A kind of heat-conducting exhaust tape and preparation method thereof
By using hydrolysis-resistant insulating materials and thermal flame retardant tape in the lithium battery pack of new energy vehicles, combined with structured mesh release profiles, the thermal runaway management and service life problems are solved, efficient thermal conductivity and flame retardant performance are achieved, and the battery is extended The service life of the bag.
Patent Information
- Application Number
- CN202211723138.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The thermal runaway management and service life challenges of lithium battery packs in new energy vehicles, and existing materials are difficult to meet multiple performance requirements such as thermal conductivity, insulation, flame retardant and hydrolysis resistance.
Use hydrolysis-resistant insulating materials as the substrate, combined with pressure-sensitive adhesives with thermal conductivity, flame retardant and high bonding properties to form exhaust channels through structured mesh release profiles, improving thermal conductivity and flame retardant performance, and improving through specific combinations and treatments Thermal conductivity of the adhesive layer.
It achieves excellent bonding performance, electrical insulation performance, hydrolysis resistance and good thermal conductivity and flame retardant properties of the tape, quickly discharge bubbles, extend service life, and improves the heat dissipation efficiency in the battery pack.
Smart Images

Figure CN116200137B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of automotive tapes, and in particular relates to a heat-conducting exhaust tape and a preparation method thereof. Background Art
[0002] New energy vehicles have developed rapidly in the past decade, gradually forming a huge and complete new energy material industry chain. The rapid development of new energy vehicles is inseparable from the increasing performance of lithium batteries, which in turn has driven the synchronous development of the lithium battery related supporting product industry chain.
[0003] At present, the biggest problems plaguing new energy vehicles include endurance, thermal runaway management, spontaneous combustion, and service life. Increasing the range can be achieved by increasing the number of battery cells and increasing energy density, but the increase in the number of battery cells will inevitably lead to an increase in the number of welding points and an increase in the difficulty coefficient of heat dissipation, which increases the difficulty of thermal runaway management of battery packs. The service life requirements of new energy vehicles have gradually extended from 8 years to 15 years, which poses a great challenge to the weather resistance, hydrolysis resistance, fatigue resistance, etc. of various materials. Therefore, the requirements for thermal conductivity, insulation, flame retardancy, weather resistance and other properties of new energy battery supporting materials are becoming increasingly urgent, and general materials have been difficult to meet the design and application requirements. As a material with a large amount of usage inside the battery pack, adhesive tape not only needs to bear the bonding function, but also needs to meet the functions of thermal conductivity, flame retardancy, insulation, hydrolysis resistance, etc. Summary of the invention
[0004] The present invention aims to solve the above problems and provides a thermally conductive exhaust tape and a preparation method thereof, which not only performs the bonding function but also meets the functional requirements of thermal conductivity, flame retardancy, insulation, hydrolysis resistance, etc.
[0005] According to the technical solution of the present invention, the thermally conductive exhaust tape comprises a first grid release layer, a first adhesive layer, a substrate layer, a second adhesive layer and a second grid release layer which are sequentially stacked;
[0006] The substrate layer is made of hydrolysis-resistant insulating material;
[0007] The first adhesive layer and the second adhesive layer are prepared from the following components in parts by weight:
[0008]
[0009]
[0010] The present invention adopts hydrolysis-resistant insulating material as the base material, giving the tape excellent hydrolysis resistance; coating a heat-conductive, flame-retardant, high-adhesive pressure-sensitive adhesive (adhesive layer) to give the tape higher thermal conductivity and good flame-retardant properties; and giving the pressure-sensitive adhesive surface a structured exhaust channel through a structured grid release profile, which can quickly eliminate bubbles caused by the bonding construction, thereby eliminating the adverse effect of the air layer on the heat dissipation between devices in the battery pack.
[0011] Furthermore, the thickness of the substrate layer is 0.002-0.1 mm, and the material thereof is selected from PET (polyethylene terephthalate), PC (polycarbonate), PP (polypropylene) or PI (polyimide) film.
[0012] Preferably, the thickness of the substrate layer is 0.012-0.075 mm, preferably 0.03-0.075 mm, such as 36 μm, 50 μm, or 75 μm; and the material thereof is PET film.
[0013] Furthermore, the thickness of the first adhesive layer and the second adhesive layer are both 0.01-0.15 mm, wherein the thickness of the first adhesive layer and the second adhesive layer are the same or different.
[0014] Preferably, the thickness of the first adhesive layer and the second adhesive layer are both 0.02-0.085 mm, preferably 0.05-0.085 mm, such as 82 μm, 75 μm, or 62.5 μm.
[0015] Furthermore, the release force of the first grid release layer is 2-8 g / 25 mm, and the thickness is 30-70 μm; the release force of the second grid release layer is 10-30 g / 25 mm, and the thickness is 80-130 μm.
[0016] Furthermore, the first grid release layer and the second grid release layer are both multi-layer structures, including a release film substrate layer, a microstructure coating layer and a release agent layer stacked in sequence. The release agent layer is laminated to the adhesive layer, specifically, the release agent layer of the first grid release layer is laminated to the first adhesive layer, and the release agent layer of the second grid release layer is laminated to the second adhesive layer.
[0017] Furthermore, the release film substrate layer is selected from PET base film, glassine paper or kraft paper.
[0018] Furthermore, the microstructure coating layer is made of thermoplastic resin, and the thermoplastic resin is selected from PE (thermoplastic resin), PP, PMMA (polymethyl methacrylate) or TPU (thermoplastic polyurethane elastomer rubber); preferably, the microstructure coating layer is PE resin.
[0019] Furthermore, the microstructure coating layer is processed by coating a layer of thermoplastic resin on the release film substrate, and then laminating the layer with a mesh roller that engraves fixed patterns.
[0020] Specifically, the thermoplastic resin is coated at 280-320°C, and the temperature of the anilox roller is 280-320°C.
[0021] Furthermore, the embossing of the microstructure coating layer is selected from rhombus, square, pentagon, hexagon, heptagon, octagon, etc.; preferably, the embossing of the microstructure coating layer is rhombus or square.
[0022] Furthermore, the release agent layer adopts an addition type silicone oil release agent.
[0023] Furthermore, the polymer resin is selected from acrylic resin, polyurethane resin, silicone resin, polyurethane-modified acrylic resin, epoxy-modified acrylic resin, silicone-modified acrylic resin, natural rubber or synthetic rubber. Preferably, the polymer resin is acrylic resin.
[0024] Furthermore, the tackifying resin is selected from one or more of petroleum resin, dicyclopentadiene resin, rosin and rosin derivative resin, terpene resin, coumarone-indene resin, alkylphenol-formaldehyde resin, styrene series resin and xylene resin.
[0025] Preferably, the tackifying resin is selected from one or more of rosin and rosin derivative resins, terpene resins and petroleum resins.
[0026] Furthermore, the flame retardant is selected from one or more of phosphate compounds, organic nitrogen compounds, halogen compounds, phosphorus nitrogen compounds, dicyclopentadiene compounds, boron-based, antimony-based and aluminum-based inorganic compounds.
[0027] Specifically, the halogen compounds include tetrabromobisphenol A, tribromophenol, pentabromodiphenyl ether, decabromodiphenyl ether, decabromodiphenyl ethane, chlorinated paraffin, perchlorocyclodecane, etc.
[0028] Phosphate compounds include tributyl phosphate, tri(2-ethylhexyl) phosphate, tri(2-chloroethyl) phosphate, tri(2,3-dichloropropyl) phosphate, tri(2,3-dibromopropyl) phosphate, Pyrol99, toluene-diphenyl phosphate, tricresyl phosphate, triphenyl phosphate, (2-ethylhexyl)-diphenyl phosphate, tri(dibromopropyl) phosphate, hypophosphite, etc.;
[0029] Phosphorus and nitrogen compounds include melamine phosphate, melamine polyphosphate, ammonium polyphosphate, etc.;
[0030] Boron-based, antimony-based and aluminum-based inorganic compounds include aluminum hydroxide, magnesium hydroxide, zirconium hydroxide, organic zirconium phosphonate, fluorozirconate, boric acid, zinc borate, aluminum borate, ammonium pentaborate, sodium metaborate, ammonium fluoroborate, barium metaborate, antimony trioxide, antimony pentoxide, sodium antimonate, etc.
[0031] Preferably, the flame retardant is selected from soluble organic compounds such as some phosphate compounds, and insoluble inorganic compounds with a particle size of 0.3 to 5 μm.
[0032] Furthermore, the thermally conductive powder is one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride and silicon carbide.
[0033] Furthermore, the particle size of the thermally conductive powder is 0.01-5 μm.
[0034] Specifically, the thermally conductive powder is compounded by particles with a particle size of 10-600 nm and particles with a particle size of 1-15 μm in a mass ratio of 1:4 to 5:1. By compounding thermally conductive powders of different particle sizes, a dense thermal conductive channel with a micro-nano structure is formed, thereby improving thermal conductivity efficiency.
[0035] Furthermore, the dispersant is selected from one or more of pyridinium salts, oleates, amine salts, quaternary ammonium salts, sulfate ester salts, sulfonates, carboxylates, fatty acids, aliphatic amides, higher fatty acid metal salts, modified polyolefin salts, low molecular weight waxes and nonionic polymer copolymers.
[0036] Furthermore, the coupling agent is selected from one or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-(methacryloyloxy)propyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, benzylaminomethyltriethoxysilane, and isobutyltriethoxysilane.
[0037] Further, the organic solvent is selected from one or more of ethyl acetate, butyl acetate, acetone, butanone, cyclohexanone, isophorone, toluene, xylene, dimethyl carbonate, propylene glycol monomethyl ether and dipropylene glycol methyl ether; preferably, the organic solvent is ethyl acetate.
[0038] Another aspect of the present invention provides a method for preparing the above-mentioned thermally conductive exhaust tape, comprising the following steps:
[0039] S1: Add 50-100 parts of polymer resin, 0.3-2.5 parts of dispersant, and 0.3-1.5 parts of coupling agent to 30-100 parts of organic solvent by weight, mix well, then add 5-25 parts of tackifying resin, 10-30 parts of flame retardant and 20-100 parts of thermal conductive powder, mix well to obtain a combined liquid;
[0040] S2: grinding and filtering the combined liquid, and then adding 0.05 to 2 parts of a curing agent to obtain an adhesive composition;
[0041] S3: coating the adhesive composition on one side of the substrate layer, and attaching the first grid release layer thereto after drying to obtain a semi-finished product;
[0042] S4: coating the adhesive composition on the second grid release layer, and laminating the adhesive composition on the surface of the substrate layer of the semi-finished product after drying to obtain the thermally conductive exhaust tape.
[0043] Specifically, in step S1, the first mixing is carried out at a speed of 700-1000 r / min for 8-15 min; the second mixing is carried out at a speed of 700-1000 r / min for 100-180 min;
[0044] In the step S2, the grinding times are 3-5 times, and the mixture is filtered through a 400-mesh filter cloth; after adding the curing agent, the mixture is stirred at a speed of 700-1000 r / min for 35-60 minutes and then defoamed to obtain the adhesive composition.
[0045] The technical solution of the present invention has the following advantages over the prior art:
[0046] (1) The adhesive tape prepared by the present invention has excellent bonding performance, electrical insulation performance, hydrolysis resistance, good thermal conductivity and flame retardancy, can quickly remove bubbles after lamination, and is easy to use;
[0047] (2) By laminating the release film with a specific shape to the adhesive layer, a structured exhaust channel is formed in the adhesive layer, giving the adhesive layer excellent bubble removal performance, which is conducive to the rapid exhaust of the tape during lamination and solves the influence of the air bubbles generated at the lamination interface on the adhesive strength and thermal conductivity of the tape;
[0048] (3) By introducing flame retardants into acrylic resin, the adhesive layer is endowed with excellent flame retardant properties; by compounding nano-micron-sized thermal conductive powder, a micro-nanostructured thermal conductive channel is formed in the adhesive, which greatly improves the thermal conductivity of the adhesive layer;
[0049] (4) Through customized hydrolysis-resistant PET material, the tape is provided with excellent insulation performance on the one hand, and on the other hand, it is given better hydrolysis resistance and longer service life;
[0050] (5) By selecting and matching the thickness of the substrate layer and the adhesive layer, the excellent bonding performance, thermal conductivity and flame retardancy of the adhesive tape are guaranteed at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1It is a schematic diagram of the structure of the heat-conducting exhaust tape of the present invention.
[0052] Explanation of the accompanying drawings: 11 - first grid release layer; 12 - first adhesive layer; 13 - substrate layer; 14 - second adhesive layer; 15 - second grid release layer. DETAILED DESCRIPTION
[0053] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0054] The testing standards and instruments in the embodiments of the present invention are as follows:
[0055] (1) Thickness: Refer to GB / T 13541-92, the test equipment is Mitutoyo 547-400S digital thickness gauge;
[0056] (2) Peel force: refer to GB / T 2792-1998 standard, the test equipment is Kejian KJ-1065A tensile testing machine;
[0057] (3) Shear strength: Refer to GB / T 7124-2008 standard, the test equipment is Shimadzu universal testing machine;
[0058] (4) Thermal conductivity: refer to SATM D5470 standard, the test equipment is Ruiling's LW-9389 testing machine;
[0059] (5) Flame retardant grade; refer to UL94-2021 standard test;
[0060] (6) Tensile strength: refer to GB / T 13542.2-2009 standard, the test equipment is Shimadzu universal testing machine;
[0061] (7) Aging peel strength: The tape product is attached to a standard steel plate and placed in a double 85 aging box. After 2000 hours, the peel strength is tested.
[0062] (8) Aging tensile strength: Place the tape product in a double 85 aging box, place it for 2000 hours, and then take it out to test the tensile strength.
[0063] In the examples of the present invention, if no specific conditions are specified, the experiments were carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be purchased commercially.
[0064] like Figure 1 As shown, the thermally conductive exhaust tape of the present invention comprises a first grid release layer 11, a first adhesive layer 12, a substrate layer 13, a second adhesive layer 14 and a second grid release layer 15 which are sequentially stacked from top to bottom.
[0065] Among them, the substrate layer 13 is made of hydrolysis-resistant insulating material with a thickness of 0.002 to 0.1 mm; the thickness of the first adhesive layer 12 and the second adhesive layer 14 are both 0.01 to 0.15 mm; the release force of the first grid release layer 11 is 2 to 8 g / 25 mm, and the thickness is 30 to 70 μm; the release force of the second grid release layer 14 is 10 to 30 g / 25 mm, and the thickness is 80 to 130 μm.
[0066] Example 1
[0067] The thermally conductive exhaust tape of the present embodiment includes a first grid release layer 11 , a first adhesive layer 12 , a substrate layer 13 , a second adhesive layer 14 , and a second grid release layer 15 which are sequentially stacked from top to bottom.
[0068] Among them, the substrate layer is 36μm PET (hydrolysis-resistant PET, Dongcai, D269-UV), the first grid release layer is Degussa 7327 grid release film, the second grid release layer is Degussa 7309 grid release film, and the first adhesive layer and the second adhesive layer are prepared from an adhesive composition with a thickness of 82μm.
[0069] The adhesive composition comprises the following components by weight: 100 parts of acrylic resin (Kunshan Shimei, PS-8541), 5 parts of rosin resin (Kemao Chemical, 138), 10 parts of terpene resin (Arakawa Chemical, T-85), 12 parts of organic phosphate (Lingxing New Materials, RSF-11C), 20 parts of 30nm aluminum oxide (Deko Island Gold, DK410-1), 20 parts of 3μm aluminum oxide (Maoteng, AC-102G), 0.5 parts of dispersant (Yike Chemical, YCK-2440), 0.6 parts of coupling agent (Chengong Silicone, CG-560), 0.6 parts of epoxy curing agent (Lutian, L-70), and 70 parts of ethyl acetate.
[0070] The preparation method of the thermally conductive exhaust tape of this embodiment is as follows:
[0071] S1: Weigh 100 parts of acrylic resin PS-8541, 0.5 parts of YCK-2440 dispersant, 0.6 parts of CG-560 coupling agent and 70 parts of ethyl acetate, and stir at 800r / min for 10 minutes. Gradually add 5 parts of 138 resin and 10 parts of T-85 resin, and stir at 800r / min for 30 minutes. Keep stirring at high speed, and gradually add 12 parts of RSF-11C, 20 parts of DK410-1 and 20 parts of AC-102G. After all are added, the combined liquid is dispersed at 800r / min for 120 minutes.
[0072] S2: The combined liquid prepared in S1 was ground three times by a sand mill, and then filtered with a 400-mesh filter cloth to obtain a ground combined liquid.
[0073] S3: 0.6 parts of L-70 curing agent was added to the grinding combination liquid prepared in S2, and stirred at a speed of 300 r / min for 45 minutes to obtain an adhesive composition.
[0074] S4: The adhesive composition prepared in S3 is coated on a PET substrate, air-dried in an oven system, and then affixed with a 7327 mesh release film, which is rolled up to obtain a semi-finished product.
[0075] S5: The adhesive composition obtained in S3 is coated on a 7309 mesh release film, air-dried in an oven system, and then bonded to a semi-finished PET surface obtained in S4, which is then rolled up to obtain a thermally conductive exhaust tape.
[0076] Example 2
[0077] The structure of the thermally conductive exhaust tape, the composition of the adhesive composition and the method for preparing the tape in this embodiment are the same as those in Embodiment 1. The difference is that the thickness of the substrate layer is 50 μm, and the thickness of the first adhesive layer and the second adhesive layer are both 82 μm.
[0078] Example 3
[0079] The structure of the thermally conductive exhaust tape, the composition of the adhesive composition and the method for preparing the tape of this embodiment are the same as those of Embodiment 1. The difference is that the thickness of the substrate layer is 75 μm, and the thickness of the first adhesive layer and the second adhesive layer are both 62.5 μm.
[0080] Example 4
[0081] The structure and thickness of each layer of the heat-conducting exhaust tape of this embodiment are the same as those of Example 1, except that the adhesive composition comprises the following components by weight: 100 parts of acrylic resin (Kunshan Shimei, PS-8541), 5 parts of rosin resin (Kemao Chemical, 138), 10 parts of terpene resin (Arakawa Chemical, T-85), 12 parts of organic phosphate (Lingxing New Materials, RSF-11C), 28 parts of 30nm alumina (Deko Island Gold, DK410-1), 12 parts of 3μm alumina (Maoteng, AC-102G), 0.5 parts of dispersant (Yike Chemical, YCK-2440), 0.6 parts of coupling agent (Chengong Silicone, CG-560), 0.6 parts of epoxy curing agent (Lutian, L-70), and 70 parts of ethyl acetate. The components of the adhesive composition involved in the tape preparation method are replaced with the above amounts.
[0082] Comparative Example 1
[0083] The structure, thickness of each layer, composition of the adhesive composition and the method for preparing the thermally conductive exhaust tape of this comparative example are the same as those of Example 1. The difference is that the material of the substrate layer is ordinary PET (Xiangyu, PD-xy).
[0084] Comparative Example 2
[0085] The structure and thickness of each layer of the heat-conducting exhaust tape of this comparative example are the same as those of Example 1, except that the adhesive composition comprises the following components by weight: 100 parts of acrylic resin (Kunshan Shimei, PS-8541), 5 parts of rosin resin (Kemao Chemical, 138), 10 parts of terpene resin (Arakawa Chemical, T-85), 12 parts of organic phosphate (Lingxing New Materials, RSF-11C), 0.2 parts of dispersant (Yike Chemical, YCK-2440), 0.36 parts of coupling agent (Chengong Silicone, CG-560), 0.6 parts of epoxy curing agent (Lutian, L-70), and 35 parts of ethyl acetate. The components of the adhesive composition involved in the tape preparation method are replaced with the above amounts.
[0086] Comparative Example 3
[0087] The structure, thickness of each layer, composition of the adhesive composition and tape preparation method of the thermal conductive exhaust tape of this comparative example are the same as those of Example 1. The difference is that the materials of the release layers are different: the first release layer is Huamei HMX36T10 release film, and the second release layer is Huamei HMX50T30 release film.
[0088] Comparative Example 4
[0089] The structure of the heat-conducting exhaust tape, the composition of the adhesive composition and the method for preparing the tape in this comparative example are the same as those in Example 1. The difference is that the thickness of the substrate layer is 125 μm, and the thickness of the first adhesive layer and the second adhesive layer are both 37.5 μm.
[0090] Comparative Example 5
[0091] The structure and thickness of each layer of the heat-conducting exhaust tape of this comparative example are the same as those of Example 1, except that the adhesive composition comprises the following components by weight: 100 parts of acrylic resin (Kunshan Shimei, PS-8541), 5 parts of rosin resin (Kemao Chemical, 138), 10 parts of terpene resin (Arakawa Chemical, T-85), 12 parts of organic phosphate (Lingxing New Materials, RSF-11C), 40 parts of 3μm aluminum oxide (Mao Teng, AC-102G), 0.5 parts of dispersant (Yike Chemical, YCK-2440), 0.6 parts of coupling agent (Chengong Silicone, CG-560), 0.6 parts of epoxy curing agent (Lutian, L-70), and 70 parts of ethyl acetate. The components of the adhesive composition involved in the tape preparation method are replaced with the above amounts.
[0092] Results Analysis
[0093] The performance of the thermally conductive exhaust tapes in Examples 1-4 and Comparative Examples 1-5 was tested, including the thickness, peel force, dynamic shear strength, thermal conductivity, flame retardant grade, mechanical strength and aged mechanical strength of the tapes, and the results are shown in Table 1.
[0094] Table 1 Comparison of thermally conductive exhaust tape performance between the embodiment and the comparative example
[0095]
[0096]
[0097] As can be seen from the above table, the present invention can ensure that the tensile strength retention rate of the adhesive tape is greater than 60% after 2000 hours of double 85 aging by introducing hydrolysis-resistant PET, while the conventional PET substrate directly breaks. The grid release film is structurally designed to give the adhesive layer a structured exhaust channel, which is not only conducive to the flatness and beauty of the bonding interface after bubble removal, but also can improve the thermal conductivity of the tape to a certain extent. Through the reasonable design of the thickness of the tape substrate and the adhesive layer, the short-board effect caused by the low thermal conductivity of the plastic film can be greatly improved. At the same time, the micro-nano structure formed by nano- and micron-level thermal conductive materials forms a dense heat conduction channel inside the material, which can improve the thermal conductivity of the tape to a certain extent.
[0098] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from them are still within the protection scope of the invention.
Claims
1. A thermally conductive exhaust tape, It is characterized in that It comprises a first grid release layer, a first adhesive layer, a substrate layer, a second adhesive layer and a second grid release layer which are sequentially stacked; The substrate layer is made of hydrolysis-resistant insulating material, the material of the substrate layer is selected from PET, and the thickness of the substrate layer is 0.002-0.1 mm; the thickness of the first adhesive layer and the second adhesive layer are both 0.0625-0.15 mm; The first adhesive layer and the second adhesive layer are prepared from the following components in parts by weight: 50~100 parts of polymer resin; 5-25 parts of tackifying resin; Flame retardant 10~30 parts; Thermal conductive powder 20~100 parts; Dispersant 0.3~2.5 parts; Coupling agent 0.3~1.5 parts; Curing agent 0.05~2 parts; 30-100 parts of organic solvent; The release force of the first grid release layer is 2-8 g / 25 mm, and the thickness is 30-70 μm; the release force of the second grid release layer is 10-30 g / 25 mm, and the thickness is 80-130 μm; The first grid release layer and the second grid release layer both include a release film substrate layer, a microstructure coating layer and a release agent layer stacked in sequence; The thermal conductive powder is compounded by mixing particles with a particle size of 10-600nm and particles with a particle size of 1-15μm in a mass ratio of 1:4-5:1; the polymer resin is acrylic resin PS-8541; and the tackifying resin is rosin resin and terpene resin.
2. The thermally conductive exhaust tape according to claim 1, It is characterized in that The flame retardant is selected from one or more of phosphate compounds, organic nitrogen compounds, halogen compounds, phosphorus nitrogen compounds, dicyclopentadiene compounds, boron, antimony and aluminum inorganic compounds.
3. The thermally conductive exhaust tape according to claim 1, It is characterized in that The thermal conductive powder is one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride and silicon carbide.
4. A method for preparing the thermally conductive exhaust tape according to any one of claims 1 to 3, It is characterized in that The following steps are included: S1: Add 50-100 parts of polymer resin, 0.3-2.5 parts of dispersant, and 0.3-1.5 parts of coupling agent to 30-100 parts of organic solvent by weight, mix well, then add 5-25 parts of tackifying resin, 10-30 parts of flame retardant and 20-100 parts of thermal conductive powder, mix well to obtain a combined liquid; S2: grinding and filtering the combined liquid, and then adding 0.05 to 2 parts of a curing agent to obtain an adhesive composition; S3: coating the adhesive composition on one side of the substrate layer, and attaching the first grid release layer thereto after drying to obtain a semi-finished product; S4: coating the adhesive composition on the second grid release layer, and laminating the adhesive composition on the surface of the substrate layer of the semi-finished product after drying to obtain the thermally conductive exhaust tape.