weight ratio of the silicon composite structure obtained according to Preparation Example 3 to the composite obtained according to Preparation Example 1 is changed to 99.5:0.5, the composite negative electrode active material is prepared in the same manner as in Example 1.

[0215] Example 4: 5wt% Al2O3@Gr complex Coating silicon composite structure

[0216] Except that the weight ratio of the silicon composite structure obtained according to Preparation Example 3 to the composite obtained according to Preparation Example 1 is changed to 95:5, the composite negative electrode active material is prepared in the same manner as in Example 1.

[0217] Example 5: 1 wt% Al2O3@Gr complex + 0.1 wt% CNT Coating silicon composite structure

[0218] A composite negative electrode active material was prepared in the same manner as in Example 1, except that the weight ratio of the silicon composite structure obtained according to Preparation Example 3, the composite obtained according to Preparation Example 1, and carbon nanotubes (CNT) was 98.9:1.0:0.1.

[0219] Carbon nanotubes (CNT) were additionally used in addition to the silicon composite structure obtained according to Preparation Example 3 and the composite obtained according to Preparation Example 1.

[0220] The CNT has a length of 200 nm to 300 nm, and the carbon nanotubes have a diameter of about 10 nm.

[0221] Example 6: 1 wt% Al2O3@Gr complex Coating The silicon composite structure has alumina particles with a diameter of 200 nm.

[0222] A composite negative electrode active material was prepared in the same manner as in Example 1, except that the composite obtained according to Preparation Example 2 was used in place of the composite obtained according to Preparation Example 1.

[0223] Example 7: 1 wt% Al2O3@Gr complex Coating [Amorphous carbon-coated silicon composite structure]

[0224] A composite negative electrode active material was prepared in the same manner as in Example 1, except that the amorphous carbon-coated silicon composite structure obtained according to Preparation Example 4 was used in place of the silicon composite structure obtained according to Preparation Example 3.

[0225] Example 8: 1 wt% Al2O3@Gr complex Coating SiO x

[0226] Except that SiO having an average particle diameter of 6 μm x (0<x<2) was used as the silicon-based negative electrode active material to replace the silicon composite structure obtained according to Preparation Example 3, a composite negative electrode active material was prepared in the same manner as in Example 1.

[0227] Comparison Example 1: Bare Silicon Composite Structure

[0228] The silicon composite structure prepared according to Preparation Example 3 was used as it is as a negative electrode active material.

[0229] Comparative Example 2: 1 wt% [Al2O3 + Graphene (Gr)] mixture Coating silicon composite structure

[0230] A composite negative active material was prepared in the same manner as in Example 1, except that a simple mixture of Al₂O₃ particles (average particle size: about 20 nm) and graphene at a weight ratio of 60:40 was used in place of the composite prepared according to Preparation Example 1.

[0231] Compare Example 3: A l2 A simple mixture of O3@Gr and silicon composite structures

[0232] A simple mixture of the silicon composite structure prepared according to Preparation Example 3 and the composite prepared according to Preparation Example 1 at a weight ratio of 99:1 was used as the negative active material.

[0233] Comparative Example 4: 1 wt% SiO2@Gr composite Coating silicon composite structure

[0234] A composite negative active material was prepared in the same manner as in Example 1, except that the composite obtained in Comparative Preparation Example 1 was used in place of the composite prepared according to Preparation Example 1.

[0235] Comparison Example 5: Bare SiO x

[0236] SiO having an average particle size of 6 μm was used as it is x (0<x<2) as the negative active material.

[0237] (Fabrication of lithium battery (full cell), wet negative electrode)

[0238] Example 9

[0239] (Preparation of negative electrode)

[0240] A slurry was prepared by mixing the composite negative active material prepared according to Example 1, graphite, a CMC / SBR binder (1:1 weight ratio mixture), and deionized water. The mixing ratio of the solid content of the mixture of the composite negative active material and graphite to the CMC / SBR binder was 97.5:2.5 (weight ratio). In the mixture of the composite negative active material prepared according to Example 1 and graphite, the weight ratio of the composite negative active material to graphite was 2:98.

[0241] The slurry was bar-coated on a copper foil current collector to a thickness of 100 μm, dried at room temperature, vacuum-dried again at 120°C under vacuum conditions, and rolled to prepare a negative electrode.

[0242] (Fabrication of positive electrode)

[0243] LiNi 0.91 Co 0.05 Al 0.04A mixture of O2 (hereinafter referred to as NCA91) composite positive electrode active material, carbon conductive material (Denka Black) and polyvinylidene fluoride (PVDF) in a weight ratio of 96:2:2 was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry.

[0244] The slurry was rod-coated to a thickness of 40 μm on an aluminum current collector, dried at room temperature, dried again under vacuum at 120 °C, and rolled to prepare the positive electrode.

[0245] (Manufacturing of coin-operated batteries)

[0246] A coin cell was manufactured using the positive and negative electrodes prepared as described above, a polypropylene separator (Celgard 3510), and a solution of 1.15 M LiPF6 and 1.5 wt% vinylene carbonate (VC) dissolved in ethylene carbonate (EC) + ethyl methyl carbonate (EMC) + dimethyl carbonate (DMC) (volume ratio 2:4:4) as the electrolyte.

[0247] Examples 10 to 16

[0248] The coin cell is manufactured in the same manner as in Example 9, except that each of the composite negative electrode active materials prepared according to Examples 2 to 8 is used instead of the composite negative electrode active material prepared according to Example 1.

[0249] Comparison Examples 6 to 10

[0250] Except that each of the negative electrode active materials prepared according to Comparative Examples 1 to 5 is used instead of the composite negative electrode active material prepared according to Example 1, the coin cell is manufactured in the same manner as in Example 9.

[0251] (Manufacturing of lithium batteries (full cells) and dry anodes)

[0252] Example 17

[0253] (Preparation of the negative electrode)

[0254] The composite negative electrode active material (which is a dry first negative electrode active material), graphite (which is a dry second negative electrode active material), carbon conductive material (Denka Black) (which is a dry conductive material), and polytetrafluoroethylene (PTFE) (which is a dry binder) prepared according to Example 1 were added to a blade mixer in a weight ratio of 1.8:90.2:4:4, and then a first dry mixing was performed at 25°C and 1000 rpm for 10 minutes to prepare a first mixture in which the first negative electrode active material, the second negative electrode active material, the conductive material, and the binder were uniformly mixed.

[0255] Then, to fibrillate the binder, the first mixture was subjected to a second mixing at 25°C and 1000 rpm for 10 minutes to prepare the second mixture. No separate solvent was used in the preparation of the first and second mixtures.

[0256] The prepared second mixture was fed into an extruder and extruded to prepare a self-standing membrane with a sheet-like layer of negative electrode active material. The extrusion pressure was 50 MPa.

[0257] A carbon layer, serving as an intermediate layer, is positioned on one surface of a 12 μm thick copper film to prepare a first laminate in which the intermediate layer is located on one surface of the negative electrode current collector.

[0258] An intermediate layer was prepared by coating an aluminum film with a composition comprising a carbon conductive material (Denka Black) and polyvinylidene fluoride (PVDF) and then drying it. The thickness of the intermediate layer, located on one surface of the aluminum film, was approximately 1 μm.

[0259] The negative electrode active material layer is placed on the middle layer of the first laminate and rolled to prepare the negative electrode.

[0260] (The manufacture of the positive electrode)

[0261] LiNi 0.91 Co 0.05 Al 0.04 A mixture of O2 (referred to as NCA91 in the text), carbon conductive material (Denka Black), and polyvinylidene fluoride (PVDF) in a weight ratio of 96:2:2 was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry.

[0262] The slurry was rod-coated to a thickness of 40 μm on an aluminum current collector, dried at room temperature, dried again under vacuum at 120 °C, and rolled to prepare the positive electrode.

[0263] (Manufacturing of coin-operated batteries)

[0264] A coin cell was manufactured using the positive and negative electrodes prepared as described above, a polypropylene separator (Celgard 3510), and a solution of 1.15 M LiPF6 and 1.5 wt% vinylene carbonate (VC) dissolved in ethylene carbonate (EC) + ethyl methyl carbonate (EMC) + dimethyl carbonate (DMC) (volume ratio 2:4:4) as the electrolyte.

[0265] Compare Example 11

[0266] A coin-type battery was fabricated in the same manner as in Example 17, except that the negative active material prepared according to Comparative Example 1 was used as the dry first negative active material in place of the composite negative active material prepared according to Example 1.

[0267] Evaluation Example 1: Evaluation of specific surface area and particle size

[0268] The specific surface area and particle size of each of the silicon composite structure prepared according to Preparation Example 3, the composite negative active material prepared according to Example 1, and the SiO prepared according to Comparative Example 5 were measured x (0<x<2) and the composite negative active material prepared according to Example 8. The results are shown in Table 1.

[0269] The specific surface area was measured by a nitrogen adsorption method. The particle size was measured using a laser scattering particle size distribution analyzer.

[0270] [Table 1]

[0271] <![CDATA[Specific surface area[m 2 / g]]]> D10[μm] D50[μm] D90[μm] Preparation Example 3 4.5 4.7 9.5 16.8 Example 1 7.0 3.5 8.6 16.1 Compare Example 5 6.0 4.1 6.1 9.0 Example 8 8.0 3.1 5.9 10.1

[0272] As shown in Table 1, the composite negative active material prepared according to Example 1 has a larger specific surface area and smaller D10, D50, and D90 particle sizes than the silicon composite structure prepared according to Preparation Example 3.

[0273] In addition, compared with the SiO prepared according to Comparative Example 5 x (0<x<2), the composite negative active material prepared according to Example 8 has a larger specific surface area and smaller D10, D50, and D90 particle sizes.

[0274] Evaluation Example 2: XPS Spectroscopic Evaluation (I)

[0275] In the process of preparing the composite prepared according to Preparation Example 1, XPS spectra were measured over time using Qunatum 2000 (Physical Electronics). Before heating, the XPS spectra of the C1s orbital and Al2p orbital of the sample were measured after 1 minute, 5 minutes, 30 minutes, 1 hour, and 4 hours, respectively. At the initial stage of heating, only the peak of the Al2p orbital appeared, and no peak of the C1s orbital appeared. After 30 minutes, the peak of the C1s orbital clearly appeared, and the size of the peak of the Al2p orbital decreased significantly.

[0276] After 30 minutes, near 284.5 eV, the peak of the C1s orbital clearly appeared due to the C-C bonds and C=C bonds caused by graphene growth.

[0277] As the reaction time elapses, the oxidation number of aluminum decreases, so that the peak position of the Al2p orbital shifts toward a lower binding energy (eV).

[0278] Accordingly, it is found that as the reaction proceeds, graphene grows on the Al₂O₃ particles, and Al₂O as a reduction product of Al₂O₃ is produced x (0<x<3).

[0279] The average amounts of carbon and aluminum were measured through XPS analysis results of 10 regions of the composite sample prepared according to Preparation Example 1. Regarding the measurement results, the deviation of the aluminum amount for each region was calculated. The deviation of the aluminum amount is expressed as a percentage of the average value, and this percentage is referred to as uniformity. The percentage of the average value of the deviation of the aluminum amount (that is, the uniformity of the aluminum amount) is 1%. Accordingly, it is found that alumina is uniformly distributed in the composite prepared according to Preparation Example 1.

[0280] Evaluation Example 3: XPS Spectroscopic Evaluation (II)

[0281] The silicon composite structure prepared according to Preparation Example 3, the composite negative active material (Al₂O₃@Gr composite-coated silicon composite structure) prepared according to Example 1, and the SiO prepared according to Comparative Example 5 x (0<x<2) and the XPS spectra of the composite negative active material (Al₂O₃@Gr composite-coated SiO prepared according to Example 8 x (0<x<2)) are shown in Figures 2A to 3D .

[0282] As shown in Figures 2A to 2D , compared with the silicon composite structure (bare SCN) prepared according to Preparation Example 3, in the case of the composite negative active material (SCN GB) prepared according to Example 1, the size of the carbon peak is partially reduced, the size of the oxygen peak is increased, the size of the silicon peak is partially reduced, and the size of the aluminum peak is significantly increased. Accordingly, it is confirmed that the composite including aluminum and oxygen is coated on the surface of the silicon composite structure.

[0283] As shown in Figures 3A to 3D , compared with the SiO prepared according to Comparative Example 5 x (0<x<2) (bare SiO x ), in the case of the composite negative active material (SiO x GB) prepared according to Example 8, the size of the carbon peak is partially reduced, the size of the oxygen peak is increased, the size of the silicon peak is partially reduced, and the size of the aluminum peak is significantly increased. Accordingly, it is confirmed that the composite including aluminum and oxygen is coated on the surface of the silicon composite structure.

[0284] The amounts of elements obtained from the XPS spectra of the silicon composite structure prepared according to Preparation Example 3, the composite negative active material prepared according to Example 1, the SiO prepared according to Comparative Example 5 x (0<x<2) and the composite negative active material prepared according to Example 8 are shown in Table 2.

[0285] [Table 2]

[0286]

[0287] As shown in Table 2, the silicon composite structure prepared according to Preparation Example 3 and the SiO prepared according to Comparative Example 5 x (0<x<2) do not contain aluminum (Al) element.

[0288] In contrast, in Example 1 and Example 8, the amounts of aluminum (Al) element in the composite negative active material are 1.2 at% and 3.3 at%, respectively.

[0289] Evaluation Example 4: SEM, HR-TEM, and SEM-EDS Analysis

[0290] The composite negative active material (Al2O3@Gr composite-coated silicon composite structure) prepared according to Example 1 and the composite negative active material (Al2O3@Gr composite-coated SiO) prepared according to Example 8 were analyzed using a scanning electron microscope (SEM), a high-resolution transmission electron microscope, and SEM-energy dispersive X-ray spectroscopy (EDS) x (0<x<2)). For the SEM-EDS analysis, FEI Titan 80-300 from Philips was used.

[0291] The composite prepared according to Preparation Example 1 shows a structure in which Al2O3 particles and Al2O as a reduction product thereof z (0<z<3) particles are embedded in graphene. It is found that the graphene layer is located outside one or more particles selected from Al2O3 particles and Al2O z (0<z<3) particles. One or more particles selected from Al2O3 particles and Al2O z (0<z<3) particles are uniformly distributed. At least one of the Al2O3 particles and the Al2O z (0<z<3) particles has a particle size of about 20 nm. The particle size of the composite prepared according to Preparation Example 1 is about 50 nm to about 200 nm.

[0292] It has been confirmed that in the composite negative active materials prepared according to Example 1 and Example 8, the shell formed by the composite including graphene is disposed on the silicon composite structure core or the SiO x (0<x<2) core.

[0293] SEM-EDS mapping analysis was performed on the composite negative active materials prepared according to Example 1 and Example 8.

[0294] Figure 4A The SEM image of the composite negative active material of Example 1 is shown. Figure 4B shows the SEM-EDS mapping image of the composite negative active material of Example 1.

[0295] As shown Figure 4B in the figure, it is confirmed that aluminum (Al) is distributed on the surface of the composite negative active material of Example 1.

[0296] Figure 4C shows the SEM image of the composite negative active material of Example 8. Figure 4D shows the SEM-EDS mapping image of the composite negative active material of Example 8.

[0297] As shown Figure 4D in the figure, it is confirmed that aluminum (Al) is distributed on the surface of the composite negative active material of Example 8.

[0298] It has been confirmed that in the composite negative active materials prepared according to Example 1 and Example 8, the composite prepared according to Preparation Example 1 is uniformly coated on the silicon composite structure core or SiO x (0<x<2) core to form a shell.

[0299] Evaluation Example 5: Charge / Discharge Characteristics Test at Room Temperature (25℃)

[0300] Each of the lithium batteries fabricated in Examples 9 to 16 and Comparative Examples 6 to 10 was charged at 25°C with a constant current of 0.1C rate until the voltage reached 4.5V (vs. Li), then the current was cut off at a rate of 0.02C while the voltage was maintained at 4.5V in a constant voltage mode. Subsequently, each lithium battery was discharged with a constant current of 0.1C rate until the voltage reached 2.75V (vs. Li) (formation cycle).

[0301] Each lithium battery that had undergone the formation cycle was charged at 25°C with a constant current of 0.2C rate until the voltage reached 4.5V (vs. Li), then the current was cut off at a rate of 0.02C while the voltage was maintained at 4.5V in a constant voltage mode. Subsequently, each lithium battery was discharged with a constant current of 0.2C rate until the voltage reached 2.75V (vs. Li) (the 1st cycle). This cycle was repeated 50 times under the same conditions up to the 50th cycle.

[0302] In all charge / discharge cycles, a 10-minute rest period was provided after each charge / discharge cycle. Some results of the charge-discharge experiments at room temperature are shown in Table 3 below. The initial efficiency is defined by Equation 1 below, and the capacity retention rate is defined by Equation 2.

[0303] <Equation 1>

[0304] Initial efficiency [%] = [Discharge capacity during formation cycle / Charge capacity during formation cycle] × 100%

[0305] Equation 2

[0306] Capacity retention rate [%] = [Discharge capacity at 50th cycle / Discharge capacity at 1st cycle] × 100%

[0307] [Table 3]

[0308]

[0309]

[0310] As shown in Table 3, the lithium batteries of Examples 9 to 16 have improved lifespan characteristics compared to the lithium batteries of Comparative Examples 6 to 10.

[0311] The improved lifetime properties were determined to be due to the suppression of the internal resistance of the lithium battery by inhibiting the formation of a solid electrolyte membrane (SEI) on the surface and / or inside the negative electrode active material through composite coating.

[0312] By using a composite negative electrode active material coated with a composite, the lithium batteries of Examples 9 to 12 have improved lifespan characteristics.

[0313] In the case of the lithium battery in Example 13, the lifespan characteristics were further improved by using a composite negative electrode active material that includes carbon nanotubes in addition to the composite.

[0314] Compared to the lithium batteries of Examples 9 to 13, the lithium battery of Example 14 has relatively poor life characteristics because the coating thickness is increased by using aluminum oxide with a particle size of 200 nm.

[0315] The lithium battery in Comparative Example 7 includes a composite negative electrode active material in which a simple mixture of aluminum oxide and graphene is coated on a core, and a uniform coating is not obtained on the core due to the aggregation of graphene.

[0316] In the lithium battery of Comparative Example 8, no coating was formed on the silicon composite structure because a composite and silicon composite structure were used as the negative electrode active material.

[0317] Although not shown in the table, the lithium battery of Example 17 has improved lifespan characteristics compared to the lithium battery of Comparative Example 11.

[0318] Evaluation Example 6: Evaluation of High-Rate Charging Characteristics at Room Temperature

[0319] Each of the lithium-ion batteries manufactured in Examples 9 to 17 and Comparative Examples 6 to 10 was charged at 25°C with a constant current at a rate of 0.1C until the voltage reached 4.5V (relative to Li), and then cut off with a current at a rate of 0.02C while maintaining the voltage at 4.5V in a constant voltage mode. Subsequently, each lithium-ion battery was discharged with a constant current at a rate of 0.2C until the voltage reached 2.75V (relative to Li) (formation cycling).

[0320] Each lithium-ion battery that has undergone formation cycling is charged at 25°C with a constant current at a rate of 0.2C until the voltage reaches 4.5V (relative to Li), and then cut off with a current at a rate of 0.02C while maintaining the voltage at 4.5V in constant voltage mode. Subsequently, each lithium-ion battery is discharged at a constant current at a rate of 0.2C until the voltage reaches 2.75V (relative to Li) (Cycle 1).

[0321] Each lithium-ion battery that had undergone its first cycle was charged at 25°C with a constant current at a rate of 0.5C until the voltage reached 4.5V (relative to Li), and then cut off with a current at a rate of 0.02C while maintaining the voltage at 4.5V in constant voltage mode. Subsequently, each lithium-ion battery was discharged at a constant current at a rate of 0.2C until the voltage reached 2.8V (relative to Li) (second cycle).

[0322] Each lithium battery that had undergone its second cycle was charged at 25°C with a constant current at a rate of 1.0C until the voltage reached 4.5V (relative to Li), then disconnected with a current at a rate of 0.02C while maintaining the voltage at 4.5V in constant voltage mode. Subsequently, each lithium battery was discharged at a constant current at a rate of 0.2C until the voltage reached 2.8V (relative to Li) (third cycle).

[0323] Each lithium-ion battery that had undergone its third cycle was charged at 25°C with a constant current at a rate of 2.0C until the voltage reached 4.5V (relative to Li), then disconnected with a current at a rate of 0.02C while maintaining the voltage at 4.5V in constant voltage mode. Subsequently, each lithium-ion battery was discharged at a constant current at a rate of 0.2C until the voltage reached 2.8V (relative to Li) (fourth cycle).

[0324] Each lithium-ion battery that had undergone its fourth cycle was charged at 25°C with a constant current at a rate of 3.0C until the voltage reached 4.5V (relative to Li), then disconnected with a current at a rate of 0.02C while maintaining the voltage at 4.5V in constant voltage mode. Subsequently, each lithium-ion battery was discharged at a constant current at a rate of 0.2C until the voltage reached 2.8V (relative to Li) (fifth cycle).

[0325] A 10-minute stop time was provided after each charge / discharge cycle in all charge / discharge cycles. Some results of the high-rate charging characteristics experiments at room temperature are shown in Table 4. The high-rate characteristics are defined by Equation 3 below.

[0326] Equation 3

[0327] High rate performance [%] = [3.0C rate charging capacity (5th cycle charging capacity) / 0.1C rate charging capacity (formation cycle charging capacity)] × 100%

[0328] [Table 4]

[0329] High magnification characteristics [%) Comparison Example 6: Bare Silicon Composite Structure (Uncoated) 51.2 <![CDATA[Example 9: 1 wt% Al₂O₃@Gr Coating / Silicon Composite Structure Core]]> 54.1 <![CDATA[Comparative Example 10: Bare SiO x (no coating)]]> 51.4 <![CDATA[Example 16: 1 wt% Al₂O₃@Gr Coating / SiO x Core]]> 54.7

[0330] As shown in Table 4, compared with the lithium batteries of Comparative Example 6 and Comparative Example 10 without coating, the lithium batteries of Example 9 and Example 16 coated with the composite of Preparation Example 1 have improved high-rate characteristics.

[0331] Evaluation Example 7: Evaluation of the expansion rate of the negative electrode at high temperature (55℃)

[0332] Each of the lithium-ion batteries manufactured in Examples 9 to 16 and Comparative Examples 6 to 10 was charged at 25°C with a constant current at a rate of 0.1C until the voltage reached 4.4V (relative to Li), and then cut off with a current at a rate of 0.05C while maintaining the voltage at 4.4V in a constant voltage mode. Subsequently, each lithium-ion battery was discharged at a constant current at a rate of 0.1C until the voltage reached 2.8V (relative to Li) (formation cycling).

[0333] The lithium battery that has undergone formation cycle is charged at 25°C with a constant current at a rate of 0.7C until the voltage reaches 4.5V (relative to Li), and then the charge is cut off.

[0334] Then, while the charged lithium battery underwent float charging at a constant voltage of 4.5V (relative to Li), the expansion rate of the negative electrode at 55°C was measured after 7, 10, 14, 17, and 20 days. Some results are shown in Table 5. The expansion rate of the negative electrode is expressed by Equation 4.

[0335] Equation 4

[0336] Thickness expansion rate (%) = [(Thickness of the negative electrode after 20 days of storage - Thickness of the negative electrode before assembly) / Thickness of the negative electrode before assembly] × 100%

[0337] "Thickness of the negative electrode before assembly" refers to the thickness of the negative electrode measured before assembling the lithium battery.

[0338] "Thickness of the negative electrode after 20 days of storage" refers to the thickness of the negative electrode measured after the lithium battery is removed from the oven after being stored for 20 days.

[0339] Table 5

[0340] Negative electrode expansion rate [%) Comparison Example 6: Bare Silicon Composite Structure (Uncoated) 12.2 <![CDATA[Example 9: 1 wt% Al₂O₃@Gr Coating / Silicon Composite Structure Core]]> 9.3 <![CDATA[Comparative Example 10: Bare SiO x (no coating)]]> 7.6 <![CDATA[Example 16: 1 wt% Al₂O₃@Gr Coating / SiO x Core]]> 4.1

[0341] As shown in Table 5, the expansion rate of the negative electrode of the lithium battery in Example 9 is significantly less than that of the negative electrode of the lithium battery in Comparative Example 6.

[0342] The expansion rate of the negative electrode of the lithium battery in Example 16 is significantly less than that of the negative electrode of the lithium battery in Comparative Example 10.

[0343] The reduction in expansion rate was determined to be due to the composite coating significantly reducing side reactions between the negative electrode active material and the electrolyte, thereby inhibiting the formation of a thick solid electrolyte interphase (SEI) film.

[0344] According to one aspect, since the composite negative electrode active material includes a shell comprising a first metal oxide and a first carbonaceous material, the cycle characteristics of the lithium battery are improved and its volume change is suppressed.

[0345] It should be understood that the embodiments described herein are to be considered in a descriptive sense only and not for limiting purposes. The description of features or aspects within each embodiment should generally be considered applicable to other similar features or aspects in other embodiments. Although one or more embodiments have been described with reference to figures, it will be understood by those skilled in the art that various changes in form and detail may be made therein without departing from the spirit and scope of the disclosure as defined by the appended claims.

Claims

1. A composite negative electrode active material, said composite negative electrode active material comprising: nuclear; as well as A shell, located on the surface of the core and conforming to the surface of the core, The core includes silicon-containing structures, silicon-containing compounds, or combinations thereof. The shell comprises at least one first metal oxide represented by the formula M a O b wherein 0 < a < 3, 0 < b < 4, and when a is 1, 2, or 3, b is not an integer; and a first carbonaceous material, and The at least one first metal oxide is located in the matrix of the first carbonaceous material, and M is at least one metal selected from groups 2 to 13, 15 and 16 of the periodic table. The first carbonaceous material is a crystalline carbonaceous material. wherein the structure comprising silicon comprises a silicon composite structure and the compound comprising silicon comprises SiO x wherein 0 < x < 2, The silicon composite structure includes porous silicon secondary particles, and The porous silicon secondary particles are aggregates of multiple silicon composite primary particles.

2. The composite negative electrode active material according to claim 1, wherein, The silicon composite structure also includes a first carbon sheet located on the porous silicon secondary particles. in, each of the plurality of silicon composite primary particles includes silicon, silicon monoxide on the silicon, and a second carbon sheet on the silicon monoxide, wherein the silicon monoxide is SiO x , 0 < x < 2.

3. The composite negative electrode active material according to claim 1, wherein, The silicon composite structure has a porosity of 60% or less or is non-porous, and the silicon composite structure has a non-spherical shape.

4. The composite negative electrode active material according to claim 2, wherein, The first carbon sheet and the second carbon sheet are the same sheet, and The first carbon sheet and the second carbon sheet are each independently graphene, graphite, carbon fiber, graphitic carbon, graphene oxide, or a mixture thereof.

5. The composite negative electrode active material according to claim 1, wherein, The silicon-containing structure further includes a carbonaceous coating on the silicon composite structure, the carbonaceous coating comprising a first amorphous carbon. The silicon-containing structure further includes a second amorphous carbon located within the silicon composite structure, the silicon composite structure comprising porous silicon secondary particles, and the second amorphous carbon located within the pores of the porous silicon secondary particles. The first amorphous carbon and the second amorphous carbon each independently include pitch carbon, soft carbon, hard carbon, mesophase pitch carbide, calcined coke, carbon fiber or mixtures thereof.

6. The composite negative electrode active material according to claim 1, wherein, The at least one first metal oxide comprises a first metal, and the first metal comprises at least one selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb and Se.

7. The composite negative electrode active material according to claim 1, wherein, The at least one first metal oxide includes at least one selected from the following substances: Al2O z , where 0<z<3; NbO x , where 0<x<2.5; MgO x , where 0<x<1; Sc2O z , where 0<z<3; TiO y , where 0<y<2; ZrO y , where 0<y<2; V2O z , where 0<z<3; WO y , where 0<y<2; MnO y , where 0<y<2; Fe2O z , where 0<z<3; Co3O w , where 0<w<4; PdO x , where 0<x<1; CuO x , where 0<x<1; AgO x , where 0<x<1; ZnO x , where 0<x<1; Sb2O z , where 0<z<3; and SeO y , where 0<y<2.

8. The composite negative electrode active material according to claim 1, wherein, The shell further comprises M a O c represented second metal oxide, wherein 0<a≤3, 0<c≤4, and when a is 1, 2 or 3, c is an integer, The second metal oxide comprises the same metal as the at least one first metal oxide, and The ratio c / a of the second metal oxide has a larger value than the ratio b / a of the first metal oxide.

9. The composite negative electrode active material according to claim 8, wherein, The second metal oxide is selected from Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3, and SeO2, and The first metal oxide is a reduction product of the second metal oxide.

10. The composite negative electrode active material according to claim 8, wherein, The particle size is selected from at least one of the first metal oxide and the second metal oxide, and is between 1 nm and 100 nm.

11. The composite negative electrode active material according to claim 8, wherein, The shell comprises the first carbonaceous material protruding from the surface of at least one of the first metal oxide and the second metal oxide, and The thickness of the shell is 1 nm to 5 μm.

12. The composite negative electrode active material according to claim 8, wherein, The shell comprises at least one selected from a composite comprising the first metal oxide and the first carbonaceous material, and a product obtained by grinding the composite. The amount of at least one selected from the composite comprising the first metal oxide and the first carbonaceous material and the product obtained by grinding the composite is from 0.1 wt% to 5 wt% of the total weight of the composite negative electrode active material.

13. The composite negative electrode active material according to claim 12, wherein, The first carbonaceous material has a branched structure, and the first metal oxide is distributed within the branched structure. The branched structure comprises multiple first carbonaceous material particles in contact with each other.

14. The composite negative electrode active material according to claim 12, wherein, The first carbonaceous material has at least one structure selected from spherical structures, helical structures of multiple spherical structures connected to each other, and cluster structures of multiple spherical structures aggregated together. The first metal oxide is distributed in the spherical structure, which has a size of 50 nm to 300 nm; the helical structure has a size of 500 nm to 100 μm; and the cluster structure has a size of 0.5 mm to 10 mm. The composite is a wrinkled multifaceted spherical or planar structure, and at least one of the first metal oxide and the second metal oxide is distributed inside or on the surface of the wrinkled multifaceted spherical or planar structure. The first carbonaceous material extends from the first metal oxide by a distance of 10 nm or less and includes at least 1 to 20 layers of the first carbonaceous material, and the total thickness of the first carbonaceous material is 0.6 nm to 12 nm.

15. The composite negative electrode active material according to claim 1, wherein, The shell further includes a second carbonaceous material comprising fibrous carbon, and the second carbonaceous material includes at least one selected from carbon nanofibers and carbon nanotubes. The second carbonaceous material has a length of 1000 μm or less, and a diameter of 50 nm or less. The amount of the second carbonaceous material is 0.001 wt% to 5 wt% of the total weight of the composite negative electrode active material.

16. The composite negative electrode active material according to claim 1, wherein, The specific surface area of ​​the composite negative electrode active material is 1m². 2 / g to 100m 2 / g, and The composite negative electrode active material has an average particle size D50 of 1 μm to 30 μm, a D10 of 0.1 μm to 10 μm, and a D90 of 10 μm to 50 μm.

17. A negative electrode comprising the composite negative electrode active material according to any one of claims 1 to 16.

18. A negative electrode, said negative electrode comprising: Dry composite negative electrode active material, dry conductive material and dry binder, among which, The dry composite negative electrode active material includes: nucleus; and A shell, located on the surface of the core and conforming to the surface of the core, wherein, The core includes silicon-containing structures, silicon-containing compounds, or combinations thereof. The shell comprises: at least one first metal oxide, represented by formula M a O b wherein 0<a≤3, 0<b<4, and when a is 1, 2 or 3, b is not an integer; and a first carbonaceous material, and The at least one first metal oxide is located in the matrix of the first carbonaceous material, and M is at least one metal selected from groups 2 to 13, 15 and 16 of the periodic table. The first carbonaceous material is a crystalline carbonaceous material. The silicon-containing structure includes a silicon composite structure, and the silicon-containing compound includes SiO₂. x , of which 0 <x<2, The silicon composite structure includes porous silicon secondary particles, and The porous silicon secondary particles are aggregates of multiple silicon composite primary particles.

19. A lithium battery, said lithium battery comprising: A positive electrode; a negative electrode according to claim 17; and an electrolyte disposed between the positive electrode and the negative electrode.

Citation Information

Patent Citations

  • Negative active material, lithium secondary battery including the material and method for manufacturing the material

    CN111326729A

  • Silicon-based negative active material, preparing method of preparing same and rechargeable lithium battery including same

    US20140057176A1