An ultrafiltration membrane based on polyionic liquid brush functionalization and its preparation method and application

By forming a polyionic liquid brush on the surface of the PVDF ultrafiltration membrane, it solves the problems of reduced flux and shortened lifespan of existing membrane technology in organic and biological pollution, achieves improved antibacterial and anti-pollution performance, and is suitable for wastewater treatment.

CN116212637BActive Publication Date: 2024-10-01UNIV OF SCI & TECH OF CHINA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202211570545.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-08
Publication Date
2024-10-01
Estimated Expiration
2042-12-08

AI Technical Summary

Technical Problem

Existing membrane technology is difficult to achieve both antibacterial properties and high flux when faced with organic and biological pollution, and the introduction of antibacterial agents can easily affect the anti-organic/biological effects of the membrane, resulting in shortened membrane life and high energy consumption.

Method used

An ultrafiltration membrane based on polyionic liquid brush functionalization is used to generate an α-bromoisobutyl functionalized dopamine initiator through the reaction of dopamine and α-bromoisobutyryl bromide, and the buffer and ionic liquid are combined to perform atom transfer radical polymerization. , forming a polyionic liquid brush, fixed on the surface of the PVDF ultrafiltration membrane, enhancing its antibacterial and anti-pollution properties.

Benefits of technology

It has been achieved that while maintaining high flux, it can significantly improve the membrane's anti-biological and organic pollution performance, extend the membrane life, reduce energy consumption, and verify its effectiveness through actual water treatment experiments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116212637B_ABST
    Figure CN116212637B_ABST
Patent Text Reader

Abstract

The present invention provides an ultrafiltration membrane based on polyionic liquid brush functionalization and its preparation method and application. The preparation method provided by the present invention comprises the following steps: firstly reacting dopamine with α-bromoisobutyryl bromide to obtain an α-bromoisobutyl functionalized dopamine initiator; then diluting the α-bromoisobutyl functionalized dopamine initiator with a buffer to obtain an α-bromoisobutyl functionalized dopamine initiator dilution; then, applying the α-bromoisobutyl functionalized dopamine initiator dilution to the surface of an ultrafiltration membrane for reaction to obtain an ultrafiltration membrane with initiation sites on the surface; finally, applying a certain ionic liquid mixture to the surface of the ultrafiltration membrane with initiation sites on the surface to perform an atom transfer radical polymerization reaction to obtain an ultrafiltration membrane based on polyionic liquid brush functionalization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of membrane technology, and in particular to an ultrafiltration membrane based on polyionic liquid brush functionalization and a preparation method and application thereof. Background Art

[0002] Membrane separation technology has been widely used in water and wastewater treatment processes. However, membranes encounter organic and biological fouling during long-term operation. The formation of biological fouling is complex, among which the adhesion of microorganisms and organic molecules plays a vital role. More seriously, the attached organic pollutants and microorganisms lead to problems such as decreased membrane flux, frequent membrane cleaning, high energy consumption, and shortened membrane life. Therefore, developing functionalized membranes that can resist the adhesion of organic and biological molecules and kill bacteria at the same time is a more attractive strategy.

[0003] Zwitterionic polymers can delay the attachment of microorganisms to the membrane surface, but they cannot inactivate bacterial cells. Therefore, related studies have used antimicrobial agents such as cationic polymers, carbon-based nanomaterials, silver and zwitterionic polymers to prepare diblock functional membranes to achieve a strategy that combines "defense" and "attack". However, it is worth noting that for the actual membrane filtration process, the barrier of water passing through the long polymer brush functionalized membrane is not offset by the change in the hydrophilicity of the long polymer brushes. Therefore, hydrophilic cationic polymers may become a material that delays membrane biofouling. However, in actual research and development, it is often difficult to achieve both organic and biological fouling and killing bacteria at the same time. If antibacterial substances are introduced to improve antibacterial properties, it is easy to affect the membrane flux and anti-organic / biological effects, making the development of membranes with the above effects face greater challenges. Summary of the invention

[0004] In view of this, the present invention provides an ultrafiltration membrane based on polyionic liquid brush functionalization and its preparation method and application. The ultrafiltration membrane based on polyionic liquid brush functionalization provided by the present invention can not only effectively improve the antibacterial property of the membrane, but also effectively resist biological and organic pollution, maintain a high flux in the face of biological and organic pollution, and reduce the damage of biological and organic pollution to the membrane flux.

[0005] The present invention provides a method for preparing an ultrafiltration membrane based on polyionic liquid brush functionalization, comprising the following steps:

[0006] a) reacting dopamine with α-bromoisobutyryl bromide to obtain an α-bromoisobutyl functionalized dopamine initiator reaction solution;

[0007] b) mixing the α-bromoisobutyl functionalized dopamine initiator reaction solution with a buffer solution to obtain an α-bromoisobutyl functionalized dopamine initiator dilution solution;

[0008] c) applying the α-bromoisobutyl functionalized dopamine initiator dilution to the surface of an ultrafiltration membrane for reaction to obtain an ultrafiltration membrane with initiation sites on the surface;

[0009] d) applying the ionic liquid mixture to the surface of the ultrafiltration membrane with initiation sites on the surface to carry out an atom transfer radical polymerization reaction to obtain an ultrafiltration membrane functionalized with a polyionic liquid brush;

[0010] in,

[0011] The ionic liquid mixed solution comprises: an ionic liquid, a solvent and an additive;

[0012] The ionic liquid is a tetrafluoroborate ionic liquid; and the alkyl chain of the cation in the ionic liquid is a C4 alkyl chain;

[0013] The additives are reducing agents and ligands.

[0014] Preferably, in step d), the ionic liquid is 1-butyl-3-methylimidazolium tetrafluoroborate.

[0015] Preferably, in step d), the atom transfer radical polymerization reaction time is 6 to 12 hours.

[0016] Preferably, in step c), the reaction time is 10 to 90 minutes.

[0017] Preferably, in step a), the molar ratio of dopamine:α-bromoisobutyryl bromide is preferably (1-3.15):1.05.

[0018] Preferably, in step a), the reaction is carried out in the presence of an acid binding agent;

[0019] The acid binding agent is at least one of triethylamine, pyridine and sodium carbonate.

[0020] Preferably, the dosage ratio of dopamine in step a) to the buffer in step b) is preferably 2.1 mmol to (50-150) mL.

[0021] Preferably, in step c), pouring the α-bromoisobutyl functionalized dopamine initiator dilution onto the surface of the ultrafiltration membrane; specifically comprising: preparing an ultrafiltration membrane fixture before step b), and immediately and rapidly pouring the α-bromoisobutyl functionalized dopamine initiator dilution into the ultrafiltration membrane fixture after obtaining the α-bromoisobutyl functionalized dopamine initiator dilution in step b);

[0022] The ultrafiltration membrane fixture is prepared by the following method: attaching the ultrafiltration membrane to a substrate, and then fixing the ultrafiltration membrane to the substrate with a frame.

[0023] The present invention also provides an ultrafiltration membrane based on polyionic liquid brush functionalization obtained by the preparation method described in the above technical solution.

[0024] The present invention also provides an application of the ultrafiltration membrane based on polyionic liquid brush functionalization described in the above technical solution in wastewater treatment.

[0025] The preparation method provided by the invention comprises the following steps: firstly reacting dopamine with α-bromoisobutyryl bromide to obtain an α-bromoisobutyl functionalized dopamine initiator; then diluting the α-bromoisobutyl functionalized dopamine initiator with a buffer to obtain a diluted α-bromoisobutyl functionalized dopamine initiator solution; then applying the diluted α-bromoisobutyl functionalized dopamine initiator solution to the surface of an ultrafiltration membrane for reaction to obtain an ultrafiltration membrane with initiation sites on the surface; and finally applying a certain ionic liquid mixed solution to the surface of the ultrafiltration membrane with initiation sites on the surface to perform an atom transfer radical polymerization reaction to obtain an ultrafiltration membrane based on polyionic liquid brush functionalization. The present invention uses dopamine and α-bromoisobutyryl bromide to react to obtain α-bromoisobutyl functionalized dopamine initiator, treats and reacts the surface of an ultrafiltration membrane with the specific initiator, forms a specific linker and initiation site on the surface of the ultrafiltration membrane, and then introduces a specific ionic liquid to the surface of the ultrafiltration membrane. Under the action of the specific linker at the initiation site, an atom transfer radical polymerization reaction is performed to fix the polyionic liquid brush on the membrane surface. The polyvinylidene fluoride anti-biological and organic dual-pollution ultrafiltration membrane based on the surface modification of the polyionic liquid brush of the present invention fixes a certain hydrophilic polyionic liquid brush on the membrane surface by the ATRP technology, giving the PVDF ultrafiltration membrane excellent antibacterial properties without losing the hydrophilicity of the membrane surface; the polyionic liquid brush fixed on the membrane surface can prevent bacteria from adhering to the membrane surface to achieve the purpose of "defense". Compared with the original ultrafiltration membrane, the ultrafiltration membrane functionalized with polyionic liquid brush finally obtained by the present invention has improved anti-biological and anti-organic pollution performance during the dynamic filtration process. The actual water treatment experiment further proves the practical application value of the prepared ultrafiltration membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0027] Figure 1 It is the surface morphology structure diagram of the film samples obtained in Comparative Examples 1-2 and Example 1; wherein, Figure 1 (a) is the surface morphology structure diagram of the film sample obtained in Comparative Example 1, Figure 1 (b) is the surface morphology structure diagram of the film sample obtained in Comparative Example 2, Figure 1 (c) is a surface morphology structure diagram of the film sample obtained in Example 1;

[0028] Figure 2 It is the Fourier infrared transform spectrum of the film samples obtained in Comparative Examples 1-2 and Example 1; wherein, Figure 2 (a) is the Fourier transform infrared spectrum of the film sample obtained in Comparative Example 1, Figure 2 (b) is the Fourier transform infrared spectrum of the film sample obtained in Comparative Example 2, Figure 2 (c) is the Fourier transform infrared spectrum of the film sample obtained in Example 1;

[0029] Figure 3 The antibacterial test results of the film samples obtained in Comparative Examples 1-2 and Example 1 are shown;

[0030] Figure 4 The water flux test effect diagram of the membrane samples obtained in Comparative Examples 1-2 and Example 1;

[0031] Figure 5 The anti-biological fouling performance test results of the membrane samples obtained in Comparative Examples 1-2 and Example 1 are shown in FIG.

[0032] Figure 6 The results of the test of the anti-organic pollution performance of the membrane samples obtained in Comparative Examples 1-2 and Example 1 are shown;

[0033] Figure 7 The actual wastewater filtration performance test effect diagram of the membrane samples obtained in Comparative Example 1 and Example 1;

[0034] Figure 8 The figure is a synthetic route diagram of the preparation method of the present invention. DETAILED DESCRIPTION

[0035] The present invention provides a method for preparing an ultrafiltration membrane based on polyionic liquid brush functionalization, comprising the following steps:

[0036] a) reacting dopamine with α-bromoisobutyryl bromide to obtain an α-bromoisobutyl functionalized dopamine initiator reaction solution;

[0037] b) mixing the α-bromoisobutyl functionalized dopamine initiator reaction solution with a buffer solution to obtain an α-bromoisobutyl functionalized dopamine initiator dilution solution;

[0038] c) applying the α-bromoisobutyl functionalized dopamine initiator dilution to the surface of an ultrafiltration membrane for reaction to obtain an ultrafiltration membrane with initiation sites on the surface;

[0039] d) applying the ionic liquid mixture to the surface of the ultrafiltration membrane with initiation sites on the surface to carry out an atom transfer radical polymerization reaction to obtain an ultrafiltration membrane based on polyionic liquid brush functionalization;

[0040] in,

[0041] The ionic liquid solution comprises: an ionic liquid, a solvent and an additive;

[0042] The ionic liquid is at least one of a tetrafluoroborate ionic liquid, a hexafluorophosphate ionic liquid and a bromide ionic liquid; and the alkyl chain of the cation in the ionic liquid is a C4 alkyl chain;

[0043] The additives are reducing agents and ligands.

[0044] Regarding step a) :

[0045] a) dopamine reacts with α-bromoisobutyryl bromide to obtain an α-bromoisobutyl functionalized dopamine initiator reaction solution.

[0046] In the present invention, the sources of dopamine (DA) and α-bromoisobutyryl bromide (BIBB) are not particularly limited, and they can be commercial products. In the present invention, the molar ratio of dopamine: α-bromoisobutyryl bromide is preferably (1-3.15): 1.05, specifically 1.0: 1.05, 1.5: 1.05, 2.0: 1.05, 2.1: 1.05, 2.5: 1.05, 3.0: 1.05, 3.15: 1.05, and more preferably 2.1: 1.05.

[0047] In the present invention, the temperature of the reaction is not particularly limited, and it can be carried out at room temperature, which can be 20 to 30°C, specifically 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C. In the present invention, the reaction time is preferably 0.5 to 3.5h, specifically 0.5h, 1.0h, 1.5h, 2.0h, 2.5h, 3.0h, 3.5h, and more preferably 3h. In the present invention, the reaction process is preferably accompanied by stirring. The stirring rate is preferably 50 to 100rpm, specifically 50rpm, 60rpm, 70rpm, 80rpm, 90rpm, 100rpm.

[0048] In the present invention, the reaction is preferably carried out in the presence of an acid binding agent. In the present invention, the acid binding agent is preferably at least one of triethylamine (TEA), pyridine and sodium carbonate. In the present invention, the molar ratio of the acid binding agent: α-bromoisobutyryl bromide is preferably (1-3): 1.05, specifically 1.00: 1.05, 1.05: 1.05, 1.50: 1.05, 2.00: 1.05, 2.50: 1.05, 3.00: 1.05, more preferably 1.05: 1.05.

[0049] In the present invention, the reaction is preferably carried out in an organic solvent medium. The organic solvent is preferably at least one of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) and tetrahydrofuran (THF). In the present invention, the amount ratio of the solvent: dopamine is preferably (10-30) mL: 2.1 mmol, specifically 10 mL: 2.1 mmol, 15 mL: 2.1 mmol, 20 mL: 2.1 mmol, 25 mL: 2.1 mmol, 30 mL: 2.1 mmol, more preferably 20 mL: 2.1 mmol.

[0050] In the present invention, the reaction is preferably carried out under protective atmosphere conditions. In the present invention, the type of gas providing the protective atmosphere is not particularly limited, and it can be a conventional protective gas well known to those skilled in the art, such as nitrogen or argon. The protective gas is a high-purity gas with a purity of ≥99.99%. Specifically, the protective gas is introduced into the reaction vessel to replace the air and form a protective atmosphere in the reaction vessel.

[0051] In the present invention, step a) preferably specifically includes: putting dopamine and an organic solvent into a reaction vessel, and passing high-purity nitrogen; the passing time is preferably 30 minutes; vacuuming during freezing, and passing nitrogen to prevent the solvent from coming out during thawing; specifically, when high-purity nitrogen is added to the reaction vessel for 30 minutes, the temperature of the entire system is reduced and frozen, and then the nitrogen blowpipe is replaced with a three-way port and the remaining oxygen in the bottle is pumped out with a water pump, and then thawing occurs in the system. Then, an acid binding agent and α-bromoisobutyryl bromide are added, and high-purity nitrogen is continued to be passed, and the reaction is carried out at room temperature under stirring conditions to generate an α-bromoisobutyl functionalized dopamine initiator, and the system is obtained. The reaction liquid containing the α-bromoisobutyl functionalized dopamine initiator. Among them, the amount ratio between the substances, the reaction conditions, etc. are consistent with those described above.

[0052] Regarding step b) :

[0053] b) mixing the α-bromoisobutyl functionalized dopamine initiator reaction solution with a buffer solution to obtain an α-bromoisobutyl functionalized dopamine initiator dilution solution.

[0054] In the present invention, the buffer solution is also called a buffer solution, preferably a Tris-HCl buffer solution, and the pH value of the Tris-HCl buffer solution is 8.5. The source of the Tris-HCl buffer solution is not particularly limited in the present invention, and it can be a commercial product.

[0055] In the present invention, the dosage ratio of dopamine in step a) to buffer in step b) is preferably 2.1 mmol: (50-150) mL, specifically 2.1 mmol: 50 mL, 2.1 mmol: 100 mL, 2.1 mmol: 150 mL, and more preferably 2.1 mmol: 100 mL.

[0056] The present invention has no particular restrictions on the manner of mixing the α-bromoisobutyl functionalized dopamine initiator and the buffer solution, and the materials can be mixed uniformly according to conventional mixing methods in the art, such as stirring and mixing. After mixing, a diluted α-bromoisobutyl functionalized dopamine initiator solution is obtained.

[0057] Regarding step c) :

[0058] c) applying the α-bromoisobutyl functionalized dopamine initiator dilution solution to the surface of an ultrafiltration membrane for reaction to obtain an ultrafiltration membrane with initiation sites on the surface.

[0059] In the present invention, the ultrafiltration membrane is preferably a polymer ultrafiltration membrane, more preferably a polyvinylidene fluoride (PVDF) ultrafiltration membrane. In the present invention, the PVDF ultrafiltration membrane is preferably an ultrafiltration membrane with a molecular weight cutoff of 100 to 250 kDa, specifically 100 kDa, 150 kDa, 200 kDa, 250 kDa. The present invention has no special restrictions on the source of the ultrafiltration membrane, and it can be a commercial product, such as a commercial PVDF ultrafiltration membrane.

[0060] In the present invention, the ultrafiltration membrane is preferably pretreated before use, that is, a pretreated ultrafiltration membrane is used. In the present invention, the pretreatment preferably includes: first soaking the ultrafiltration membrane in anhydrous ethanol, then ultrasonically cleaning it with deionized water, then rinsing it with deionized water, and then soaking it in deionized water for standby use, and then taking it out at any time when using it. Among them, the soaking time in anhydrous ethanol is preferably 10 to 30 minutes, specifically 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, and more preferably 20 minutes. The conditions for the ultrasonic cleaning are preferably: power 40 to 100W, specifically 40W, 50W, 60W, 70W, 80W, 90W, 100W, and more preferably 80W; time 10 to 60 minutes, specifically 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, and more preferably 30 minutes.

[0061] In the present invention, the method of applying the α-bromoisobutyl functionalized dopamine initiator dilution to the surface of the ultrafiltration membrane is preferably: pouring the α-bromoisobutyl functionalized dopamine initiator dilution on the surface of the ultrafiltration membrane. Specifically, an ultrafiltration membrane fixture is prepared in advance, and after obtaining the α-bromoisobutyl functionalized dopamine initiator dilution in step b), it is immediately and quickly poured into the ultrafiltration membrane fixture. In the present invention, the ultrafiltration membrane fixture is preferably prepared in the following manner: the ultrafiltration membrane is attached to a substrate, and then the ultrafiltration membrane is fixed to the substrate with a frame, and then the α-bromoisobutyl functionalized dopamine initiator dilution is poured into the frame to fully immerse the ultrafiltration membrane surface. Among them, before attaching the ultrafiltration membrane to the substrate, the ultrafiltration membrane is preferably cut first. The substrate is preferably a glass sheet. The frame is preferably a Teflon frame, and the ultrafiltration membrane is fixed on the substrate by the frame, similar to the pattern of a photo frame. Since the frame is raised, it is equivalent to forming a shallow groove on the surface of the ultrafiltration membrane, and then the α-bromoisobutyl functionalized dopamine initiator dilution is poured into the frame to fully impregnate the ultrafiltration membrane. In the present invention, the timing of pre-preparing the ultrafiltration membrane fixture is preferably after step a) obtaining the α-bromoisobutyl functionalized dopamine initiator and before step b) preparing the α-bromoisobutyl functionalized dopamine initiator dilution.

[0062] In the present invention, after the α-bromoisobutyl functionalized dopamine initiator dilution is applied to the surface of the ultrafiltration membrane, it is allowed to stand for reaction. The temperature conditions of the reaction are not particularly limited, and it can be carried out at room temperature, which can be 20 to 30°C, specifically 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C. The reaction time is preferably 10 to 90 minutes, specifically 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 60 minutes, 70 minutes, 80 minutes, 90 minutes, and more preferably 30 minutes. After the above reaction, excess dopamine self-polymerizes on the membrane surface and covalently binds to the α-bromoisobutyl functionalized dopamine initiator in the reaction solution to obtain an ultrafiltration membrane with initiation sites on the surface.

[0063] The dopamine added in the present invention is excessive. In the above reaction process, dopamine reacts with α-bromoisobutyl bromide to form an α-bromoisobutyl functionalized dopamine initiator reaction solution, the reaction solution is diluted into a Tris-HCl solution, the excessive dopamine self-polymerizes in a Tris-HCl buffer solution with a pH of 8.5 to form polydopamine, and covalently combines with the α-bromoisobutyl functionalized dopamine initiator solution, and the initiator is fixed on the surface of the PVDF membrane by utilizing the viscosity of dopamine, that is, the polydopamine is mainly self-polymerized to form the polydopamine, and the α-bromoisobutyl functionalized dopamine initiator is covalently combined and the initiator is fixed to the membrane surface by utilizing the viscosity, thereby obtaining an ultrafiltration membrane with initiation sites on the surface.

[0064] In the present invention, after the above reaction, the ultrafiltration membrane is preferably washed. The washing is preferably sequentially washed with methanol and deionized water, each washed multiple times, such as three times. After washing, an ultrafiltration membrane with initiation sites on the surface is obtained.

[0065] Regarding step d) :

[0066] d) applying the ionic liquid mixture to the surface of the ultrafiltration membrane with initiation sites on the surface to carry out atom transfer radical polymerization reaction to obtain an ultrafiltration membrane functionalized based on polyionic liquid brushes.

[0067] In the present invention, the ionic liquid mixed solution comprises: ionic liquid, solvent and additives.

[0068] In the present invention, the ionic liquid (IL) is a tetrafluoroborate ionic liquid (i.e., the anion is BF4 - ); and the alkyl chain in the cation in the ionic liquid is a C4 alkyl chain. In the present invention, the ionic liquid is more preferably 1-butyl-3-methylimidazolium tetrafluoroborate. In the present invention, the molar ratio of the ionic liquid: α-bromoisobutyryl bromide in step a) is preferably (2-4):1.05, specifically 2.0:1.05, 2.5:1.05, 3.0:1.05, 3.4:1.05, 3.5:1.05, 4.0:1.05, more preferably 3.4:1.05.

[0069] In the present invention, the solvent is preferably at least one of a methanol solution and an ethanol solution. The methanol solution is a methanol aqueous solution, and the same is true for the ethanol solution. In the present invention, the volume percentage concentration of the methanol solution is preferably 20-80 vol%, more preferably 80 vol%; the volume percentage concentration of the ethanol solution is preferably 20-80 vol%, more preferably 80 vol%. In the present invention, the amount ratio of the solvent: ionic liquid is preferably (50-100) mL: 3.4 mmol, more preferably 100 mL: 3.4 mmol.

[0070] In the present invention, the additive is preferably a reducing agent and a ligand, and is preferably ascorbic acid and 2,2-bipyridine (Bpy); wherein the ascorbic acid is a reducing agent, and the rapid conversion between low-valent copper and high-valent copper during the reaction is conducive to maintaining the concentration of active species and reducing the amount of copper salt. The ascorbic acid in the system reduces the high-valent copper to low-valent copper. The 2,2-bipyridine is a ligand, which is a transition metal Cu +1ligand. The molar ratio of ascorbic acid to ionic liquid is preferably (1-3):3.4, specifically 1:3.4, 2:3.4, 3:3.4, and more preferably 2:3.4. The molar ratio of 2,2-bipyridine to ionic liquid is preferably (0.05-0.15):3.4, specifically 0.05:3.4, 0.06:3.4, 0.07:3.4, 0.08:3.4, 0.09:3.4, 0.096:3.4, 0.10:3.4, 0.11:3.4, 0.12:3.4, 0.13:3.4, 0.14:3.4, 0.15:3.4, and more preferably 0.096:3.4.

[0071] In the present invention, the preparation method of the ionic liquid is not particularly limited, and the materials can be mixed uniformly. The specific process can be as follows: the ionic liquid is dissolved in a solvent, and then an additive is added and stirred uniformly to obtain an ionic liquid mixture.

[0072] In the present invention, the method of applying the ionic liquid mixture to the surface of the ultrafiltration membrane with induction sites on the surface is preferably immersion, that is, the ultrafiltration membrane with induction sites on the surface obtained in step c) is placed in the ionic liquid mixture. There is no special restriction on the dosage ratio of the two, as long as the ionic liquid mixture can completely submerge the ultrafiltration membrane with induction sites on the surface.

[0073] In the present invention, after applying the ionic liquid mixture to the surface of the ultrafiltration membrane with initiation sites on the surface, atom transfer radical polymerization (ATRP) is carried out. In the present invention, the reaction is preferably carried out under protective atmosphere conditions. In the present invention, there is no special restriction on the type of gas providing the protective atmosphere, and it can be a conventional protective gas well known to those skilled in the art, such as nitrogen or argon. The protective gas is a high-purity gas with a purity of ≥99.99%. Specifically, a protective gas is introduced into the reaction system and evacuated to replace the air and form a protective atmosphere in the reaction system. In the present invention, the reaction is preferably carried out in the presence of CuBr; specifically, after the protective atmosphere is formed, CuBr is added to the system and the reaction is sealed. In the present invention, the molar ratio of CuBr: ionic liquid is preferably (0.020-0.050): 3.4, specifically 0.020: 3.4, 0.025: 3.4, 0.030: 3.4, 0.035: 3.4, 0.040: 3.4, 0.045: 3.4, 0.048: 3.4, 0.050: 3.4, more preferably 0.048: 3.4. In the present invention, the temperature of the atom transfer radical polymerization reaction is not particularly limited, and can be room temperature, which can be 20-30°C, specifically 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, preferably 25°C. The time of the atom transfer radical polymerization reaction is preferably 6-12h, more preferably 12h. Through the above-mentioned atom transfer radical polymerization reaction, the ionic liquid (IL) undergoes polymerization reaction at the initiation site to generate a polyionic liquid (PIL) and is grafted onto the surface of the ultrafiltration membrane. The polyionic liquid brush is fixed on the surface of the ultrafiltration membrane to obtain an ultrafiltration membrane functionalized with a polyionic liquid brush.

[0074] In the present invention, after the above reaction, washing is preferably performed, preferably washing with methanol and deionized water in sequence, to remove excess unreacted ionic liquid monomers and excess polyionic liquid, thereby obtaining an ultrafiltration membrane based on polyionic liquid brush functionalization.

[0075] In the present invention, step d) preferably specifically comprises: placing the surface of the ultrafiltration membrane with initiation sites obtained in step c) in an ionic liquid mixture, introducing a protective gas into the reaction system and evacuating to replace the air and form a protective atmosphere in the reaction system, then adding CuBr, and conducting an atom transfer radical polymerization reaction in a closed manner, followed by washing to obtain an ultrafiltration membrane functionalized based on a polyionic liquid brush. In step d) of the present invention, atom transfer radical polymerization is used for surface grafting modification, and the grafting structure and density are accurately controlled by controlling the polymerization conditions, the number and type of monomers, and the reaction conditions and temperature are controllable, so that the membrane surface can be better functionalized, and a PIL brush with hydrophilicity and antibacterial properties is introduced on the surface, effectively improving the antifouling performance of the membrane.

[0076] The synthetic route of the preparation method of the present invention is as follows Figure 8 As shown, Figure 8 The figure is a synthetic route diagram of the preparation method of the present invention.

[0077] In the present invention, combined with the ultrafiltration membrane pretreatment and other details, the above-mentioned preparation method of the present invention preferably specifically includes the following steps:

[0078] S1. Pre-treat the ultrafiltration membrane for standby use.

[0079] S2, dopamine and solvent are placed in a reaction container, high-purity nitrogen is introduced to expel the air in the three-necked flask, then an acid binding agent and α-bromoisobutyryl bromide are added, high-purity nitrogen is continued to be introduced and stirred, and the reaction is carried out at room temperature to obtain a reaction solution containing α-bromoisobutyl functionalized dopamine initiator.

[0080] S3, taking out the ultrafiltration membrane pretreated in step S1, sticking it on a glass sheet, and then fixing the ultrafiltration membrane with a Teflon frame.

[0081] S4, mixing the reaction solution containing the α-bromoisobutyl functionalized dopamine initiator obtained in step S2 with Tris-HCl buffer to obtain a diluted solution of the α-bromoisobutyl functionalized dopamine initiator.

[0082] S5, the α-bromoisobutyl functionalized dopamine initiator dilution obtained in step S4 is quickly poured into the Teflon frame of step S3 to fully immerse the surface of the ultrafiltration membrane, and the ultrafiltration membrane is allowed to stand at room temperature for polymerization reaction. After the reaction is completed, the ultrafiltration membrane is washed to obtain an ultrafiltration membrane with initiation sites on the surface.

[0083] S6, dissolving the ionic liquid in a solvent, then adding ascorbic acid and 2,2-bipyridine, stirring evenly, and obtaining an ionic liquid mixture. Immerse the ultrafiltration membrane with initiation sites on the surface obtained in step S5 in the ionic liquid mixture, introduce high-purity nitrogen into the system and evacuate to fully discharge the air in the system, then add CuBr, seal and perform atom transfer radical polymerization at room temperature, after the reaction is completed, wash the membrane to remove excess unreacted ionic liquid monomers and excess polyionic liquid, thereby obtaining an ultrafiltration membrane based on polyionic liquid brush functionalization.

[0084] In the above steps S1 to S6, the types of substances, dosages and process condition parameters are consistent with those described in the previous technical solution and will not be repeated here.

[0085] The present invention also provides an ultrafiltration membrane based on polyionic liquid brush functionalization obtained by the preparation method described in the above technical solution.

[0086] The present invention also provides an application of the ultrafiltration membrane based on polyionic liquid brush functionalization described in the above technical solution in wastewater treatment.

[0087] The preparation method provided by the invention comprises the following steps: firstly reacting dopamine with α-bromoisobutyryl bromide to obtain an α-bromoisobutyl functionalized dopamine initiator; then diluting the α-bromoisobutyl functionalized dopamine initiator with a buffer to obtain a diluted α-bromoisobutyl functionalized dopamine initiator solution; then applying the diluted α-bromoisobutyl functionalized dopamine initiator solution to the surface of an ultrafiltration membrane for reaction to obtain an ultrafiltration membrane with initiation sites on the surface; and finally applying a certain ionic liquid mixed solution to the surface of the ultrafiltration membrane with initiation sites on the surface to perform an atom transfer radical polymerization reaction to obtain an ultrafiltration membrane based on polyionic liquid brush functionalization. The present invention uses dopamine and α-bromoisobutyryl bromide to react to obtain α-bromoisobutyl functionalized dopamine initiator, treats and reacts the surface of an ultrafiltration membrane with the specific initiator, forms a specific linker and initiation site on the surface of the ultrafiltration membrane, and then introduces a specific ionic liquid to the surface of the ultrafiltration membrane. Under the action of the specific linker at the initiation site, an atom transfer radical polymerization reaction is performed to fix the polyionic liquid brush on the membrane surface. The polyvinylidene fluoride anti-biological and organic dual-pollution ultrafiltration membrane based on the surface modification of the polyionic liquid brush of the present invention fixes a certain hydrophilic polyionic liquid brush on the membrane surface through the ATRP technology, giving the PVDF ultrafiltration membrane excellent antibacterial properties without losing the hydrophilicity of the membrane surface; the polyionic liquid brush fixed on the membrane surface can prevent bacteria from adhering to the membrane surface to achieve the purpose of "defense", and the positive charge carried by the imidazole ring disturbs the surface potential of negatively charged bacteria, thereby killing the bacteria adhering to the membrane surface. The polyionic liquid brush functionalized ultrafiltration membrane finally obtained by the present invention has improved anti-biological and anti-organic pollution performance in the dynamic filtration process compared with the original ultrafiltration membrane. The practical application value of the prepared ultrafiltration membrane is further proved by actual water treatment experiments. In the prior art CN114377563, after the hydrophobic ionic liquid is grafted on the surface, although the antibacterial performance of the membrane is increased, the membrane water flux is reduced by 10% compared with the original membrane, and the hydrophobicity of the membrane surface is increased, which will deteriorate the anti-organic pollution performance of the ultrafiltration membrane. The present invention is further improved by using hydrophilic polydopamine as an initiator and then grafting a hydrophilic ionic liquid. The membrane water flux in the present invention is increased compared with the original membrane flux, the hydrophilicity is improved, and it has a good anti-organic pollution ability while maintaining the ability to inactivate bacteria. Finally, through actual water filtration experiments, we concluded that the target membrane maintains good anti-fouling ability in the actual water treatment process.

[0088] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0089] Example 1

[0090] S1. Soak a commercial PVDF ultrafiltration membrane (molecular weight cutoff of 100 kDa) in anhydrous ethanol for 20 min, then ultrasonically clean it with deionized water for 30 min, rinse it with deionized water several times, and then soak it in deionized water for use.

[0091] S2. Put 2.1mmol dopamine and 20mL N,N-dimethylformamide into a three-necked flask, and pass high-purity nitrogen for 30 minutes to expel the air in the three-necked flask. Then, add 1.05mmol triethylamine and 1.05mmol α-bromoisobutyryl bromide, continue to pass high-purity nitrogen and stir, and react at room temperature 25°C for 3h to obtain a reaction solution containing α-bromoisobutyl functionalized dopamine initiator.

[0092] S3. Take out the PVDF ultrafiltration membrane in step S1 from the deionized water, cut it into a size of 9×12 cm and stick it on a glass sheet, and then fix the ultrafiltration membrane with a Teflon frame.

[0093] S4. Mix the reaction solution containing the α-bromoisobutyl functionalized dopamine initiator obtained in step S2 with 100 mL of Tris-HCl buffer to obtain a diluted solution of the α-bromoisobutyl functionalized dopamine initiator.

[0094] S5, the α-bromoisobutyl functionalized dopamine initiator dilution obtained in step S4 is quickly poured into the Teflon frame of step S3 to fully immerse the surface of the PVDF ultrafiltration membrane, and the ultrafiltration membrane is allowed to stand at room temperature 25°C for 30 minutes for polymerization reaction. After the reaction is completed, the ultrafiltration membrane is washed with methanol 3 times and deionized water 3 times in sequence to obtain an ultrafiltration membrane with initiation sites on the surface.

[0095] S6, 3.4mmol ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate was dissolved in 100mL methanol aqueous solution (80vol%), and then 2mmol ascorbic acid and 96μmol 2,2-bipyridine were added, and stirred evenly to obtain an ionic liquid mixture. The ultrafiltration membrane with initiation sites on the surface obtained in step S5 was immersed in the ionic liquid mixture, and high-purity nitrogen was introduced into the system for 30min and vacuumed to fully discharge the air in the system, and then 48μmol CuBr was added, sealed and reacted at room temperature 25°C for atom transfer radical polymerization. After 12h of reaction, the membrane was rinsed with methanol and deionized water in turn to remove excess unreacted ionic liquid monomers and excess polyionic liquids, thereby obtaining an ultrafiltration membrane based on polyionic liquid brush functionalization.

[0096] Example 2

[0097] The process was carried out in accordance with Example 1, except that the reaction time in step S6 was 6 h.

[0098] Comparative Example 1

[0099] Blank control PVDF ultrafiltration membrane:

[0100] A commercial PVDF ultrafiltration membrane (molecular weight cutoff of 100 kDa) was soaked in anhydrous ethanol for 20 min, then ultrasonically cleaned with deionized water for 30 min, rinsed with deionized water several times, and then soaked in deionized water for use.

[0101] Comparative Example 2

[0102] Ultrafiltration membrane with initiation sites on the surface:

[0103] The method is implemented in accordance with Example 1, except that only steps S1 to S5 are performed, and step S6 is no longer performed, that is, an ultrafiltration membrane with induction sites on the surface is finally obtained.

[0104] Comparative Example 3

[0105] The process is carried out in accordance with Example 1, except that the ionic liquid in step S6 is replaced by 1-butyl-3-methylimidazolium hexafluorophosphate.

[0106] Comparative Example 4

[0107] The process is carried out in accordance with Example 1, except that the ionic liquid in step S6 is replaced by 1-butyl-3-methylimidazolium bromide.

[0108] Comparative Example 5

[0109] The process was carried out in accordance with Example 2, except that the reaction time in step S6 was 24 h.

[0110] Example 3: Product Characterization and Testing

[0111] 1. Morphology characterization

[0112] The film samples obtained in Comparative Examples 1-2 and Example 1 were subjected to microscopic morphology characterization (SEM characterization), as shown in FIG. Figure 1 As shown, Figure 1 The surface morphology structure diagram of the film samples obtained in Comparative Examples 1-2 and Example 1, wherein: Figure 1 (a) is the surface morphology structure diagram of the film sample obtained in Comparative Example 1, Figure 1 (b) is the surface morphology structure diagram of the film sample obtained in Comparative Example 2, Figure 1 (c) is a surface morphology structure diagram of the membrane sample obtained in Example 1. It can be seen that the morphology of Example 1 is compared with that of Comparative Examples 1-2, and it can be seen that the deposition of PDA on the original PVDF and the subsequent ATRP reaction have almost no effect on the membrane surface morphology and pore structure.

[0113] 2. ATR-FTIR characterization

[0114] The film samples obtained in Comparative Examples 1-2 and Example 1 were characterized by Fourier transform infrared spectroscopy (ATR-FTIR). Figure 2 As shown, Figure 2 It is the Fourier infrared transform spectrum of the film samples obtained in Comparative Examples 1-2 and Example 1, wherein: Figure 2 (a) is the Fourier transform infrared spectrum of the film sample obtained in Comparative Example 1, Figure 2 (b) is the Fourier transform infrared spectrum of the film sample obtained in Comparative Example 2, Figure 2 (c) is the Fourier transform infrared spectrum of the film sample obtained in Example 1. It can be seen that the 1650 and 3400 cm -1 The stretching vibration peaks of C=N and CH appeared at the membrane surface. The two new peaks came from the grafted imidazole ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate, proving that the imidazole ionic liquid was successfully grafted onto the membrane surface.

[0115] 3. Antibacterial test

[0116] The antibacterial activity of ultrafiltration membrane samples was measured by colony forming unit counting method:

[0117] Luria-Bertani (LB) liquid medium and Luria-Bertani (LB) solid medium were sterilized in a sterilizer in Luria-Bertani (LB) phosphate buffer solution (PBS). Escherichia coli was cultured in Luria-Bertani (LB) liquid medium until OD = 1 in the exponential phase, then washed three times by centrifugation with sterile phosphate buffer solution (PBS) and resuspended to a concentration of 5 × 10 5 CFU / mL. The membrane sample was cut into 1×1cm 2 Soak the membrane in alcohol for 10 minutes to wash away surface impurities and bacteria, then rinse with sterile PBS buffer solution 3 times. 20 μL of bacterial solution was dropped on the surface of the membrane sample and cultured at 37°C for 6 hours. The PVDF membrane in comparative example 1 was used as a blank control. The contacted membrane was placed in a PBS buffer solution and ultrasonically cleaned for 10 minutes to wash off the bacteria. Take 70 μL of the cleaned bacterial solution and evenly spread it on the LB solid culture medium. After culturing at 37°C for 12 hours, the number of live bacterial colonies was recorded. The number of bacterial colonies after the surface of the PVDF membrane modified by contact with the polyionic liquid brush was compared with the blank control to obtain the antibacterial efficiency of the modified membrane.

[0118] Taking Comparative Examples 1-2 and Example 1 as examples, the test results are as follows Figure 3 As shown, Figure 3The antibacterial test effect diagram of the membrane samples obtained in Comparative Examples 1-2 and Example 1, wherein a represents Comparative Example 1, b represents Comparative Example 2, and c represents Example 1. It can be seen that compared with the blank polyvinylidene fluoride ultrafiltration membrane of Comparative Example 1 and the ultrafiltration membrane obtained in Comparative Example 2, the antibacterial effect of the anti-biological contamination polyvinylidene fluoride ultrafiltration membrane based on polyionic liquid brush functionalization obtained in Example 1 is significantly improved, and the colony count is only about 33%, that is, the antibacterial rate reaches 67%, indicating that the ultrafiltration membrane based on polyionic liquid brush functionalization obtained in the present invention can effectively improve the bactericidal performance.

[0119] Similarly, other examples were also tested for antibacterial properties, and the results are shown in Table 1:

[0120] Table 1: Antibacterial test results

[0121] Antibacterial rate, % Example 1 67 Comparative Example 3 55

[0122] From the test results in Table 1, it can be seen that the antibacterial rate of the ultrafiltration membrane based on polyionic liquid brush functionalization obtained in the present invention reaches more than 67%, showing excellent antibacterial effect. After changing the type of ionic liquid in Comparative Example 3, the antibacterial rate is significantly reduced.

[0123] 4. Water flux test

[0124] The test was conducted using a cross-flow filtration device. Specifically, the membrane sample was cut into a size suitable for the filtration system (3×4 cm) and immersed in deionized water overnight. The pure water flux was measured using deionized water. First, the filtration system was pre-pressed at a pressure of 0.2 MPa to stabilize the filtration system. The pre-pressing time was 1.5 hours. After the flux was stable, the pressure was adjusted to 0.1 MPa. The measurement was continued for 20 minutes, and the flux change data was recorded.

[0125] Taking Comparative Examples 1-2 and Example 1 as examples, the test results are as follows Figure 4 As shown, Figure 4 The water flux test effect diagram of the membrane samples obtained in Comparative Examples 1-2 and Example 1, wherein a represents Comparative Example 1, b represents Comparative Example 2, and c represents Example 1. It can be seen that compared with the blank polyvinylidene fluoride ultrafiltration membrane of Comparative Example 1 and the ultrafiltration membrane obtained in Comparative Example 2, the water flux of the anti-biological contamination polyvinylidene fluoride ultrafiltration membrane based on polyionic liquid brush functionalization obtained in Example 1 is improved, indicating that the ultrafiltration membrane based on polyionic liquid brush functionalization obtained in the present invention can effectively improve the bactericidal performance.

[0126] Similarly, water flux tests were also performed on other embodiments, and the results are shown in Table 2:

[0127] Table 2: Water flux test results

[0128] <![CDATA[Water flux, m -2 ·h -1 ·bar -1 > Example 1 430 Example 2 436 Comparative Example 1 416 Comparative Example 3 367 Comparative Example 4 419 Comparative Example 5 333

[0129] It can be seen from the test results in Table 2 that the water flux of the product obtained in Example 1-2 of the present invention is 430m -2 ·h -1 bar -1 The above results are significantly improved compared with the blank group (Comparative Example 1). After changing the type of ionic liquid in Comparative Examples 3-4, the water flux of the product is significantly reduced or only equal to that of the original membrane, proving that the use of a specific type of ionic liquid in the present invention is beneficial to improving the water flux of the product. After extending the polymerization reaction time in Comparative Example 4, the water flux of the product is also significantly reduced.

[0130] 5. Anti-biological contamination performance test

[0131] The test was conducted using a cross-flow filtration device. Specifically, the membrane sample was cut into a size suitable for the filtration system (3×4 cm). First, the filtration system was stabilized by pre-pressing with deionized water at a pressure of 0.2 MPa for 1.5 h. The filtration system was prepared using a cross-flow filtration device containing 1.16 mM C6H5Na3O7, 0.94 mM NH4Cl, 0.45 mM KH2PO4, 0.5 mM CaCl2, 0.5 mM NaHCO3, 2.0 mM NaCl, 0.6 mM MgSO4 and an initial concentration of 10 E. coli. 3 CFU / mL simulated wastewater was used as the feed solution. Under the conditions of 30°C and a flow rate of 60LPH, the system pressure was adjusted at around 0.1MPa to make the initial flux consistent. The filtration was stable for 8h, and the changes in membrane flux were recorded.

[0132] Taking Comparative Examples 1-2 and Example 1 as examples, the test results are as follows Figure 5 As shown, Figure 5 The figures are the effect diagrams of the anti-biological fouling performance of the membrane samples obtained in Comparative Examples 1-2 and Example 1, wherein a represents Comparative Example 1, b represents Comparative Example 2, and c represents Example 1. It can be seen that as time goes by, the membrane flux of the membrane samples of Comparative Examples 1-2 decreases significantly and the stability is poor, while the downward trend of the membrane flux of Example 1 slows down, significantly slowing down and reducing the membrane flux decline rate, and the membrane flux retention rate is still relatively high, proving that the ultrafiltration membrane based on polyionic liquid brush functionalization obtained in the present invention can effectively improve the anti-biological fouling performance.

[0133] 6. Anti-organic pollution performance test

[0134] The test was conducted using a cross-flow filtration device. Specifically, the membrane sample was cut to a size suitable for the filtration system (3×4 cm). First, the filtration system was stabilized by pre-pressing with deionized water at a pressure of 0.2 MPa for 1.5 h. The simulated wastewater with an initial bovine serum albumin (BSA) of 500 mg / L was used as the feed solution. The system pressure was adjusted at about 0.1 MPa at 30°C and a flow rate of 60 LPH to make the initial flux consistent. The filtration was stabilized for 8 h, and the membrane flux changes were recorded.

[0135] Taking Comparative Examples 1-2 and Example 1 as examples, the test results are as follows Figure 6 As shown, Figure 6 The figures are the test results of the anti-organic pollution performance of the membrane samples obtained in Comparative Examples 1-2 and Example 1, wherein a represents Comparative Example 1, b represents Comparative Example 2, and c represents Example 1. It can be seen that as time goes by, the membrane flux of the membrane samples of Comparative Examples 1-2 decreases significantly and the stability is poor, while the downward trend of the membrane flux of Example 1 slows down, significantly slows down and reduces the membrane flux decline rate, and the membrane flux retention rate is still high, proving that the ultrafiltration membrane based on polyionic liquid brush functionalization obtained in the present invention can effectively improve the organic pollution performance.

[0136] 7. Actual wastewater filtration performance test

[0137] The experiment was conducted using a cross-flow filtration device. Specifically, the membrane sample was cut to a size suitable for the filtration system (3×4cm). First, deionized water was pre-pressed at a pressure of 0.2MPa to stabilize the filtration system, and the pre-pressing time was 1.5h. The effluent of the sequencing batch reactor (SBR) was used as the feed solution. Before the experiment, the effluent of the bioreactor was pretreated with filter paper to remove suspended particles. Under the conditions of 30℃ and a flow rate of 90LPH, the system pressure was adjusted at around 0.1MPa to make the initial flux consistent, and the filtration was stabilized for 90min (recorded as the first cycle), and the membrane flux change was recorded. The contaminated membrane was removed and ultrasonically cleaned with deionized water, and the membrane was re-pressed for testing, and the filtration was stabilized for 90min (recorded as the second cycle), and the flux recovery rate was determined. Then the contaminated membrane was removed again, and ultrasonically cleaned with deionized water, and the membrane was re-pressed for testing, and the filtration was stabilized for 90min (recorded as the third cycle), and the flux recovery rate (i.e., the ratio of the membrane flux in the nth cycle / the membrane flux in the first cycle) was determined.

[0138] Taking Comparative Example 1 and Example 1 as examples, the test results are as follows Figure 7 As shown, Figure 7 The actual wastewater filtration performance test effect diagram of the membrane samples obtained in Comparative Example 1 and Example 1, wherein a represents Comparative Example 1 and b represents Example 1. It can be seen that: ① In each cycle, as time goes on, the membrane flux of the membrane sample of Comparative Example 1 decreases significantly and the stability is poor, while the downward trend of the membrane flux of Example 1 slows down, significantly slowing down and reducing the membrane flux decline rate, and the membrane flux retention rate is still high, with good stability. ② Compared with the first cycle, the membrane flux recovery rate of the membrane sample of Comparative Example 1 in the second to third cycles is lower, and the membrane flux recovery rate of the membrane sample of Example 1 is higher and improved compared with Comparative Example 1, proving that the ultrafiltration membrane based on polyionic liquid brush functionalization obtained by the present invention improves the membrane recovery performance and has good regeneration and recycling performance.

[0139] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A method for preparing an ultrafiltration membrane based on polyionic liquid brush functionalization, It is characterized in that The following steps are involved: a) placing dopamine and a solvent in a reaction vessel, introducing high-purity nitrogen to expel the air in the three-necked flask, then adding an acid binding agent and α-bromoisobutyryl bromide, continuing to introduce high-purity nitrogen while stirring, and reacting at room temperature to obtain a reaction solution containing α-bromoisobutyl functionalized dopamine initiator; b) mixing the α-bromoisobutyl functionalized dopamine initiator reaction solution with a buffer solution to obtain an α-bromoisobutyl functionalized dopamine initiator dilution solution; c) applying the α-bromoisobutyl functionalized dopamine initiator dilution to the surface of an ultrafiltration membrane for reaction to obtain an ultrafiltration membrane with initiation sites on the surface; d) applying the ionic liquid mixture to the surface of the ultrafiltration membrane with initiation sites on the surface to carry out an atom transfer radical polymerization reaction to obtain an ultrafiltration membrane functionalized with a polyionic liquid brush; in, The ionic liquid mixed solution comprises: an ionic liquid, a solvent and an additive; The ionic liquid is 1-butyl-3-methylimidazolium tetrafluoroborate ionic liquid; and the alkyl chain of the cation in the ionic liquid is a C4 alkyl chain; The additives are reducing agents and ligands.

2. The preparation method according to claim 1, It is characterized in that In step d), the atom transfer radical polymerization reaction time is 6 to 12 hours.

3. The preparation method according to claim 1, It is characterized in that In step c), the reaction time is 10 to 90 minutes.

4. The preparation method according to claim 1, It is characterized in that In step a), the molar ratio of dopamine to α-bromoisobutyryl bromide is (1-3.15):1.

05.

5. The preparation method according to claim 1, It is characterized in that In step a), the reaction is carried out in the presence of an acid binding agent; The acid binding agent is at least one of triethylamine, pyridine and sodium carbonate.

6. The preparation method according to claim 1, It is characterized in that The dosage ratio of dopamine in step a) to buffer in step b) is 2.1 mmol to (50-150) mL.

7. The preparation method according to claim 1, It is characterized in that In step c), pouring the α-bromoisobutyl functionalized dopamine initiator dilution onto the surface of the ultrafiltration membrane; specifically comprising: preparing an ultrafiltration membrane fixture before step b), and immediately and rapidly pouring the α-bromoisobutyl functionalized dopamine initiator dilution into the ultrafiltration membrane fixture after obtaining the α-bromoisobutyl functionalized dopamine initiator dilution in step b); The ultrafiltration membrane fixture is prepared by the following method: attaching the ultrafiltration membrane to a substrate, and then fixing the ultrafiltration membrane to the substrate with a frame.

8. An ultrafiltration membrane based on polyionic liquid brush functionalization prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the ultrafiltration membrane based on polyionic liquid brush functionalization as claimed in claim 8 in wastewater treatment.

Citation Information

Patent Citations

  • Preparation method of silicon substrate capable of carrying out hydrophilic and hydrophobic reversible transition

    CN102731143A

  • Preparation method of poly-dopamine modified PVDF membrane

    CN106310965A

  • Polyvinylidene fluoride composite film comprising modified polydopamine nano-particles and preparation method of composite film

    CN109351213A

  • Amphoteric substance-based polyamide nanofiltration membrane surface modification method

    CN113083019A

  • Preparation method of polyion liquid brush surface grafting modified anti-biological pollution PVDF ultrafiltration membrane