A method for manufacturing non-quenched and tempered steel for engine crankshaft with tensile strength ≥1100MPa
Through smelting and process optimization, non-tempered steel for engine crankshafts with tensile strength ≥1100MPa was prepared, which solved the problem of insufficient tensile strength in the prior art and achieved improvements in high strength, toughness and hardening performance.
Patent Information
- Application Number
- CN202211536095.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-02
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2042-12-02
AI Technical Summary
In the prior art, the tensile strength of the non-tempered steel for engine crankshafts does not exceed 1000 MPa, and there is a lack of a method for manufacturing non-tempered steel for crankshafts with a strength of more than 1000 MPa.
Scrap steel and molten iron are used as raw materials, and pyrote is added to adjust the sulfur content in the molten steel, control the chemical composition of the steel, and heat it using continuous casting technology and step-by-step heating furnace, combining high-pressure water descaling and multiple rolling Process, control the cooling speed, and prepare non-tempered steel with tensile strength ≥1100MPa.
The tensile strength of the steel reaches ≥1100MPa, the yield strength is ≥735MPa, and the elongation is ≥12%, meeting the requirements of high strength, high toughness and good hardening properties.
Smart Images

Figure HDA0003977718190000011 
Figure HDA0003977718190000012 
Figure HDA0003977718190000021
Abstract
Description
Technical Field
[0001] The invention relates to the field of alloy steel manufacturing, in particular to a method for manufacturing non-quenched and tempered steel for high-strength crankshafts. Background Art
[0002] As a common key basic technology supporting the transformation of the automobile industry, lightweighting is a common choice for domestic and foreign automobile manufacturers to cope with energy challenges in the context of energy conservation and emission reduction, and is the only way for the sustainable development of the automobile industry.
[0003] In the process of vehicle lightweighting, engine lightweighting is one of the important contents. According to statistics, the weight of the engine accounts for about 12% of the weight of the vehicle. The lightweighting of the engine can improve the power of the vehicle, save materials, reduce manufacturing costs, and reduce fuel consumption and exhaust emissions. It has become a topic that cannot be ignored in vehicle development.
[0004] In an engine, the crankshaft mass accounts for about 10% of the engine mass. By using high-strength materials to "slim down" the crankshaft, the crankshaft design can be made more compact and miniaturized, and high power and high torque performance can be obtained, which helps to reduce the weight of the engine.
[0005] At present, engine crankshafts at home and abroad usually use ferrite + pearlite non-quenched and tempered steel materials with a tensile strength level of 800-900MPa. After searching:
[0006] The Chinese patent with the authorization announcement number CN 104264040B and the announcement date of October 5, 2016, entitled "A non-quenched and tempered steel and a method for manufacturing the same, and a crankshaft manufactured using the non-quenched and tempered steel", discloses a non-quenched and tempered steel material for an engine crankshaft. The chemical composition of the steel is as follows: C: 0.37-0.43%, Si: 0.55-0.65%, Mn: 1.46-1.56%, V: 0.07-0.13%, Nb: 0.015-0.035%, N: 0.012-0.017%, and the remainder is iron and other unavoidable impurities; the steel has a tensile strength ≥880MPa and a yield strength ≥550MPa.
[0007] The Chinese patent document with application publication number CN 112372253A and publication date 2021.02.19 and titled “A method for preparing a non-quenched and tempered steel for an engine crankshaft and a forging thereof” discloses a non-quenched and tempered steel material for an engine crankshaft, the chemical composition of the steel material being as follows: C: 0.37-0.42; Si: 0.50-0.65; Mn: 1.30-1.50; S: 0.045-0.060; Ni: 0.120-0.150; P: 0.010~0.025; Cr: 0.10~0.20; Mo: 0.015~0.050; Cu: 0.03~0.20; Ni: 0.120~0.150; V: 0.08~0.13; Al: 0.010~0.015; Ti: ≤0.010; N: ≥150ppm; aluminum-nitrogen ratio ≤1, titanium-nitrogen ratio ≤0.67; the tensile strength of the steel is greater than 900MPa, and the yield strength is greater than 580MPa.
[0008] The Chinese patent document with application publication number CN 113862576A and publication date of December 31, 2021, and titled "A non-quenched and tempered steel, crankshaft and production method thereof", discloses a non-quenched and tempered steel material for an engine crankshaft, the chemical composition of the steel being as follows by mass percentage: C: 0.45-0.51%, Si: 0.20-0.37%, Mn: 1.00-1.20%, P: ≤0.025%, S: 0.010-0.035%, Cr: 0.05-0.25%, V: 0.05-0.10%, Ni: ≤0.20%, Cu: ≤0.20%, Mo: ≤0.04%, N: 0.008-0.020%, Ti: 0.010-0.025%, and the rest being Fe and unavoidable impurities; the steel has a tensile strength ≥820MPa and a yield strength ≥500MPa.
[0009] The tensile strength of the above-disclosed non-quenched and tempered steels for crankshafts does not exceed 1000 MPa, and there is a lack of non-quenched and tempered steels for crankshafts with a strength of more than 1000 MPa in the market. Summary of the invention
[0010] The object of the present invention is to provide a method for manufacturing non-quenched and tempered steel for engine crankshafts with a tensile strength of ≥1100 MPa, wherein the prepared steel has a higher tensile strength.
[0011] The technical solution adopted by the present invention to solve the above problem is: a method for manufacturing non-quenched and tempered steel for engine crankshaft with tensile strength ≥1100MPa, comprising:
[0012] Step 1, smelting: using scrap steel and molten iron as raw materials, and adding pyrite to adjust the sulfur content in the molten steel, and adjusting the composition of the molten steel with reference to the chemical composition of the steel. The chemical composition of the steel is C: 0.42-0.50%, Si: 0.60-0.80%, Mn: 1.40-1.65%, P: ≤0.015%, S: 0.060-0.090%, Cr: 0.20-0.30%, Ni: 0.10-0.25%, Al: 0.010-0.030%, Ti: 0.015-0.025%, V: 0.15-0.25%, N: 0.015-0.022%, B: 0.0005-0.0025%, and the balance is Fe and unavoidable impurity elements;
[0013] Step 2, continuous casting: Use continuous casting process to cast square continuous casting billets with specifications of 300mm×300mm or above, and control the casting superheat at 20-35℃. Electromagnetic stirring of the crystallizer and the end of the continuous casting process are used to improve the surface and internal quality of the billet;
[0014] Step 3, heating: use a walking beam heating furnace to heat the ingot, the preheating section temperature is controlled at 680-850°C, the heating section temperature is controlled at 1000-1060°C, the soaking section temperature is controlled at 1140-1200°C, the total heating time is more than 380 minutes, of which the preheating section time is ≥120 minutes;
[0015] Step 4, rolling: after the ingot is out of the heating furnace, high-pressure water is used to descale it, the rolling temperature is 1000-1030°C, 6 initial rolling mills + 6 intermediate rolling mills + 6 finishing rolling mills are used for rolling, and the final rolling temperature is controlled at 930-960°C, and the round steel with a specification of φ80-130mm is rolled;
[0016] Step 5, cooling: After rolling, cool on the cooling bed, control the step speed to make the cooling rate 0.4 ~ 0.8 ℃ / s, and ensure that the temperature of the lower cooling bed is ≤ 550 ℃.
[0017] Preferably, the chemical composition of the steel is C: 0.43-0.47%, Si: 0.70-0.78%, Mn: 1.50-1.60%, P: ≤0.012%, S: 0.065-0.075%, Cr: 0.22-0.28%, Ni: 0.12-0.16%, Al: 0.016-0.022%, Ti: 0.015-0.020%, V: 0.18-0.20%, N: 0.016-0.020%, B: 0.0015-0.0020%, and the remainder is Fe and unavoidable impurity elements.
[0018] The chemical composition design of the non-quenched and tempered steel for the engine crankshaft with a tensile strength of ≥1100MPa of the present invention is determined as follows: C is the most basic and effective strengthening element in steel, and its use cost is the most economical. Considering that the crankshaft surface needs to be subjected to medium-frequency induction quenching treatment, in order to ensure that the material has sufficient strength / hardness and hardenability while taking into account a certain plasticity, C is determined to be 0.42-0.50%, and preferably C is 0.43-0.47%.
[0019] Si can be used as a deoxidizer and a reducing agent in the steelmaking process. At the same time, Si has a strong solid solution strengthening effect in steel, which can significantly improve the elastic limit, yield strength and tensile strength of steel, especially the yield strength. The fatigue strength of the crankshaft requires a high yield strength ratio. Therefore, Si is one of the key elements in the crankshaft material. Si is determined to be 0.60-0.80%, and Si is preferably 0.70-0.78%.
[0020] Mn is an effective element for deoxidation and desulfurization in steel, which improves the strength and hardness of steel, significantly improves the hardenability of steel, and improves the hot processing performance of steel; at the same time, Mn is the element with the strongest binding force with S in steel, and the formed MnS compound helps to improve the cutting performance of steel. Mn is determined to be 1.40-1.65%, and Mn is preferably 1.50-1.60%.
[0021] P is a harmful impurity in steel, and is an element with a low melting point and easy to segregate. Its content in steel needs to be controlled to determine P: ≤ 0.015%, preferably P: ≤ 0.012%.
[0022] S is also usually a harmful impurity in steel, but it can significantly improve the cutting performance of steel when it reaches a certain content. While the strength of the steel of the present invention is improved, it is bound to cause deterioration of the cutting performance during processing. For this reason, S element is artificially added, and S: 0.060~0.090%, preferably S: 0.065~0.075%.
[0023] Cr can effectively improve the hardenability of steel to obtain the required strength and reduce the tendency of surface decarburization during heating of steel. However, since it is a strong carbide precipitation element, it will affect the performance of the induction quenching layer. Therefore, the content cannot be too high. It is determined that: Cr: 0.20~0.30%, preferably Cr: 0.22~0.28%.
[0024] Ni can improve the strength of steel while ensuring good plasticity / toughness, but the resource is scarce and the cost is high. Therefore, Ni is determined to be 0.10-0.25%, and Ni is preferably 0.12-0.16%.
[0025] Al is an effective deoxidizer. The AlN formed can refine the grains. When the content is low, the effect is not obvious. When the content is high, it is easy to form coarse inclusions and deteriorate the performance of the steel. Determine Al: 0.010~0.030%:, preferably 0.016~0.022%
[0026] Ti and N have a strong bonding force, and the formed TiN particles can pin the grain boundary and inhibit the growth of grains during crankshaft forging. The Ti content is determined to be 0.015-0.025%, and preferably Ti content is 0.015-0.020%.
[0027] V has a high solubility in steel and is one of the most commonly used and effective strengthening elements for non-quenched and tempered steel. It affects the structure and properties of steel by forming V (C, N) compounds that precipitate at grain boundaries, thereby refining ferrite grains and improving the strength and toughness of steel. V and Ni are also precious alloys. V is determined to be 0.15-0.25%, and V is preferably 0.18-0.20%.
[0028] N is a common element in non-quenched and tempered steel. It mainly enhances the precipitation strengthening effect and refines the grains, increases the N content in the steel, expands the precipitation range of carbonitrides, and improves the effective effect of microalloying elements. The same mechanical properties can be obtained with a smaller content of microalloying elements. N is determined to be 0.015-0.022%, preferably N: 0.016-0.020%. The molten steel can be nitrogen-added by blowing nitrogen.
[0029] The design principle of the chemical composition system of the present application is: under certain nitrogen content conditions, V / Ti element composite microalloying is used while adding a trace amount of B element, so as to give full play to the role of B element in stabilizing austenite and improving phase transformation / precipitation strengthening effect, and the improvement of hardenability by a trace amount of B element can also increase the depth of the crankshaft quenching layer, thereby improving the fatigue strength of the crankshaft. B is determined to be 0.0005-0.0025%, and B is preferably 0.0015-0.0020%.
[0030] Compared with the prior art, the advantages of the present invention are: the steel microstructure obtained according to the above method is uniform ferrite + pearlite, the tensile strength is ≥1100MPa, the yield strength is ≥735MPa, the elongation is ≥12%, and the crankshaft produced by forging technology also meets the above mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The chemical composition of the steel corresponding to Examples 1-3 of the present invention;
[0032] Figure 2 The steel microstructure diagram 100× obtained in Example 1 of the present invention (ferrite ratio 11.14%);
[0033] Figure 3 The steel microstructure diagram 100× obtained in Example 2 of the present invention (ferrite ratio 9.94%);
[0034] Figure 4 The steel microstructure diagram 100× obtained in Example 3 of the present invention (ferrite ratio 8.39%);
[0035] Figure 5 The electrolyte quantity result of the small sample of sulfide inclusions in the non-quenched and tempered steel for crankshafts involved in the present invention is 100×;
[0036] Figure 6 The mechanical properties of the steel corresponding to Examples 1-3 of the present invention simulate the crankshaft forging. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0038] Use Figure 1 The chemical composition shown in FIG. 3 is used to produce the high-strength non-quenched and tempered steel for crankshafts of the present invention;
[0039] Ceq=C+Si / 7+Mn / 5+Cr / 9+V / 2+Ni / 22+Cu / 9
[0040] The non-quenched and tempered steel for engine crankshaft with tensile strength ≥1100MPa is manufactured according to the following production process:
[0041] Smelting
[0042] Scrap steel and molten iron are used as raw materials, with the molten iron ratio being around 50%, and pyrite is added to minimize the amount of ferropyrite alloy and ferropyrite wire added in the later stage, thereby reducing production costs. The molten steel after initial refining in a 100-ton electric furnace is refined outside the furnace and then degassed, and the mass percentage of each chemical element is strictly controlled and implemented in accordance with standard requirements.
[0043] Continuous Casting
[0044] A 300mm×300mm square continuous casting machine was used for casting, and the casting superheat was controlled at 20-35°C. Electromagnetic stirring of the crystallizer and the end electromagnetic stirring were adopted to improve the surface and internal quality of the ingot.
[0045] heating
[0046] Use a walking beam heating furnace to heat the ingot, with the temperature of the preheating section controlled at 680-850°C, the temperature of the heating section controlled at 1000-1060°C, the temperature of the soaking section controlled at 1140-1200°C, and the total heating time of 380 minutes or more, of which the preheating section time must be ≥120 minutes to ensure that the ingot heats up slowly and is heated sufficiently and evenly.
[0047] Rolling
[0048] After the ingot leaves the heating furnace, it is descaled with high-pressure water, the starting rolling temperature is 1000-1030°C, and then it is rolled using 6 primary rolling mills + 6 intermediate rolling mills + 6 finishing rolling mills, with the final rolling temperature controlled at 930-960°C; the maximum rolling specification is φ130mm.
[0049] cool down
[0050] After rolling, place the machine on the cooling bed and control the step speed so that the cooling rate is controlled at 0.4-0.8℃ / s to ensure that the temperature of the lower cooling bed is ≤550℃.
[0051] The engine crankshaft with tensile strength ≥1100MPa obtained in Example 1-3 was forged with non-quenched and tempered steel to simulate crankshaft forging, that is, the φ130mm steel was forged into φ50mm sample bars and then the mechanical properties were tested. The results are as follows: Figure 6 .
[0052] Depend on Figure 6 It can be seen from the properties shown that the mechanical properties of the materials manufactured in Examples 1-3 all meet the design requirements of the invention, and a non-quenched and tempered steel for engine crankshafts with a tensile strength ≥1100MPa is obtained, and the manufacturing process is simple, which has high application value and advantages in the field of non-quenched and tempered steel for crankshafts.
[0053] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.
Claims
1. A method for manufacturing non-quenched and tempered steel for engine crankshaft with tensile strength ≥1100MPa, characterized in that: include, Step 1, smelting: using scrap steel and molten iron as raw materials, and adding pyrite to adjust the sulfur content in the molten steel, and regulating the composition of the molten steel with reference to the chemical composition of the steel. The chemical composition of the steel is C: 0.43-0.47%, Si: 0.70-0.78%, Mn: 1.50-1.60%, P: ≤0.012%, S: 0.065-0.075%, Cr: 0.22-0.28%, Ni: 0.12-0.16%, Al: 0.016-0.022%, Ti: 0.015-0.020%, V: 0.18-0.20%, N: 0.016-0.020%, B: 0.0015-0.0020%, and the balance is Fe and unavoidable impurity elements; Step 2, continuous casting: Use continuous casting process to cast square continuous casting billets with specifications of 300mm×300mm or above, and control the casting superheat at 20-35℃. Electromagnetic stirring of the crystallizer and the end of the continuous casting process are used to improve the surface and internal quality of the billet; Step 3, heating: use a walking beam heating furnace to heat the ingot, the preheating section temperature is controlled at 680-850°C, the heating section temperature is controlled at 1000-1060°C, the soaking section temperature is controlled at 1140-1200°C, the total heating time is more than 380 minutes, of which the preheating section time is ≥120 minutes; Step 4, rolling: after the ingot is out of the heating furnace, high-pressure water is used to descale it, the rolling temperature is 1000-1030°C, 6 initial rolling mills + 6 intermediate rolling mills + 6 finishing rolling mills are used for rolling, and the final rolling temperature is controlled at 930-960°C, and the round steel with a specification of φ80-130mm is rolled; Step 5, cooling: After rolling, cool on the cooling bed, control the step speed so that the cooling rate is 0.4-0.8℃ / s, and ensure that the temperature of the lower cooling bed is ≤550℃; the obtained steel microstructure is uniform ferrite + pearlite, the tensile strength is ≥1100MPa, the yield strength is ≥735MPa, and the elongation is ≥12%. The crankshaft produced by the forging process also meets the above mechanical properties.
Citation Information
Patent Citations
Non-quenched and tempered steel, its manufacturing method, and crankshaft made of the non-quenched and tempered steel
CN104264040B
Steel for non-quenched-and-tempered crankshaft of engine and preparation method of forging of steel
CN112372253A
Non-quenched and tempered steel, crankshaft and production method of crankshaft
CN113862576A
High strength fracture splitting connecting rod non-quenched and tempered steel and continuous casting production process thereof
CN109252097A
Non-quenched and tempered steel motor shaft and machining method thereof
CN109759779A