A corrosion-resistant electromagnetic protective coating, coating, preparation method and application thereof, and wind power generation equipment

By using electromagnetic protective coatings containing nitrogen compounds and oxides on offshore wind power equipment, combined with a self-cleaning layer, the problems of electrochemical corrosion and anti-electromagnetic interference of existing coatings in the marine environment are solved, and anti-electromagnetic interference and resistance to electromagnetic interference are achieved. Corrosive dual effect, suitable for offshore wind power equipment.

CN116200103BActive Publication Date: 2024-10-01CHANGPING BEIJING ELECTROMAGNETIC PROTECTION
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202310149723.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-22
Publication Date
2024-10-01
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

Existing electromagnetic protective coatings have electrochemical corrosion problems in the marine environment, cannot meet the harsh marine environment requirements, and cannot achieve both electromagnetic interference resistance and corrosion resistance.

Method used

An electromagnetic protective coating containing nitrides and oxides is used. By adjusting the ratio of nitrides and oxides, anti-electromagnetic interference properties are formed, and combined with a self-cleaning layer, a corrosion-resistant electromagnetic protective coating is prepared. The coating consists of an anti-interference layer and It consists of a self-cleaning layer with a coating thickness of 2mm and is cured at room temperature.

Benefits of technology

It achieves the dual advantages of anti-electromagnetic interference and corrosion resistance in harsh environments. It can pass high and low temperature, seawater resistance, humidity and heat resistance and other tests, and has excellent environmental corrosion resistance to meet the needs of offshore wind power equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116200103B_ABST
    Figure CN116200103B_ABST
Patent Text Reader

Abstract

The present invention discloses a corrosion-resistant electromagnetic protective coating, a coating and a preparation method and application thereof, and a wind power generation equipment. The anti-interference coating is prepared by nitride and oxide. Different anti-electromagnetic wave interference characteristics can be obtained by adjusting the ratio of nitride and oxide. The electromagnetic protective coating is obtained by mixing with an amine curing agent. A self-cleaning coating is prepared on the basis of the electromagnetic protective coating. In the operation of coating spraying, the corrosion-resistant protective coating has both corrosion resistance and anti-electromagnetic interference function, meeting the requirements of civil and military industries. The present invention also discloses an application of nitride and oxide in corrosion-resistant electromagnetic protective coating and a preparation method thereof, as well as wind power generation equipment sprayed with corrosion-resistant electromagnetic protective coating, so that the wind power generation equipment has the characteristics of anti-electromagnetic interference in harsh environments, while taking into account corrosion resistance, and has the dual advantages of anti-electromagnetic interference and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electromagnetic protective coating, a coating, a preparation method and application thereof, and a wind power generation device, and in particular to a corrosion-resistant electromagnetic protective coating, a coating, a preparation method and application thereof, and a wind power generation device. Background Art

[0002] With the development of the world economy, new energy has become the direction of development for all countries. Among them, wind power, which is radiation-free, air pollution-free and renewable, is a recognized new green and clean energy. Compared with onshore wind power, offshore wind power generation has the advantages of high wind turbine utilization, large single-unit capacity and being far away from people. At present, my country's newly added offshore installed capacity ranks first in the world, and the cumulative installed capacity accounts for 23% of the world, reaching 6.7GW, ranking third in the world after the United Kingdom and Germany. Therefore, the market capacity in this direction is huge and there is much to be done.

[0003] Wind power generation equipment generally includes blades, fans, tower bodies, and underwater foundations. 80% of these structural parts are made of metal. Metal materials have a strong reflection effect on electromagnetic waves, which greatly increases the radar scattering area and has an adverse effect on the combat performance of military radars and communication equipment. Its strong reflection can cause the receiver signal of radar communication equipment to be saturated or even destroyed, affecting the normal functioning of military equipment.

[0004] Operating environments such as high humidity, high salt fog, ultraviolet radiation, seawater immersion, and alternating dry and wet conditions in the splash zone have put forward higher requirements on the marine environment resistance of offshore wind power equipment. The main method to solve this problem is to coat the surface of wind power equipment with zinc-rich heavy anti-corrosion coating to achieve the purpose of material protection. However, this material does not have the function of resisting electromagnetic interference.

[0005] In order to achieve the requirements of being light, thin and broadband, existing electromagnetic protective coatings all use iron powder and iron alloy powder as absorbents. It is well known that iron powder and iron alloy powder will have electrochemical corrosion problems if exposed to complex marine application environments for a long time. They cannot meet the requirements of harsh marine environments and are in urgent need of improvement. Summary of the invention

[0006] The purpose of the present invention is to provide corrosion-resistant electromagnetic protective coatings, coatings, preparation methods and applications thereof, and wind power generation equipment. The electromagnetic protective coatings and wind power generation equipment used are not only resistant to electromagnetic interference, but also have corrosion resistance, thereby solving the shortcomings of the prior art.

[0007] The present invention provides the following scheme:

[0008] An electromagnetic protection coating includes a nitride and an oxide, wherein the nitride has a chemical expression as shown in Formula 1:

[0009] Formula 1: Fe α Co 1-α-β-γ-δ B β C γ D δ ;

[0010] Where: α: 0.50-0.74, β: 0.001-0.05; γ: 0.001-0.1, δ: 0.001-0.1; where the lower right subscript of the chemical formula represents the molar percentage of each component;

[0011] Fe is iron, Co is cobalt;

[0012] B is at least one of titanium, zirconium, niobium, vanadium, tungsten or molybdenum, and / or: B also includes at least one of lanthanide elements;

[0013] C is silicon or aluminum, and D is at least one of the lanthanide elements;

[0014] Oxide: has the chemical expression shown in Formula 2:

[0015] Formula 2: A3B2Fe 24 O 41 ;

[0016] Among them: Fe is iron element; O is oxygen element;

[0017] A includes barium, strontium or calcium;

[0018] B includes cobalt, zinc, manganese, copper and nickel.

[0019] A method for preparing a corrosion-resistant electromagnetic protective coating, specifically comprising:

[0020] According to the chemical expressions, nitrides and oxides are prepared;

[0021] Preparation of anti-interference coating: uniformly mixing nitride, oxide, resin and organic solvent, performing dispersion treatment, and obtaining different anti-electromagnetic wave interference properties by adjusting the ratio of nitride and oxide to form a first component having nitride and oxide;

[0022] The second component includes an amine curing agent;

[0023] Curing treatment: mixing the first component and the second component evenly, and performing curing treatment to obtain an electromagnetic protection coating;

[0024] The preparation of nitride specifically includes:

[0025] Ingredients: Use analytically pure powdered raw materials and prepare them under nitrogen protection environment according to the alloy composition requirements;

[0026] Mechanical alloying: Add the raw materials into an argon-protected high-energy ball mill for mechanical alloying;

[0027] After mechanical alloying is completed, the material is cooled to room temperature and transferred to a rotary atmosphere reactor under nitrogen protection;

[0028] Nitriding treatment: Rotary atmosphere reactor, using ammonia, nitrogen or hydrogen as nitriding source;

[0029] Passivation treatment: Mix the magnetic powder and potassium dichromate solution evenly, disperse at high speed, filter, wash with deionized water until colorless and transparent, then wash with acetone, and then dry in a vacuum drying oven for later use;

[0030] The preparation of the oxide specifically comprises:

[0031] Ingredients: Use analytically pure powdered raw materials and prepare the ingredients according to the chemical molecular formula of the oxide;

[0032] Primary ball milling: Grind and mix the raw materials using wet ball milling;

[0033] Pre-calcination: subjecting the ball-milled mixture obtained by the first ball-milling to a high-temperature solid-phase reaction;

[0034] Secondary ball milling: The crushed raw materials are ground twice using a mixed ball mill;

[0035] Sintering: subjecting the secondary ball-milled mixture to a high-temperature solid-phase reaction;

[0036] Crushing and screening: crushing and screening the sintered materials;

[0037] Also included is the preparation of self-cleaning coatings:

[0038] Filler surface treatment: Surface treatment of filler is carried out by adding 0.5wt~1wt% of KH550 silane coupling agent in a high-speed mixer;

[0039] Filler mixing: add 100 parts of polydimethylsiloxane and 10-20 parts of filler into a vacuum kneader at one time;

[0040] Dispersion treatment: add 100 parts of the above mixture into a planetary stirring disperser, and add 110-180 parts of petroleum ether;

[0041] Screen filtration: Use screen to filter the coating to obtain the third component;

[0042] Evenly mix: 100 parts by mass of the third component and 5-10 parts by mass of the fourth component are mixed and aged to generate a self-cleaning coating.

[0043] Furthermore, in the process of preparing the anti-interference coating, the nitride, oxide, resin and organic solvent are uniformly mixed and dispersed, specifically: the equipment used for the dispersion treatment is a high-speed disperser, a sand mill, a ball mill or a three-roll mill;

[0044] The amine curing agent specifically includes aliphatic amine curing agents and polyamide curing agents;

[0045] In the aging treatment step of the anti-interference coating: 100 parts by mass of the first component and 12 parts by mass of the second component are mixed evenly, and the mixture is aged for 15 minutes to obtain the electromagnetic protection coating;

[0046] Spray the cured material onto the surface of the metal material with a coating thickness of 2mm and cure at room temperature;

[0047] In the process of preparing the filler surface treatment of the self-cleaning coating, the speed of the high-speed mixer is 1000 rpm, the treatment time is 3 min to 10 min, and the filler is one or more of white carbon black, aluminum oxide, and calcium carbonate;

[0048] During the filler mixing process for the preparation of self-cleaning coatings, the temperature of the vacuum kneader is 100°C.

[0049] ~150°C, mix for 1 to 5 hours;

[0050] In the dispersion process of preparing the self-cleaning coating, the planetary stirring disperser is used for dispersion at a speed of 50 rpm for 1 h to 2 h.

[0051] Further, in the process of preparing the filler mixing of the self-cleaning coating, the vacuum kneader is maintained at a temperature of 100° C. to 150° C. and mixed for 1 hour to 5 hours;

[0052] In the dispersion process of preparing the self-cleaning coating, the planetary stirring disperser is used for dispersion at a speed of 50 rpm for 1 h to 2 h;

[0053] In the screen filtration process of preparing the self-cleaning coating, a screen of 300 to 400 mesh is used for filtering.

[0054] Furthermore, in the process of preparing the ingredients of the nitride, a laser particle size analyzer is used to detect whether the particle size meets the requirement of D50<10 μm;

[0055] In the process of preparing the mechanical alloying of nitrides, specifically: the volume of the high-energy ball mill is 1L, and tungsten carbide grinding balls are used.

[0056] Furthermore, in the process of primary ball milling for preparing the oxide, the prepared material is loaded into a drum ball mill for 24 to 48 hours, with a ball-to-material ratio of 5 to 20, and the material is dried after discharge, and the average particle size of the mixed material is tested to be less than 0.5 microns;

[0057] In the process of pre-sintering the oxide, the temperature range is 1000°C to 1350°C, and the reaction time is 2 to 8 hours;

[0058] In the process of crushing and screening the oxides, a 200-mesh standard sieve is used for grading, and the material below the 200-mesh sieve is a qualified product.

[0059] A corrosion-resistant electromagnetic protective coating is prepared by adopting the preparation method of the electromagnetic protective coating.

[0060] A corrosion-resistant electromagnetic protective coating comprises an anti-interference layer, a self-cleaning layer and a metal base layer, wherein the surface of the metal base layer is treated by a sandblasting process, and the anti-interference layer and the self-cleaning layer are sprayed with corrosion-resistant electromagnetic protective paint.

[0061] Furthermore, the anti-interference layer is arranged between the self-cleaning layer and the metal base layer.

[0062] The invention discloses an application of nitride and oxide in a corrosion-resistant electromagnetic protective coating and a preparation method thereof.

[0063] A wind power generation equipment, wherein the wind power generation equipment is sprayed with corrosion-resistant electromagnetic protective paint and / or has a corrosion-resistant electromagnetic protective coating.

[0064] Compared with the prior art, the present invention has the following advantages:

[0065] The present invention provides a corrosion-resistant electromagnetic protective paint, a coating, a preparation method and application thereof, and a wind power generation equipment, which have the characteristics of anti-electromagnetic interference in harsh environments while taking into account corrosion resistance, and have the dual advantages of anti-electromagnetic interference and corrosion resistance.

[0066] The present invention can be applied to wind power generation equipment, so that the wind power generation equipment has the characteristic of being resistant to seawater corrosion, which not only meets the anti-electromagnetic interference requirements of the wind power generation equipment, but also meets the requirements of strong corrosion resistance in the marine environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0068] Figure 1 It is a flow chart of the preparation method of corrosion-resistant electromagnetic protective coating.

[0069] Figure 2 It is a schematic diagram of the structure of the corrosion-resistant electromagnetic protective coating.

[0070] Figure 3 It is a flow chart of the overall preparation method of the corrosion-resistant electromagnetic protective coating preparation method.

[0071] Figure 4 It is a coordinate diagram of electromagnetic parameters (81wt%) corresponding to M1 in Example 5.

[0072] Figure 5 It is a coordinate diagram of the electromagnetic parameters (73wt%) corresponding to N1 in Example 5.

[0073] Figure 6 It is a coordinate diagram of the reflectivity test results in Example 5 (2mm).

[0074] Figure 7 It is a coordinate diagram of the electromagnetic parameters (73wt%) corresponding to N2 in Example 6.

[0075] Figure 8 It is a coordinate diagram of the reflectivity test results in Example 6 (2mm). DETAILED DESCRIPTION

[0076] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0077] It can be seen from the following examples that the present invention provides a seawater corrosion-resistant electromagnetic protective coating, a coating and a preparation method thereof with a composite structure. The coating is both resistant to seawater corrosion and can reduce the radar scattering area. It consists of an anti-electromagnetic interference coating and a self-cleaning layer. The anti-interference layer is composed of epoxy resin, nitride and oxide, and the self-cleaning layer has a hydrophobic self-cleaning effect. By adjusting the ratio of nitride and oxide, the anti-electromagnetic interference characteristics of the material at different frequencies can be adjusted. In addition, the coating can pass various harsh tests of environmental resistance such as high and low temperature, seawater resistance, and humidity and heat resistance, and has excellent environmental corrosion resistance.

[0078] Embodiment 1:

[0079] An electromagnetic protection coating includes a nitride and an oxide, wherein the nitride has a chemical expression as shown in Formula 1:

[0080] Formula 1: Fe α Co 1-α-β-γ-δ B β C γ D δ ;

[0081] Where: α: 0.50-0.74, β: 0.001-0.05; γ: 0.001-0.1, δ: 0.001-0.1; where the lower right subscript of the chemical formula represents the molar percentage of each component;

[0082] Fe is iron, Co is cobalt;

[0083] B is at least one of titanium, zirconium, niobium, vanadium, tungsten or molybdenum, and / or: B also includes at least one of lanthanide elements;

[0084] C is silicon or aluminum, and D is at least one of the lanthanide elements, that is, D in Formula 1 includes at least one or more of the rare earth lanthanide elements;

[0085] The lanthanide elements include: lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium.

[0086] Oxide: has the chemical expression shown in Formula 2:

[0087] Formula 2: A3B2Fe 24 O 41 ;

[0088] Among them: Fe is iron element; O is oxygen element;

[0089] A includes barium, strontium and calcium, and at least includes barium;

[0090] B includes cobalt, zinc, manganese, copper and nickel, and at least includes cobalt;

[0091] It can be seen from this embodiment that adjusting the ratio of nitride to oxide can adjust the anti-electromagnetic interference characteristics of the material at different frequencies, obtain anti-electromagnetic interference characteristics in different frequency bands, and can meet the requirements of different application scenarios.

[0092] This embodiment also discloses an application of nitride and oxide in a corrosion-resistant electromagnetic protective coating and a preparation method thereof.

[0093] Embodiment 2: Figure 1As shown, on the basis of the above embodiment, the present invention also provides a method for preparing a corrosion-resistant electromagnetic protective coating. This embodiment can exist alone or be used to prepare the nitride and oxide in the embodiment, and can be combined with other embodiments of the present application. The steps of the preparation method specifically include:

[0094] Step S1: preparing nitride (M material) and oxide (N material);

[0095] Step S2: generating anti-interference coating;

[0096] Step S3: preparing a self-cleaning coating;

[0097] Step S4: performing spraying operation;

[0098] The following further explains steps S1 to S4 in conjunction with specific application scenarios:

[0099] According to the chemical expressions, nitrides and oxides are prepared;

[0100] Preparation of anti-interference coating: uniformly mixing nitride, oxide, resin and organic solvent, performing dispersion treatment, and obtaining different anti-electromagnetic wave interference properties by adjusting the ratio of nitride and oxide to form a first component (component A) having nitride and oxide;

[0101] Specifically, the component ratio is: the sum of M material and N material is 100 parts by mass, wherein M material: 5 parts to 70 parts, resin: 11 parts to 100 parts, solvent: 10 parts to 20 parts, and the corresponding mass parts of N material are adjusted according to different M materials.

[0102] Specifically, in the process of preparing the anti-interference coating, the nitride, oxide, resin and organic solvent are uniformly mixed and dispersed, specifically: the equipment used for the dispersion treatment is a high-speed disperser, a sand mill, a ball mill or a three-roll mill;

[0103] The amine curing agent specifically includes aliphatic amine curing agents and polyamide curing agents;

[0104] In the aging treatment step of the anti-interference coating: 100 parts by mass of the first component and 12 parts by mass of the second component are mixed evenly, and the mixture is aged for 15 minutes to obtain the electromagnetic protection coating;

[0105] Spray the cured material onto the surface of the metal material with a coating thickness of 2mm. Curing at room temperature for 4 days before subsequent operations can be carried out;

[0106] In the process of preparing the filler surface treatment of the self-cleaning coating, the speed of the high-speed mixer is 1000 rpm, the treatment time is 3 min to 10 min, and the filler is one or more of white carbon black, aluminum oxide, and calcium carbonate;

[0107] During the filler mixing process for the preparation of self-cleaning coatings, the temperature of the vacuum kneader is 100°C.

[0108] ~150°C, mix for 1 to 5 hours;

[0109] In the dispersion process of preparing the self-cleaning coating, the planetary stirring disperser is used for dispersion at a speed of 50 rpm for 1 h to 2 h.

[0110] Specifically, the preparation of nitride includes:

[0111] Ingredients: Use analytically pure powdered raw materials and prepare them under nitrogen protection environment according to the alloy composition requirements;

[0112] Specifically, in the process of preparing the ingredients of nitrides, a laser particle size analyzer is used to detect whether the particle size meets the requirement of D50<10μm; D50 refers to the particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 50%. Its physical meaning is that particles with a particle size larger than it account for 50%, and particles with a particle size smaller than it also account for 50%. D50 is also called the median diameter or median particle size.

[0113] In the process of preparing the mechanical alloying of nitrides, specifically: the volume of the high-energy ball mill is 1L, and tungsten carbide grinding balls are used; the diameters of the tungsten carbide grinding balls include: 12mm, 10mm, 8mm, 6mm, 3mm, the configuration ratio is: 15:15:30:30:10, the ball-to-material ratio is 5-25, the ball mill speed is 150rpm-500rpm, and the ball milling time is 12h-96h; in the process of nitriding treatment, NH3: 5vol%-35vol%, N2: 10vol%-50vol%, and the rest is hydrogen, and the nitriding temperature is: 320℃

[0114] ~450℃, nitriding time: 2h~12h.

[0115] Mechanical alloying: Add the raw materials into an argon-protected high-energy ball mill for mechanical alloying;

[0116] After mechanical alloying is completed, the material is cooled to room temperature and transferred to a rotary atmosphere reactor under nitrogen protection;

[0117] Nitriding treatment: Rotary atmosphere reactor, using ammonia, nitrogen and hydrogen as nitriding sources;

[0118] Passivation treatment: The magnetic powder produced after the nitriding treatment is mixed evenly with the potassium dichromate solution, filtered after high-speed dispersion, washed with deionized water until colorless and transparent, then washed with acetone, and then dried in a vacuum drying oven for use. The temperature of the vacuum drying oven can be selected and set according to different application scenarios, for example, it can be set to 120°C; a high-speed disperser can be used for high-speed dispersion. A high-speed disperser uses a high-speed agitator (such as a disc sawtooth agitator) to form a strong turbulence locally, which usually has a strong dispersing and emulsifying effect on the material, so this type of high-speed agitator is also called a high-speed disperser.

[0119] The preparation of the oxide specifically comprises:

[0120] Ingredients: Use analytically pure powdered raw materials and prepare the ingredients according to the chemical molecular formula of the oxide;

[0121] Primary ball milling: Grind and mix the raw materials using wet ball milling;

[0122] Specifically, in the process of primary ball milling for preparing oxides, the prepared materials are loaded into a drum ball mill (volume 1L), the ball milling time is 24 to 48 hours, the ball-to-material ratio is 5 to 20, the materials are dried after discharge, and the average particle size of the mixed materials is tested (air permeation method) to be less than 0.5 microns;

[0123] In the process of pre-sintering the oxide, the temperature range is 1000°C to 1350°C, and the reaction time is 2 to 8 hours;

[0124] In the process of crushing and screening the oxides, a 200-mesh standard sieve is used for grading, and the material below the 200-mesh sieve is a qualified product.

[0125] Pre-calcination: subjecting the ball-milled mixture obtained by the first ball-milling to a high-temperature solid-phase reaction;

[0126] Secondary ball milling: The crushed raw materials are ground twice using a mixed ball mill;

[0127] Sintering: subjecting the secondary ball-milled mixture to a high-temperature solid-phase reaction;

[0128] Crushing and screening: crush and screen the sintered materials.

[0129] The second component includes an amine curing agent;

[0130] Curing treatment: the first component and the second component are mixed evenly, and a curing treatment is performed to obtain an electromagnetic protective coating; illustratively, the cured material is sprayed onto the surface of the metal material, the coating thickness is 2 mm, and subsequent operations can be performed after curing at room temperature for 4 days.

[0131] Specifically, it also includes preparing a self-cleaning coating:

[0132] Filler surface treatment: Surface treatment of filler is carried out by adding 0.5wt~1wt% of KH550 silane coupling agent in a high-speed mixer;

[0133] Filler mixing: 100 parts of polydimethylsiloxane and 10 to 20 parts of filler are added into a vacuum kneader at one time; illustratively, in this embodiment, the temperature may be 100° C. to 150° C., and the mixing time may be 1 hour to 5 hours;

[0134] Dispersion treatment: 100 parts of the above mixture are added to a planetary stirring disperser, and 110-180 parts of petroleum ether are added; illustratively, in this embodiment, the planetary stirring disperser is dispersed at a speed of 50 rpm for 1h-2h (1 hour to 2 hours);

[0135] Screen filtration: The coating is filtered using a screen to obtain a third component (Group C); illustratively, in this embodiment, a screen with a mesh size of 300 to 400 can be used for filtering.

[0136] Evenly mix: 100 parts by weight of the third component (group C) and 5-10 parts by weight of the fourth component (group D) are mixed and treated to form a self-cleaning coating.

[0137] Example 3: Based on the above examples, the present invention provides a corrosion-resistant electromagnetic protective coating. The corrosion-resistant electromagnetic protective coating of this example is made of the nitrides, oxides and preparation methods of the above examples. It has the characteristics of anti-electromagnetic interference under harsh environments, while taking into account corrosion resistance, and has the dual advantages of anti-electromagnetic interference and corrosion resistance.

[0138] like Figure 2 As shown, the corrosion-resistant electromagnetic protective coating includes a composite layer structure. In this embodiment, the composite layer structure may include a self-cleaning layer 1, an anti-interference layer 2 and a metal base layer 3. The surface of the metal base layer 3 is treated by a sandblasting process, and the anti-interference layer 2 and the self-cleaning layer 1 are sprayed with a corrosion-resistant electromagnetic protective coating. The corrosion-resistant electromagnetic protective coating provided in this embodiment is both resistant to seawater corrosion and can reduce the radar scattering area. It consists of an anti-electromagnetic interference coating and a self-cleaning surface layer. The anti-interference layer is composed of epoxy resin, nitride, and oxide, and the self-cleaning layer has a hydrophobic self-cleaning effect. By adjusting the ratio of nitride and oxide, the anti-electromagnetic interference characteristics of the material at different frequencies can be adjusted. In addition, the coating can pass various harsh tests such as high and low temperature, seawater resistance, humidity and heat resistance and other environmental resistance performance, and has excellent environmental resistance characteristics. The specific application scenario of this embodiment can be that the material is sprayed or brushed on the surface of the metal structure of the equipment to form an anti-interference layer and a self-cleaning layer.

[0139] Embodiment 4: Figure 3As shown, this embodiment discloses the overall preparation method and material components of corrosion-resistant electromagnetic protective coatings and coatings, and selects specific material components. This embodiment can be combined with other embodiments in the specification of this application to form more embodiments, which will not be described in detail due to space limitations.

[0140] In this embodiment, the corrosion-resistant electromagnetic protective coating is sprayed or brushed on the surface of the metal structure of the equipment, and is divided into an anti-interference layer and a self-cleaning layer.

[0141] 1. Anti-interference layer

[0142] 1. Nitride (M material):

[0143] Raw materials: According to Fe α Co 1-α-β-γ-δ B β C γ D δ , where α: 0.50-0.74, β: 0.001-0.05; γ: 0.001-0.1, δ: 0.001-0.1, where: Fe is iron, Co is cobalt;

[0144] B is at least one of titanium, zirconium, niobium, vanadium, tungsten or molybdenum;

[0145] C is at least one of silicon and aluminum;

[0146] D is a lanthanide rare earth element, including at least one or more rare earth lanthanides; lanthanide elements include: lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium.

[0147] Raw material particle size requirements: All raw materials are analytically pure powdered, and the particle size (laser particle size analyzer) requires D50<10μm.

[0148] Step A: Mixing the raw materials in a nitrogen atmosphere according to the alloy composition requirements.

[0149] Step B: Mechanical alloying, the raw materials are added into an argon-protected high-energy ball mill for mechanical alloying operation, and the ball mill has a volume of 1L. Tungsten carbide grinding balls are used, with diameters of 12mm, 10mm, 8mm, 6mm, and 3mm, respectively, with a configuration ratio of 15:15:30:30:10, a ball-to-material ratio of 5 to 25, a ball mill speed of 150rpm to 500rpm, and a ball milling time of 12h to 96h. After mechanical alloying is completed, the material is cooled to room temperature and transferred to a rotary atmosphere reactor under nitrogen protection.

[0150] Step C: nitriding treatment, rotary atmosphere reactor, using ammonia, nitrogen and hydrogen as nitriding sources, wherein NH3: 5vol%~35vol%, N2: 10vol%~50vol%, and the rest is hydrogen, nitriding temperature: 320℃~450℃, nitriding time: 2h~12h.

[0151] Step D: passivation treatment: the magnetic powder after nitridation treatment is mixed evenly with 0.5wt% to 2wt% potassium dichromate solution in a ratio of 1:3, dispersed at high speed for 30min to 60min, filtered, washed with deionized water until colorless and transparent, then washed with acetone, and dried in a vacuum drying oven at 120°C for use.

[0152] 2. Oxide (N material):

[0153] The chemical composition formula of the material is A3B2Fe 24 O 41 ;

[0154] A is one or more of barium, strontium and calcium, at least containing barium;

[0155] B is two or more of cobalt, zinc, manganese, copper, nickel, and rare earth lanthanide elements; at least cobalt is contained; lanthanide elements include lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium;

[0156] Fe is iron, O is oxygen;

[0157] Step E: Mixing ingredients: select corresponding analytically pure oxides as raw materials and mix them according to the proportions in the above chemical formula.

[0158] Step F: primary ball milling, using wet ball milling to grind and mix the materials. Specifically, the prepared materials are loaded into a drum ball mill (volume 1L), the ball milling time is 24 to 48 hours, the ball-to-material ratio is 5 to 20, the materials are dried after discharge, and the average particle size of the mixed material is tested (air permeability method) to be less than 0.5 microns.

[0159] Step G: Pre-calcination, subjecting the first ball-milled mixture to a high-temperature solid phase reaction, the temperature range: 1000° C. to 1350° C., the reaction time: 2 to 8 hours.

[0160] Step H: Crushing: crush the pre-burned material and use a 60-mesh standard sieve for screening. The material under the 60-mesh sieve is qualified and enters the next process.

[0161] Step I: secondary ball milling, using wet ball milling to grind the crushed material, water is used as the grinding medium, specifically, the prepared material is loaded into a drum ball mill (volume 10L), bismuth trioxide, boric acid or a mixture of the two are added, the addition ratio is 0.1wt% to 0.8wt% of the crushed material, the ball milling time is 12 to 24 hours, the ball-to-material ratio is 5 to 20, the material is subjected to high-temperature drying after discharge, and the average particle size of the mixture is tested (air permeability method) to be less than 1 micron.

[0162] Step J: Sintering, subjecting the secondary ball-milled mixture to a high-temperature solid-phase reaction, the temperature range: 1000° C. to 1350° C., the reaction time: 2 to 8 hours.

[0163] Step K: Crushing and screening: crush the sintered material and grade it with a 200-mesh standard sieve. The material below the 200-mesh sieve is a qualified product.

[0164] 3. Coating preparation:

[0165] Component A: It is composed of M material, N material, resin and organic solvent, wherein M material and N material are as described above, the resin mainly includes bisphenol A epoxy resin, and the organic solvent mainly includes a combination of two or more of ethyl acetate, cyclohexanone, DMC, high aromatic hydrocarbon S100A, etc.

[0166] Specific operation: Mix various materials in component A evenly, and use a high-speed disperser, sand mill, ball mill or three-roll mill for dispersion.

[0167] Group A allocation ratio requirements:

[0168] The total of M material and N material is 100 parts, including 5-70 parts of M material, 11-100 parts of resin, and 10-20 parts of solvent. The mass fraction of N material is adjusted according to the mass fraction of M material. The anti-electromagnetic interference properties of the coating can be adjusted by adjusting the ratio of M material and N material.

[0169] Component B: amine curing agent, mainly aliphatic amine curing agent and polyamide curing agent.

[0170] 2. Self-cleaning layer

[0171] 1. Component C

[0172] Step L: Surface treatment of filler: add 0.5wt~1wt% of KH550 silane coupling agent to the filler in a high-speed mixer (volume 10L), rotate at 1000rpm, and treat for 3min~10min. The filler type is one or more of white carbon black, aluminum oxide, and calcium carbonate.

[0173] Step M: Mixing: 100 parts of polydimethylsiloxane and 10 to 20 parts of filler are added into a vacuum kneader at once, the temperature is 100° C. to 150° C., and mixed for 1 to 5 hours.

[0174] Step N: Dispersion treatment: add 100 parts of the above mixture into a planetary stirring disperser, add 110-180 parts of petroleum ether, and disperse at a speed of 50 rpm for 1 hour to 2 hours.

[0175] Step O: Filtration: filtering the coating using a 300-400 mesh screen to obtain a C component coating.

[0176] 2. Component D: Curing agent: methyl tris(butyl)oxime silane, ethyl acetate.

[0177] 3. Construction:

[0178] 1. Step P: Substrate surface treatment

[0179] The metal surface is sandblasted to clean the oxide layer on the metal surface and improve the bonding strength between the base material and the coating.

[0180] 2. Step Q: Preparation of anti-interference coating;

[0181] Q1 Ripening treatment: Mix 100 parts of component A and 10-20 parts of component B evenly, and ripen for 10-20 minutes;

[0182] Q2 Construction: Spray the cured material onto the surface of the metal material with a coating thickness of 0.5mm to 3mm.

[0183] 3. Step R: Preparation of self-cleaning layer

[0184] R1 aging treatment: mix 100 parts of component C and 5-10 parts of component D evenly, and age for 10-20 minutes;

[0185] R2 construction: Before construction, it must be confirmed that the anti-interference coating has been completely cured, and then the self-cleaning coating is evenly sprayed on the anti-interference coating with a spraying thickness of about 0.2 to 0.4 mm.

[0186] Embodiment 5: This embodiment discloses the implementation of the present invention in a specific application scenario. This embodiment can be combined with other embodiments to form more embodiments, which will not be described in detail due to space limitations.

[0187] Some standards and specifications

[0188]

[0189] 1. Nitride (M1):

[0190] Raw materials: According to Fe0.6 Co 0.3 Nb 0.02 Al 0.005 Sm 0.075 , where: Fe is iron, Co is cobalt, Nb is niobium, Sm is samarium, and analytically pure powdered raw materials are used, with a particle size (laser particle size analyzer) D50<10μm. The raw materials are prepared under nitrogen protection according to the alloy composition requirements. The raw materials are added to an argon-protected high-energy ball mill for mechanical alloying operation, and the ball mill volume is 1L. Tungsten carbide grinding balls are used, with diameters of 12mm, 10mm, 8mm, 6mm, and 3mm, respectively. The configuration ratio is: 15:15:30:30:10, the ball-to-material ratio is 20, the ball mill speed is 350rpm, and the ball milling time is 24h. After mechanical alloying, the material is cooled to room temperature and transferred to a rotary atmosphere reactor under nitrogen protection. Ammonia, nitrogen, and hydrogen are used as nitriding sources, of which NH3: 25vol%, N2: 25vol%, and the rest is hydrogen. The nitriding temperature is: 400℃, and the nitriding time is: 4h. The nitrided magnetic powder was mixed evenly with 1wt% potassium dichromate solution at a ratio of 1:3, dispersed at high speed for 45 minutes, filtered, washed with deionized water until colorless and transparent, then washed with acetone, and dried in a vacuum drying oven at 120°C for use, material number M1.

[0191] 2. Oxide (N1)

[0192] The chemical composition formula of the material is Ba 2.5 Ca 0.5 Co 1.5 La 0.5 Fe 24 O 41 , the weight percentage of each component of the ingredients is calculated as follows:

[0193] Product Name BaO CaO <![CDATA[CO2O3]]> <![CDATA[La2O3]]> <![CDATA[Fe2O3]]> Weight Percent 15.1% 1.1% 4.9% 3.2% 75.7%

[0194] The ingredients are prepared according to the proportions in the above chemical formula. The materials are ground and mixed by wet ball milling. Specifically, the prepared materials are loaded into a drum ball mill (volume 1L), the ball milling time is 36 hours, the ball-to-material ratio is 10:1, and the materials are dried after discharge. The average particle size of the mixture is tested (air permeation method) and is 0.48 microns. The mixture obtained by the first ball milling is placed in a muffle furnace for solid phase reaction, the temperature range is: 1270℃, and the reaction time is: 3 hours. The pre-burned material is crushed and sieved with a 60-mesh standard sieve. The sieved material is a qualified product and can enter the next process. The crushed material is ground by wet ball milling, and water is used as the grinding medium. Specifically, the prepared materials are loaded into a drum ball mill (volume 10L), and the addition ratio of bismuth trioxide is 0.5wt% of the crushed material. The ball milling time is: 16 hours, the ball-to-material ratio is 10:1. After discharge, the material is dried at 120℃, and the average particle size of the mixture is tested (air permeation method) 0.8 microns. The mixed material obtained by the secondary ball milling was placed in a muffle furnace for solid phase reaction, the temperature range was 1270°C, and the reaction time was 4 hours. The sintered material was crushed and graded with a 200-mesh standard sieve, and the sieved material was qualified, with material number N1.

[0195] 3. Coating preparation:

[0196] Component A: It is composed of M1 material, N1 material, resin, and organic solvent, wherein M1 material and N1 material are prepared as described above, the resin is bisphenol A epoxy resin E44, and the organic solvent is ethyl acetate. Specific operation: Mix various materials in component A evenly and use a high-speed disperser for dispersion treatment.

[0197] Allocation ratio of group A:

[0198]

[0199] Component B: Phenolic amine curing agent, commercial brand: T31, add 5 parts.

[0200] 4. Self-cleaning layer:

[0201] Component C: 4kg of white carbon black filler was added to a high-speed mixer (volume 10L), 0.75wt% of KH550 silane coupling agent was added, the speed was 1000rpm, the processing time was 10min, 100 parts of polydimethylsiloxane and 15 parts of the treated filler were added to a vacuum kneader at once, the temperature was 120℃, and mixed for 4 hours. 100 parts of the above mixture was added to a planetary stirring disperser, 150 parts of petroleum ether was added, and the mixture was dispersed at a speed of 50rpm for 1.5h. The coating was filtered using a 360-mesh screen to obtain the coating component C.

[0202] Component D: Curing agent: methyl tris(butyl)oxime silane.

[0203] 5. Construction:

[0204] The metal surface is sandblasted to clean the oxide layer on the metal surface and improve the bonding strength between the base material and the coating.

[0205] Preparation of anti-interference coating: Mix 100 parts of component A and 12 parts of component B evenly, and cure for 15 minutes; spray the cured material onto the surface of the metal material, with a coating thickness of 2mm. After curing at room temperature for 4 days, subsequent operations can be carried out.

[0206] Preparation of self-cleaning layer: Mix 100 parts of component C and 8 parts of component D evenly, cure for 15 minutes, and spray the self-cleaning coating evenly on the anti-interference coating. The coating thickness is about 0.3 mm.

[0207] like Figure 4 and Figure 5 As shown in the figure, in accordance with the requirements of GB / T 35679-2017, the coaxial method was used to prepare the corresponding test samples of M1 and N1. The sample size was φ7mm×φ3mm×3mm paraffin ring. The electromagnetic parameters of the material were tested on the Agilent 8720ET vector network analyzer, including e1 (real part of dielectric constant), e2 (imaginary part of dielectric constant), u1 (real part of magnetic permeability), and u2 (imaginary part of magnetic permeability).

[0208] like Figure 6 As shown, according to the requirements of GJB 2038A-2011, the coating of this embodiment is applied on a standard aluminum plate of 300mm×300mm, and the coating reflectivity test results are shown in the figure.

[0209] The environmental resistance data of this embodiment are shown in the following table. It can be seen from the data in the table that the environmental resistance of the coating is good.

[0210] Comparison of coating environmental resistance characteristics

[0211]

[0212] Embodiment six:

[0213] The preparation process of this embodiment is the same as that of the fifth embodiment, and the main differences are: 1. The oxide composition and preparation process are different; 2. The distribution ratio of group A is different, specifically:

[0214] 1. Oxide (material number N2)

[0215] The chemical composition formula of the material is Ba 2.8 Sr 0.2 Co 1.7 Dy 0.3 Fe 24 O 41 , the weight percentage of each component of the ingredients is calculated as follows:

[0216] Product Name BaO SrO <![CDATA[CO2O3]]> <![CDATA[Dy2O3]]> <![CDATA[Fe2O3]]> Weight Percent 16.7% 0.8% 5.5% 2.2% 74.8%

[0217] The ingredients are prepared according to the proportions in the above chemical formula. The materials are ground and mixed by wet ball milling, and the prepared materials are loaded into a drum ball mill (volume 1L), the ball milling time is 36 hours, the ball-to-material ratio is 10:1, and the materials are dried after discharge. The average particle size of the test mixture (air permeation method) is 0.5 microns. The first ball milling mixture is placed in a muffle furnace for solid phase reaction, the temperature range is: 1200℃, the reaction time is: 3 hours. The pre-burned material is crushed, and a 60-mesh standard sieve is used for screening. The sieved material is a qualified product and enters the next process. The crushed material is ground by wet ball milling, and water is used as the grinding medium. Specifically, the prepared material is loaded into a drum ball mill (volume 10L), and boric acid is added in a ratio of 0.7wt% of the crushed material. The ball milling time is: 20 hours, the ball-to-material ratio is 10:1, and the material is dried at 120℃ after discharge. The average particle size of the test mixture (air permeation method) is 0.8 microns. The secondary ball milled mixture was placed in a muffle furnace for solid phase reaction at a temperature range of 1280°C and a reaction time of 3 hours. The sintered material was crushed and graded with a 200-mesh standard sieve. The sieved material was qualified and had a material number of N2.

[0218] 2. Group A allocation ratio:

[0219]

[0220] Component B: Phenolic amine curing agent, commercially available brand: T31, add 6 parts.

[0221] like Figure 7 and Figure 8 As shown, the test results are as follows: According to the requirements of GB / T 35679-2017, the coaxial method is used to prepare the N2 corresponding test sample, and the sample size is φ7mm×φ3mm×3mm paraffin ring. The electromagnetic parameters of the material are tested on the Agilent 8720ET vector network analyzer, including e1 (real part of dielectric constant), e2 (imaginary part of dielectric constant), u1 (real part of magnetic permeability), and u2 (imaginary part of magnetic permeability). According to the requirements of GJB 2038A-2011, the coating of Example 1 is applied on a standard aluminum plate of 300mm×300mm, and the test results of the coating reflectivity are shown in the coordinate diagram. From the data analysis of the coordinate diagram, it can be seen that the corrosion-resistant electromagnetic protective coating and coating have excellent wave absorption characteristics at 10GHz~18GHz, and the coating has good environmental resistance.

[0222] Embodiment 7 (comparative example):

[0223] The preparation process of this comparative example is basically the same as that of Example 5, except that the self-cleaning layer is not applied during the construction process of this comparative example. Compared with Example 5, the coating has rust spots after 1000 hours of neutral salt spray, while Example 5 with the self-cleaning coating is excellent, which shows the importance of the self-cleaning coating in the entire coating system; the self-cleaning layer is composed of super-hydrophobic organic silicon material, and water droplets can only form water droplets on the coating, but cannot form a water film, which greatly reduces the possibility of water molecules penetrating into the coating. The corrosion-resistant protective coating of the present invention has both corrosion resistance and anti-electromagnetic interference function, meeting the requirements of civil and military industries.

[0224] Embodiment 8: This embodiment discloses a wind power generation equipment, which is sprayed with corrosion-resistant electromagnetic protective paint and / or has a corrosion-resistant electromagnetic protective coating.

[0225] Those skilled in the art will appreciate that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those generally understood by those skilled in the art in the art to which the present invention belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined.

[0226] It should be noted that certain words are used in this specification and claims to refer to specific components. Those skilled in the art should understand that different manufacturers and producers may use different terms to refer to the same component. This specification and claims do not use the difference in terms as a way to distinguish components, but use the difference in the functions of the components as the criterion for distinction.

[0227] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0228] In addition, those skilled in the art will appreciate that, although some embodiments described herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and form different embodiments. For example, any one of the embodiments claimed in the claims can be used in any combination in the embodiments of the present invention.

[0229] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0230] In addition, the technical solutions between the various embodiments of the present invention can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0231] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any way. Any feature disclosed in this specification, unless otherwise stated, can be replaced by other equivalent or alternative features with similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features. Throughout the specification, the same reference numerals indicate the same elements.

[0232] Those skilled in the art will appreciate that the modules in the devices in the embodiments can be adaptively changed and set in one or more devices different from the embodiments. The modules or units or components in the embodiments can be combined into one module or unit or component, and in addition they can be divided into multiple submodules or subunits or subcomponents. Except that at least some of such features and / or processes or units are mutually exclusive, all features disclosed in this specification (including corresponding claims, abstracts and drawings) and all processes or units of any method or device disclosed in this manner can be combined in any combination. Unless otherwise explicitly stated, each feature disclosed in this specification (including corresponding claims, abstracts and drawings) can be replaced by an alternative feature that provides the same, equivalent or similar purpose.

[0233] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A corrosion-resistant electromagnetic protective coating, characterized in that: It includes an anti-interference layer, a self-cleaning layer and a metal base layer, wherein the surface of the metal base layer is treated by a sandblasting process, the anti-interference layer is arranged between the self-cleaning layer and the metal base layer, and the anti-interference layer includes nitride and oxide, and the nitride has a chemical expression shown in Formula 1: Formula 1: Fe α Co 1-α-β-γ-δ B β C γ D δ ; Where: α: 0.50-0.74, β: 0.001-0.05; γ: 0.001-0.1, δ: 0.001-0.1, where the lower right subscript of the chemical formula represents the molar percentage of each component; Fe is iron, Co is cobalt; B is at least one of titanium, zirconium, niobium, vanadium, tungsten or molybdenum; C is silicon or aluminum, and D is at least one of the lanthanide elements; The preparation of nitrides includes: Ingredients: Use analytically pure powdered raw materials and prepare them under nitrogen protection environment according to the alloy composition requirements; Mechanical alloying: Add the raw materials into an argon-protected high-energy ball mill for mechanical alloying; After mechanical alloying is completed, the material is cooled to room temperature and transferred to a rotary atmosphere reactor under nitrogen protection; Nitriding treatment: Rotary atmosphere reactor, using ammonia, nitrogen or hydrogen as nitriding source; Passivation treatment: Mix the magnetic powder and potassium dichromate solution evenly, disperse at high speed, filter, wash with deionized water until colorless and transparent, then wash with acetone, and then dry in a vacuum drying oven for later use; Oxide: has the chemical expression shown in Formula 2: Formula 2: A3B2Fe 24 O 41 ; Among them: Fe is iron element; O is oxygen element; A includes barium, strontium or calcium; B includes cobalt, zinc, manganese, copper and nickel; the preparation method of the self-cleaning coating of the self-cleaning layer is specifically as follows: Filler surface treatment: Surface treatment of filler is carried out by adding 0.5 wt~1 wt% of KH550 silane coupling agent in a high-speed mixer; Filler mixing: Add 100 parts of polydimethylsiloxane and 10-20 parts of filler into a vacuum kneader at one time; Dispersion treatment: add 100 parts of the mixture into a planetary stirring disperser and add 110-180 parts of petroleum ether; Screen filtration: Use screen to filter the coating to obtain the third component; Mixing evenly: 100 parts by mass of the third component and 5-10 parts by mass of the fourth component are mixed and aged to generate a self-cleaning coating, wherein the fourth component is a curing agent: methyl tris(butyl)oxime silane and ethyl acetate.

2. A method for preparing the corrosion-resistant electromagnetic protective coating according to claim 1, characterized in that: include: According to the chemical expressions, nitrides and oxides are prepared; Preparation of anti-interference coating: uniformly mixing nitride, oxide, resin and organic solvent, performing dispersion treatment, and obtaining different anti-electromagnetic wave interference properties by adjusting the ratio of nitride and oxide to form a first component having nitride and oxide; The second component includes an amine curing agent; Ripening treatment: Mix the first component and the second component evenly and perform aging treatment; The preparation of nitrides includes: Ingredients: Use analytically pure powdered raw materials and prepare them under nitrogen protection environment according to the alloy composition requirements; Mechanical alloying: Add the raw materials into an argon-protected high-energy ball mill for mechanical alloying; After mechanical alloying is completed, the material is cooled to room temperature and transferred to a rotary atmosphere reactor under nitrogen protection; Nitriding treatment: Rotary atmosphere reactor, using ammonia, nitrogen or hydrogen as nitriding source; Passivation treatment: Mix the magnetic powder and potassium dichromate solution evenly, disperse at high speed, filter, wash with deionized water until colorless and transparent, then wash with acetone, and then dry in a vacuum drying oven for later use; The preparation of the oxide comprises: Ingredients: Use analytically pure powdered raw materials and prepare the ingredients according to the chemical molecular formula of the oxide; Primary ball milling: Grind and mix the raw materials using wet ball milling; Pre-calcination: subjecting the ball-milled mixture obtained by the first ball-milling to a high-temperature solid-phase reaction; Secondary ball milling: The crushed raw materials are ground twice using a mixed ball mill; Sintering: subjecting the secondary ball-milled mixture to a high-temperature solid-phase reaction; Crushing and screening: crushing and screening the sintered materials; Also included is the preparation of self-cleaning coatings: Filler surface treatment: Surface treatment of filler is carried out by adding 0.5 wt~1 wt% of KH550 silane coupling agent in a high-speed mixer; Filler mixing: Add 100 parts of polydimethylsiloxane and 10-20 parts of filler into a vacuum kneader at one time; Dispersion treatment: add 100 parts of the mixture into a planetary stirring disperser and add 110-180 parts of petroleum ether; Screen filtration: Use screen to filter the coating to obtain the third component; Mixing evenly: 100 parts by mass of the third component and 5-10 parts by mass of the fourth component are mixed and aged to generate a self-cleaning coating, wherein the fourth component is a curing agent: methyl tris(butyl)oxime silane and ethyl acetate.

3. The method for preparing a corrosion-resistant electromagnetic protective coating according to claim 2, characterized in that: In the process of preparing the anti-interference coating, the nitride, oxide, resin and organic solvent are uniformly mixed and dispersed. Specifically, the equipment used for the dispersion treatment is a high-speed disperser, a sand mill, a ball mill or a three-roll mill; The amine curing agent includes aliphatic amine curing agent and polyamide curing agent; In the aging step of the anti-interference coating: 100 parts by mass of the first component and 12 parts by mass of the second component are mixed evenly and aging is performed for 15 minutes; Spray the cured material onto the surface of the metal material with a coating thickness of 2mm and cure at room temperature; In the process of preparing the filler surface treatment of the self-cleaning coating, the speed of the high-speed mixer is 1000 rpm, the treatment time is 3 min to 10 min, and the filler is one or more of white carbon black, aluminum oxide, and calcium carbonate; In the process of preparing the filler mixing of the self-cleaning coating, the temperature of the vacuum kneader is 100°C to 150°C, and the mixing time is 1 hour to 5 hours; In the dispersion process of preparing the self-cleaning coating, the planetary stirring disperser is used for dispersion at a speed of 50 rpm for 1 h to 2 h.

4. The method for preparing a corrosion-resistant electromagnetic protective coating according to claim 2, characterized in that: In the process of preparing the filler mixing of the self-cleaning coating, the vacuum kneader is maintained at a temperature of 100°C to 150°C and mixed for 1 hour to 5 hours; In the dispersion process of preparing the self-cleaning coating, the planetary stirring disperser disperses at a speed of 50 rpm for 1 h-2 h; In the screen filtration process of preparing the self-cleaning coating, a screen of 300 to 400 mesh is used for filtering.

5. The method for preparing a corrosion-resistant electromagnetic protective coating according to claim 2, characterized in that: In the process of preparing the ingredients of nitride, a laser particle size analyzer is used to detect whether the particle size meets the requirement of D50 < 10 μm; In the process of preparing the mechanical alloying of nitrides, specifically: the volume of the high-energy ball mill is 1L, and tungsten carbide grinding balls are used.

6. The method for preparing a corrosion-resistant electromagnetic protective coating according to claim 2, characterized in that: In the process of primary ball milling for preparing oxides, the prepared materials are loaded into a drum ball mill for 24 to 48 hours, with a ball-to-material ratio of 5 to 20. After the materials are discharged, they are dried, and the average particle size of the mixed materials is tested to be less than 0.5 microns. In the process of pre-sintering the oxide, the temperature range is 1000°C to 1350°C, and the reaction time is 2 to 8 hours; In the process of crushing and screening the oxides, a 200-mesh standard sieve is used for grading, and the material below the 200-mesh sieve is a qualified product.

7. Use of nitride and oxide in the corrosion-resistant electromagnetic protective coating according to claim 1.

8. A wind power generation device, characterized in that: The wind power generation equipment is sprayed with corrosion-resistant electromagnetic protective coating and has the corrosion-resistant electromagnetic protective coating as claimed in claim 1.

Citation Information

Patent Citations

  • Resin composition

    CN101636449A

  • High temperature stability Co-doped EMI-resistance soft magnetic material and preparation method thereof

    CN101710520A

  • 0.6-18GHz-frequency-band microwave-absorbing / epoxy anti-electromagnetic interference coating material and preparation method thereof

    CN103275591A

  • High-temperature electromagnetic wave absorbent, microwave absorbing coating and preparation method of microwave absorbing coating

    CN107474618A

  • Self-cleaning super-hydrophobic long-acting anti-corrosion coating and preparation method thereof

    CN108003753A