A silver catalyst and its preparation method and application

By pretreating the porous alumina support with nitrogen-containing hydrogen peroxide solution, uniformly distributing silver particles, the problem of insufficient activity and stability of traditional silver catalysts is solved, and the catalytic efficiency of ethylene oxidation is improved.

CN116196923BActive Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111455977.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-01
Publication Date
2024-12-06
Estimated Expiration
2041-12-01

AI Technical Summary

Technical Problem

In the process of ethylene oxide production of traditional silver catalysts, the silver particles are insufficient in size and distribution uniformity, resulting in low activity, selectivity and stability, making it difficult to improve the performance of the catalyst.

Method used

The porous alumina support is pretreated with nitrogen-containing aqueous hydrogen peroxide solution to increase the roughness of the support surface, thereby evenly distributing silver particles, preventing them from aggregating and migrating, and improving catalyst performance.

Benefits of technology

It significantly improves the catalytic activity and stability of silver catalysts, and is especially suitable for ethylene oxide production reactions, which improves economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003386657970000111
    Figure BDA0003386657970000111
  • Figure BDA0003386657970000121
    Figure BDA0003386657970000121
Patent Text Reader

Abstract

The present invention belongs to the field of industrial catalysts, and relates to a silver catalyst and a preparation method and application thereof. The silver catalyst comprises the following components: i. a pretreated porous alumina carrier; and ii. silver loaded on the pretreated porous alumina carrier, and one or more of an alkali metal, an alkaline earth metal, rhenium and a coordinating agent of rhenium; the pretreatment is carried out with a nitrogen-containing hydrogen peroxide solution. The silver catalyst of the present invention has suitable or high catalytic activity, and at the same time has significantly improved stability, and is particularly suitable for the reaction of producing ethylene oxide by ethylene oxidation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of industrial catalysts, and in particular, relates to a silver catalyst and a preparation method thereof, as well as application of the silver catalyst in producing ethylene oxide by epoxidation of ethylene. Background Art

[0002] Under the action of silver catalyst, ethylene oxidation mainly produces ethylene oxide, and at the same time, side reactions occur to produce carbon dioxide and water, etc. Among them, activity, selectivity and stability are the main performance indicators of silver catalysts. The so-called activity refers to the reaction temperature required when the ethylene oxide production process reaches a certain reaction load. The lower the reaction temperature, the higher the activity of the catalyst. The so-called selectivity refers to the ratio of the number of moles of ethylene converted into ethylene oxide to the total number of moles of ethylene in the reaction. The so-called stability is expressed as the rate of decrease of activity and selectivity. The smaller the rate of decrease, the better the stability of the catalyst. In the process of ethylene oxidation to produce ethylene oxide, the use of high-activity, high-selectivity and good-stability silver catalysts can greatly improve economic benefits. Therefore, the manufacture of high-activity, high-selectivity and good-stability silver catalysts is the main direction of silver catalyst research. In addition to the composition and preparation method of the catalyst, the performance of the silver catalyst is also closely related to the performance and preparation method of the carrier used in the catalyst.

[0003] The preparation method of the silver catalyst mainly includes two processes: preparing a porous carrier (such as alumina) and applying active components and additives to the carrier.

[0004] Among them, the carrier needs to provide a certain surface load active component, and the active component is evenly dispersed thereon. The silver catalyst generally selects α-alumina as a carrier. The main method of its preparation is as follows: a binder and various additives are added to the alumina powder raw material, mixed and kneaded evenly, and then extruded into blanks of different shapes (Raschig rings, spherical particles, porous columns, saddles, etc.), and finally high-temperature sintering to make porous heat-resistant α-alumina carrier products, as described in US 5063195, US5703001 and US 5801259, etc. In the preparation process of the silver catalyst carrier, auxiliary agents are often added to improve the performance of the carrier. For example, US5100859A proposes that adding alkaline earth metals, SiO2 and zirconium oxide to the alumina carrier can improve the performance of the silver catalyst.

[0005] The application of active components and additives to the carrier is generally achieved by the impregnation activation method in industry. First, a silver-ammonia impregnation solution of a certain concentration is prepared with silver salt, various additives and organic amines to make Ag ions react with organic amines to generate silver-organic amine complex ions; then the carrier is immersed in the impregnation solution for a sufficient time, so that the silver-amine complex ions and various additive ions are impregnated to the carrier surface with the solution; after leaching, it is finally placed in an activation belt for activation. During the activation process, various silver-containing impregnation components on the carrier surface are heated and gradually decomposed, and silver ions are reduced to elemental silver, and particles of tens to hundreds of nanometers are formed on the carrier surface, thereby obtaining a finished silver catalyst.

[0006] The uniformity of the size of silver particles and the uniformity of their distribution have an important impact on the performance of silver catalysts. The gradual migration and growth of silver particles will lead to a decrease in the activity, stability, life and other properties of the catalyst. Therefore, slowing down the migration and growth of silver particles can improve the performance of the silver catalyst, especially the stability. The above-mentioned traditional industrial method for preparing silver catalysts has limited improvement in the size and distribution of silver particles. Silver particles are also prone to agglomeration and growth during the use of silver catalysts, so the improvement brought to the activity and selectivity of the catalyst is still very limited. Summary of the invention

[0007] In view of the above-mentioned state of the prior art, the inventors have conducted extensive and in-depth research in the field of silver catalysts and their preparation processes. As a result, it is found that the porous alumina carrier can be immersed in a nitrogen-containing hydrogen peroxide solution to achieve etching of the carrier, increase the roughness of the carrier surface, and thereby improve the uniformity of the size and distribution of the silver particles, effectively prevent the aggregation and growth of the silver particles, thereby effectively improving the performance of the silver catalyst.

[0008] The first aspect of the present invention provides a silver catalyst comprising the following components:

[0009] i. a pretreated porous alumina support; and

[0010] ii. silver supported on the pretreated porous alumina support, and optionally one or more of an alkali metal, an alkaline earth metal, rhenium and a synergistic promoter of rhenium;

[0011] The pretreatment is carried out using a nitrogen-containing hydrogen peroxide solution.

[0012] The second aspect of the present invention provides a method for preparing the above-mentioned silver catalyst, comprising the following steps:

[0013] a. soaking the untreated porous alumina support with a nitrogen-containing hydrogen peroxide solution;

[0014] b. performing solid-liquid separation on the mixture obtained in step a, and drying the obtained solid phase to obtain the pretreated porous alumina support;

[0015] c. impregnating the pretreated porous alumina support with a silver-containing impregnation solution to obtain a solid-liquid mixture;

[0016] d. separating the solid-liquid mixture obtained in step c, and drying the resulting solid phase;

[0017] e. Activating the dried solid phase obtained in step d to obtain the silver catalyst.

[0018] The third aspect of the present invention provides the use of the silver catalyst in the production of ethylene oxide by epoxidation of ethylene.

[0019] The silver catalyst of the invention has suitable or higher catalytic activity and significantly improved stability, and is particularly suitable for the reaction of producing ethylene oxide by ethylene oxidation.

[0020] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION

[0021] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0022] The present invention provides a silver catalyst comprising the following components:

[0023] i. a pretreated porous alumina support; and

[0024] ii. silver supported on the pretreated porous alumina support, and optionally one or more of an alkali metal, an alkaline earth metal, rhenium and a synergistic promoter of rhenium;

[0025] The pretreatment is carried out using a nitrogen-containing hydrogen peroxide solution.

[0026] According to a preferred embodiment of the present invention, the pretreatment step comprises:

[0027] a. soaking the untreated porous alumina support with a nitrogen-containing hydrogen peroxide solution;

[0028] b. subjecting the mixture obtained in step a to solid-liquid separation, and drying the obtained solid phase to obtain the pretreated porous alumina carrier.

[0029] According to some preferred embodiments of the present invention, the nitrogen-containing hydrogen peroxide solution is a mixed solution of a nitrogen-containing solution and hydrogen peroxide. The nitrogen in the nitrogen-containing hydrogen peroxide solution can come from organic amines, ammonia water, ammonium salts, various compounds containing amide groups, polymers, etc. Specifically, the nitrogen-containing solution includes but is not limited to organic amines, ammonia water, NH4+ Preferably, the nitrogen-containing solution is at least one of ethylenediamine, ethanolamine, ammonia water, ammonium fluoride aqueous solution, and NH4HCO3 aqueous solution.

[0030] According to some preferred embodiments of the present invention, the weight of nitrogen in the nitrogen-containing hydrogen peroxide solution accounts for 0.01-10 weight % of the total weight of the solution, preferably, the weight of nitrogen in the nitrogen-containing hydrogen peroxide solution accounts for 0.02-5 weight % of the total weight of the solution, for example, 0.03 weight %, 0.05 weight %, 0.08 weight %, 0.1 weight %, 0.2 weight %, 0.5 weight %, 0.8 weight %, 1 weight %, 2 weight %, 3 weight %, 4 weight %. The weight of hydrogen peroxide accounts for 0.01-10 weight % of the total weight of the solution, preferably, the weight of hydrogen peroxide accounts for 0.05-8 weight % of the total weight of the solution, for example, 0.1 weight %, 0.2 weight %, 0.5 weight %, 0.8 weight %, 1 weight %, 2 weight %, 3 weight %, 4 weight %, 5 weight %, 6 weight %, 7 weight %.

[0031] The present invention has no particular limitation on the untreated porous alumina carrier, and a conventional porous alumina carrier in the art may be used, preferably having the following characteristics: α-A12O3 content>85%, preferably α-A12O3 content>90%; particle crushing strength>20N, preferably 30-150N; specific surface area of ​​0.2-7.0m 2 / g, preferably 0.5-6.0m 2 / g; water absorption>30%, preferably>40%; and, pore volume is 0.30-0.70ml / g, preferably 0.35-0.50ml / g.

[0032] According to the present invention, the catalyst can be prepared by a method comprising the following steps:

[0033] a. soaking the untreated porous alumina support with a nitrogen-containing hydrogen peroxide solution;

[0034] b. performing solid-liquid separation on the mixture obtained in step a, and drying the obtained solid phase to obtain the pretreated porous alumina support;

[0035] c. impregnating the pretreated porous alumina support with a silver-containing impregnation solution to obtain a solid-liquid mixture;

[0036] d. separating the solid-liquid mixture obtained in step c, and drying the resulting solid phase;

[0037] e. Activating the dried solid phase obtained in step d to obtain the silver catalyst.

[0038] During the soaking process, the solution should cover all the carriers, and the amount should be more than twice the weight of the carriers. At the same time, stirring, ultrasound, etc. can be performed to allow the carrier to fully contact with the solution. In order to make the soaking more uniform, the soaking time should not be less than 10 minutes.

[0039] Next, the carrier should be removed, drained, and the solid phase should be dried. The drying temperature should be between 80°C and 800°C, and the drying time should be no less than 1 hour. If the drying temperature is low, the drying time should be extended accordingly.

[0040] After the carrier treatment is completed, the treated porous alumina carrier is impregnated with a silver-containing impregnation solution, and then the silver-impregnated carrier is taken out and activated to obtain the final product.

[0041] According to the method of the present invention, in order to ensure uniform and sufficient loading of silver, the carrier is preferably evacuated in advance.

[0042] According to the method of the present invention, activation can be carried out in air or inert gas. For example, the dried solid phase can be activated in a flow of flowing air or inert gas such as nitrogen, argon, etc. at 180-700° C., preferably 200-500° C., and the activation time is usually at least 2 minutes, such as 2-120 minutes, preferably 2-60 minutes. In order to ensure that the catalyst has a high activity, the activation temperature is preferably not higher than 500° C.

[0043] According to the method of the present invention, the impregnation solution includes, in addition to the silver compound, at least one selected from the group consisting of alkali metal additives, alkaline earth metal additives, rhenium additives and rhenium synergistic additives.

[0044] According to the method of the present invention, the silver element contained in the impregnation solution comes from a silver compound, and the silver compound can be any silver compound suitable for preparing a silver catalyst for ethylene oxide production. The present invention preferably uses at least one of silver oxide, silver nitrate and silver carbonate. According to the present invention, the impregnation solution usually contains an organic amine compound, and the organic amine compound used can be any organic amine compound suitable for preparing a silver catalyst, as long as the organic amine compound can form a silver amine complex with the silver compound. For the present invention, pyridine, butylamine, ethylenediamine, 1,3-propylenediamine, ethanolamine, etc. or a mixture thereof are preferably used.

[0045] According to the present invention, the alkali metal additive can be a compound of lithium, sodium, potassium, rubidium or cesium (such as nitrate, sulfate and hydroxide) or a mixture thereof, preferably cesium nitrate, lithium nitrate and / or potassium hydroxide. The alkaline earth metal additive can be one or more compounds of magnesium, calcium, strontium and barium, such as one or more oxides, oxalates, sulfates, acetates and nitrates of the alkaline earth metal elements, preferably a barium compound and / or a strontium compound, such as barium acetate and / or strontium acetate.

[0046] According to the present invention, the rhenium promoter may be rhenium oxide, perrhenic acid, perrhenate, or a mixture thereof, preferably perrhenic acid and / or perrhenate, such as perrhenic acid, cesium perrhenate and / or ammonium perrhenate. In addition to the silver compound, organic amine, optional alkali metal promoter, optional alkaline earth metal promoter and optional rhenium promoter, a co-promoter of the rhenium promoter may be added to the impregnation solution to further improve the activity, selectivity and stability of the obtained silver catalyst. The co-promoter of the rhenium promoter in the present invention may be one or more selected from chromium compounds, molybdenum compounds, tungsten compounds and boron compounds.

[0047] According to the present invention, the “optional” means that it may or may not be contained, such as the optional alkali metal means that the catalyst may or may not contain an alkali metal.

[0048] According to a specific embodiment of the present invention, the step of preparing a silver-containing impregnation solution comprises: dissolving silver carbonate in an aqueous solution of an organic amine such as pyridine, butylamine, ethylenediamine, 1,3-propylenediamine, ethanolamine or a mixture thereof to prepare an impregnation solution. Then, the porous α-alumina carrier is impregnated with the obtained impregnation solution for 10-60 minutes under a vacuum degree of less than 0.1 atmosphere, drained and dried, the drying temperature can be selected between room temperature and 100°C, and the drying time can be selected for 1-96 hours. Finally, the temperature is kept in the range of 200-500°C in air or inert gas for 1-120 minutes, preferably 2-60 minutes, for activation. Silver oxide, silver nitrate, etc. can also be used instead of silver carbonate.

[0049] In a specific embodiment of the silver catalyst, the alkali metal is one or more selected from lithium, sodium, potassium, rubidium and cesium; preferably cesium and / or potassium, most preferably cesium. The alkaline earth metal is one or more selected from magnesium, calcium, strontium and barium, preferably strontium and / or barium. The synergistic auxiliary element of rhenium is selected from at least one of chromium, molybdenum, tungsten and boron.

[0050] According to the silver catalyst of the present invention, silver is dispersed on the surface and pores of the alumina carrier. In order to control the economic efficiency on the basis of ensuring the catalyst performance, based on the total weight of the silver catalyst, the content of silver element in the silver catalyst is 1-35wt%, preferably 5-30wt%; the content of nitrogen element is 1-1500ppm, preferably 10-1000ppm; the content of alkali metal element is 0-2000ppm, preferably 10-1500ppm; the content of rhenium element is 0-1500ppm, preferably 10-1000ppm; the content of synergistic auxiliary element of rhenium is 0-1000ppm, preferably 10-500ppm.

[0051] The silver catalyst of the invention can be applied to the reaction of producing ethylene oxide by epoxidation of ethylene.

[0052] The present invention will be further described below in conjunction with embodiments, but the scope of the present invention is not limited to these embodiments.

[0053] Determination of catalyst performance: The activity and selectivity of various silver catalysts of the present invention are tested by a laboratory microreactor (hereinafter referred to as "microreactor") evaluation device. The reactor used in the microreactor evaluation device is a stainless steel reaction tube with an inner diameter of 4 mm, and the reaction tube is placed in a heating jacket. The filling volume of the catalyst is 1 mL, and there is an inert filler at the bottom so that the catalyst bed is located in the constant temperature zone of the heating jacket. The activity and selectivity determination conditions adopted by the present invention are as follows: reaction gas composition, ethylene (C2H4), 28.0±1.0 mol%; oxygen (O2), 7.4±0.2 mol%; carbon dioxide (CO2), <5.0 mol%; stabilizing gas (N2), balance; inhibitor ethylene dichloride, 0.1-2.0 ppm; space velocity, 8000 / h; reactor outlet EO concentration, 3.0 mol%; space-time yield, 470 kg EO / m 3 Cat. / h.

[0054] When the above reaction conditions are stably reached, the gas composition at the reactor inlet and outlet is continuously measured. The selectivity is calculated according to the following formula after volume shrinkage correction is performed on the measured results:

[0055] Selectivity

[0056] Wherein, ΔEO is the difference in ethylene oxide concentration between the reactor outlet gas and the inlet gas, ΔCO2 is the difference in carbon dioxide concentration between the reactor outlet gas and the inlet gas, and the average of more than 10 groups of test data is taken as the test result of the day.

[0057] The present invention will be further described below in conjunction with embodiments, but the scope of the present invention is not limited to these embodiments.

[0058] Preparation of vector A

[0059] 600g of 50-500 mesh trihydrate A12O3 and 300g of pseudo monohydrate A12O3 through a 200 mesh sieve are placed in a mixer and mixed evenly, then transferred to a kneader, 100 ml of a 20 wt% aqueous nitric acid solution is added, and kneaded into a paste that can be extruded. Extrusion molding is a single-hole Raschig ring column with an outer diameter of 8.0mm, a length of 6.0mm, and an inner diameter of 2.0mm, and dried at 80-120°C for 2 hours to reduce the free water content to less than 10 wt% to obtain a green body. Then the green body is placed in an electric furnace, and the temperature is raised from room temperature to between 1200-1500°C over 30 hours, and the temperature is kept constant at this high temperature for 1-6 hours to obtain a white α-A12O3 carrier sample A with an α-A12O3 content of >90%, a crushing strength of 140N, and a specific surface area of ​​1.1m 2 / g, water absorption is 50%, and pore volume is 0.5ml / g.

[0060] Comparative Example 1

[0061] Add 15g of ethylenediamine, 5.5g of ethanolamine and 19g of deionized water to a stirred glass flask to obtain a mixed solution. Slowly add silver carbonate to the resulting mixed solution while stirring, and keep the temperature at 15-35°C to dissolve all the silver carbonate. The amount of silver carbonate added is such that the final impregnation solution contains 24% silver by weight. Add 0.15g of cesium nitrate and 0.2g of ammonium perrhenate, and then add deionized water to make the total mass of the solution reach 100g to prepare an impregnation solution. Take 30g of carrier A and put it in a container that can be evacuated. Evacuate to a vacuum degree of less than 0.1 atmospheres, add the above impregnation solution, immerse the carrier, and keep it for 30 minutes. Then remove the excess impregnation solution by leaching. Heat the impregnated carrier in an air flow at 250°C for 5 minutes, cool it, and the silver catalyst is prepared.

[0062] Comparative Example 2

[0063] Take 30g of carrier A, soak it in 50g of 2wt% ethylenediamine aqueous solution for half an hour and ultrasonicate it at the same time, take it out and drain it, and dry it at 500℃ for 2 hours for use. Add 15g of ethylenediamine, 5.5g of ethanolamine and 19g of deionized water in a stirred glass flask to obtain a mixed solution. Slowly add silver carbonate to the obtained mixed solution under stirring, keep the temperature at 15-35℃, so that the silver carbonate is completely dissolved, and the amount of silver carbonate added makes the final impregnation solution contain 24% silver by weight. Add 0.15g of cesium nitrate and 0.2g of ammonium perrhenate, and then add deionized water to make the total mass of the solution reach 100g to prepare an impregnation solution. Put the treated carrier A into a vacuum container, evacuate it to a vacuum degree below 0.1 atmosphere, put the above impregnation solution into it, immerse the carrier, and keep it for 30 minutes. Then leaching to remove the excess impregnation solution. Heat the impregnated carrier in an air flow at 250℃ for 5 minutes, cool it, and the silver catalyst is prepared.

[0064] Comparative Example 3

[0065] Take 30g of carrier A, soak it in 50g of 2wt% hydrogen peroxide solution for half an hour and ultrasonicate it at the same time, then take out the carrier, drain it, and dry it at 500℃ for 2 hours for use. Add 15g of ethylenediamine, 5.5g of ethanolamine and 19g of deionized water in a stirred glass flask to obtain a mixed solution. Slowly add silver carbonate to the obtained mixed solution under stirring, keep the temperature at 15-35℃, so that the silver carbonate is completely dissolved, and the amount of silver carbonate added makes the final impregnation solution contain 24% by weight of silver. Add 0.15g of cesium nitrate and 0.2g of ammonium perrhenate, and then add deionized water to make the total mass of the solution reach 100g to prepare an impregnation solution. Put the treated carrier A into a vacuum container, evacuate it to a vacuum degree below 0.1 atmosphere, put the above impregnation solution into it, immerse the carrier, and keep it for 30 minutes. Then leaching to remove the excess impregnation solution. Heat the impregnated carrier in an air flow at 250℃ for 5 minutes, cool it, and the silver catalyst is prepared.

[0066] Examples 1 to 7

[0067] Example 1

[0068] Take 30g of carrier A, soak it in 50g of 0.5wt% hydrogen peroxide solution containing 2wt% ethylenediamine for half an hour and ultrasonicate it at the same time, then take out the carrier, drain it, and dry it at 500℃ for 2 hours for use. Add 15g of ethylenediamine, 5.5g of ethanolamine and 19g of deionized water in a stirred glass flask to obtain a mixed solution. Slowly add silver carbonate to the resulting mixed solution under stirring, keep the temperature at 15-35℃, so that the silver carbonate is completely dissolved, and the amount of silver carbonate added makes the final impregnation solution contain 24% by weight of silver. Add 0.15g of cesium nitrate and 0.2g of ammonium perrhenate, and then add deionized water to make the total mass of the solution reach 100g to prepare an impregnation solution. Put the treated carrier A into a vacuum container, evacuate it to a vacuum degree below 0.1 atmosphere, put the above impregnation solution into it, immerse the carrier, and keep it for 30 minutes. Then leaching to remove the excess impregnation solution. The impregnated carrier is heated in an air flow at 250°C for 5 minutes and cooled to prepare a silver catalyst. The nitrogen content of the catalyst is 40 ppm, the alkali metal content is 550 ppm, and the rhenium content is 260 ppm.

[0069] Example 2

[0070] Take 30g of carrier A, soak it in 50g of 0.1wt% hydrogen peroxide solution containing 0.5wt% ethylenediamine for half an hour and ultrasonicate it at the same time, then take out the carrier, drain it, and dry it at 150℃ for 8 hours for use. Add 15g of ethylenediamine, 5.5g of ethanolamine and 19g of deionized water in a stirred glass flask to obtain a mixed solution. Slowly add silver carbonate to the resulting mixed solution under stirring, keep the temperature at 15-35℃, so that the silver carbonate is completely dissolved, and the amount of silver carbonate added makes the final impregnation solution contain 24% by weight of silver. Add 0.15g of cesium nitrate and 0.2g of ammonium perrhenate, and then add deionized water to make the total mass of the solution reach 100g to prepare an impregnation solution. Put the treated carrier A into a vacuum container, evacuate it to a vacuum degree below 0.1 atmosphere, put the above impregnation solution into it, immerse the carrier, and keep it for 30 minutes. Then leaching to remove the excess impregnation solution. The impregnated carrier was heated in an air flow at 250° C. for 5 minutes and then cooled to prepare a silver catalyst. The nitrogen content in the catalyst was 20 ppm.

[0071] Example 3

[0072] The steps are the same as those in Example 1, except that the support is soaked in 50 g of a 0.1 wt % hydrogen peroxide solution containing 1 wt % ethanolamine for half an hour, and the nitrogen content in the catalyst is 60 ppm.

[0073] Example 4

[0074] The steps are the same as those in Example 1, except that the support is soaked in 50 g of a 0.1 wt % hydrogen peroxide solution containing 1 wt % ammonium fluoride for half an hour, and the nitrogen content in the catalyst is 70 ppm.

[0075] Example 5

[0076] The steps are the same as those in Example 1, except that the support is soaked in 50 g of a 0.1 wt % hydrogen peroxide solution containing 2.5 wt % ammonia water for half an hour, and the nitrogen content in the catalyst is 50 ppm.

[0077] Example 6

[0078] The steps are the same as those in Example 1, except that the support is soaked in 50 g of a 5 wt % hydrogen peroxide solution containing 0.1 wt % ethylenediamine for half an hour, and the nitrogen content in the catalyst is 40 ppm.

[0079] Example 7

[0080] The steps are the same as those in Example 2, except that the carrier is soaked for half an hour with 50 g of a solution containing 0.1 wt % of ethylenediamine, 0.1 wt % of ammonium fluoride, 0.1 wt % of ammonia water, and 1 wt % of hydrogen peroxide, and the nitrogen content in the catalyst is 80 ppm.

[0081] Performance Evaluation

[0082] The activity and selectivity of each catalyst sample were measured using a microreactor evaluation device under the process conditions described in the "Determination of Catalyst Performance" section above. The test results are listed in Table 1. The reaction temperature in Table 1 is the temperature at which the cumulative EO production reaches 200 T / M 3 The value of catalyst selectivity is taken when the cumulative EO production reaches 500T / M 3 The average value of the catalyst.

[0083] Table 1

[0084]

[0085]

[0086] It can be seen from Table 1 that the silver catalyst prepared from the treated carrier has better selectivity and catalytic activity than the silver catalyst prepared from the untreated carrier, and is particularly suitable for the reaction of producing ethylene oxide by ethylene oxidation.

[0087] It can be seen that the silver catalyst obtained by immersing the porous alumina carrier in a nitrogen-containing hydrogen peroxide solution can obtain significantly improved activity and selectivity when used to catalyze the oxidation of ethylene to produce ethylene oxide.

[0088] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.

[0089] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

Claims

1. A silver catalyst comprising the following components: i. a pretreated porous alumina support; and ii. silver supported on the pretreated porous alumina support, and optionally one or more of an alkali metal, an alkaline earth metal, rhenium and a synergistic promoter of rhenium; The pretreatment is carried out using a nitrogen-containing hydrogen peroxide solution; The nitrogen-containing hydrogen peroxide solution is a mixed solution of a nitrogen-containing solution and hydrogen peroxide; The nitrogen-containing solution is organic amines, ammonia water, NH4 + At least one of the ammonium salt solutions.

2. The silver catalyst according to claim 1, wherein The pre-processing steps include: a. The untreated porous alumina support was soaked in a nitrogen-containing hydrogen peroxide solution; b. subjecting the mixture obtained in step a to solid-liquid separation, and drying the obtained solid phase to obtain the pretreated porous alumina carrier.

3. The silver catalyst according to claim 1 or 2, wherein The nitrogen-containing solution is at least one of ethylenediamine, ethanolamine, ammonia water, ammonium fluoride aqueous solution, and NH4HCO3 aqueous solution.

4. The silver catalyst according to claim 1 or 2, wherein The weight of nitrogen in the nitrogen-containing hydrogen peroxide solution accounts for 0.01-10% by weight of the total weight of the solution, and the weight of hydrogen peroxide accounts for 0.01-10% by weight of the total weight of the solution.

5. The silver catalyst according to claim 4, wherein The weight of nitrogen in the nitrogen-containing hydrogen peroxide solution accounts for 0.02-5% by weight of the total weight of the solution, and the weight of hydrogen peroxide accounts for 0.05-8% by weight of the total weight of the solution.

6. The silver catalyst according to claim 2, wherein In step a, the soaking is carried out under stirring or ultrasonic conditions, and the soaking time is not less than 10 minutes.

7. The silver catalyst according to claim 2, wherein In step b, the drying temperature is 80° C.-800° C., and the drying time is not less than 1 hour.

8. The silver catalyst according to claim 1 or 2, wherein The silver catalyst is prepared by a method comprising the following steps: a. The untreated porous alumina support was soaked in a nitrogen-containing hydrogen peroxide solution; b. The mixture obtained in step a is subjected to solid-liquid separation, and the resulting solid phase is dried to obtain the pretreated porous alumina support; c. impregnating the pretreated porous alumina support with a silver-containing impregnation solution to obtain a solid-liquid mixture; d. The solid-liquid mixture obtained in step c is subjected to solid-liquid separation, and the resulting solid phase is dried; e. Activating the dried solid phase obtained in step d to obtain the silver catalyst.

9. The silver catalyst according to claim 8, wherein The silver-containing impregnation solution comprises a silver compound and at least one selected from the group consisting of an alkali metal additive, an alkaline earth metal additive, a rhenium additive, and a synergistic additive of rhenium.

10. The silver catalyst according to claim 1 or 2, wherein The untreated porous alumina carrier has the following characteristics: α-A12O3 content>85%; particle crushing strength>20N; specific surface area of ​​0.2-7.0m 2 / g; water absorption>30%; and, pore volume is 0.30-0.70mL / g.

11. The silver catalyst according to claim 10, wherein The untreated porous alumina carrier has the following characteristics: α-A12O3 content>90%; particle crushing strength of 30-150N; specific surface area of ​​0.5-6.0m 2 / g; water absorption>40%; and, pore volume of 0.35-0.50mL / g.

12. The silver catalyst according to claim 1 or 2, wherein Based on the total weight of the silver catalyst, the content of silver element in the silver catalyst is 1-35wt%; the content of nitrogen element is 1-1500ppm; the content of alkali metal element is 0-2000ppm; the content of rhenium element is 0-1500ppm; and the content of synergistic auxiliary element of rhenium is 0-1000ppm.

13. The silver catalyst according to claim 12, wherein Based on the total weight of the silver catalyst, the content of silver element in the silver catalyst is 5-30wt%; the content of nitrogen element is 10-1000ppm; the content of alkali metal element is 10-1500ppm; the content of rhenium element is 10-1000ppm; and the content of synergistic auxiliary element of rhenium is 10-500ppm.

14. The method for preparing the silver catalyst according to any one of claims 1 to 13, comprising the following steps: a. The untreated porous alumina support was soaked in a nitrogen-containing hydrogen peroxide solution; b. The mixture obtained in step a is subjected to solid-liquid separation, and the resulting solid phase is dried to obtain the pretreated porous alumina support; c. impregnating the pretreated porous alumina support with a silver-containing impregnation solution to obtain a solid-liquid mixture; d. The solid-liquid mixture obtained in step c is subjected to solid-liquid separation, and the resulting solid phase is dried; e. Activating the dried solid phase obtained in step d to obtain the silver catalyst.

15. Use of the silver catalyst according to any one of claims 1 to 13 in producing ethylene oxide by epoxidation of ethylene.