A method for controlling surface cracks in VN microalloyed steel continuous casting billets

VN microalloy steel is produced through a vertical continuous casting machine, which controls the pulling speed and cooling water volume, optimizes the protection slag composition, solves the surface crack problem of vanadium nitrogen microalloy low-alloy high-strength steel continuous casting billet, and improves the purity of the casting billet and The crack resistance is achieved, and the fine grain structure of the steel plate is achieved after rolling.

CN116213668BActive Publication Date: 2024-11-29ANGANG STEEL CO LTD

Patent Information

Application Number
CN202310056232.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-19
Publication Date
2024-11-29
Estimated Expiration
2043-01-19

AI Technical Summary

Technical Problem

Vanadium nitrogen microalloyed low alloy high-strength steel continuous casting billet cools slowly in the austenite temperature range, causing brittleness, vibration marks promote transverse cracks at the corners, and cracks are easily generated under straightening and deformation, and straight arc slab continuous casting machine production At the time, the corners of the casting billet are prone to angular cross-cutting, which affects the steel plate material formation rate.

Method used

Vertical continuous casting machine is used to produce VN microalloy steel continuous casting billets, control the pulling speed and ladle casting time, set the cooling water volume of the second cold zone, optimize the chemical composition of the slag, ensure that the inclusions are floating and removed, and avoid deformation during straightening. Stress to control cracks on the surface of the casting billet.

Benefits of technology

Through vertical continuous casting machine production, the probability of cracks on the surface of the casting billet is reduced, the purity and homogeneity of the casting billet are improved, stress cracks are avoided, the high strength and toughness of VN microalloy steel are ensured, and the high strength and toughness of VN microalloy steel are promoted. Refined grain structure of steel plate after rolling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116213668B_ABST
    Figure CN116213668B_ABST
Patent Text Reader

Abstract

The invention relates to a method for controlling surface cracks of a VN microalloy steel continuous casting billet. A vertical continuous casting machine is used to produce the continuous casting billet, and process parameters such as the drawing speed, the ladle pouring time, and the cooling water volume in the secondary cooling zone are controlled. Compared with a traditional arc continuous casting machine, the vertical continuous casting machine ensures that inclusions have sufficient time to float up and be removed in the solidified liquid core, reduces the capture of inclusion particles by the solidified billet shell, improves the purity and homogeneity of the solidified billet shell, and reduces the probability of billet cracks caused by liquid phase precipitation type inclusions such as AlN. In addition, the vertical continuous casting machine does not need to straighten the billet, and compared with the traditional arc continuous casting machine, the problem of the billet shell being subjected to deformation stress during the straightening process is avoided, and the occurrence of stress cracks is effectively avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of continuous casting, in particular to a method for controlling surface cracks of a VN micro-alloy steel continuous casting billet. Background Art

[0002] Traditional low-alloy high-strength steel uses niobium microalloying. During the hot rolling process, niobium carbonitride is formed by deformation induction, which can inhibit the growth of recrystallization nucleation and requires higher activation energy to make the steel nucleate and grow, thereby increasing the recrystallization temperature. However, in the context of alloy reduction and green manufacturing, it is hoped to reduce the addition of precious metal niobium, reduce the rolling temperature, and reduce energy consumption. Using vanadium-nitrogen microalloying, vanadium nitride is precipitated during the controlled rolling process in the recrystallization zone, providing a nucleation core for the ferrite phase transformation in the austenite crystal. The precipitated VN particles have a pinning effect, which can effectively prevent the growth of recrystallized austenite grains and increase the effective grain boundary length, so that a large number of ferrite nucleation core positions are provided in the austenite crystal and grain boundary, achieving ferrite grain refinement after phase transformation, and having good toughness while improving strength. Compared with traditional niobium microalloyed steel, vanadium-nitrogen (VN) microalloy has lower microalloying cost, lower heating energy consumption and better comprehensive mechanical properties of steel.

[0003] However, the very slow cooling of the vanadium-nitrogen microalloyed low-alloy high-strength steel ingot during solidification in the austenite temperature range will cause VN to precipitate along the austenite grain boundaries. If the temperature of the corners of the ingot is in the peak temperature zone of nitride precipitation during straightening, it will cause the steel to become brittle. In addition, the vibration marks promote the occurrence of transverse cracks at the corners, and cracks are more likely to occur at the troughs of the vibration marks of the ingot under straightening deformation. Even under slow straightening conditions, the bonding force at the grain boundaries may be weakened, leading to cracking of the continuous casting ingot. Therefore, the problem of cracks at the corners of the continuous casting ingot of vanadium-nitrogen microalloyed steel has greatly limited the engineering application of vanadium-nitrogen microalloyed low-alloy high-strength steel.

[0004] The Chinese invention patent with the authorization announcement number CN111996466B discloses a "VN microalloyed steel and a method for producing a VN microalloyed continuous casting billet without surface cracks", with a nitrogen content of 0.011-0.2% and a vanadium content of 0.1-0.4%. During the continuous casting process, the straightening zone of the billet is avoided from experiencing the high temperature brittle temperature range by means of low superheat, low pulling speed and weak water cooling. However, within the nitrogen content range, the precipitation-temperature-time curve (PTT) of VN will move significantly to the left, resulting in a large amount of VN precipitating along the austenite grain boundary in a short time in the straightening temperature range of 850-900°C, which will cause cracking of the corners of the billet even in the straightening deformation under low pulling speed.

[0005] The Chinese invention patent with the authorization announcement number CN107866538B discloses "a method for continuous casting of square billets containing vanadium and nitrogen microalloyed peritectic steel", which uses an arc-shaped square billet continuous casting machine to produce microalloyed peritectic steel with a vanadium content of 0.05-010% and a nitrogen content of 0.006-0.012%. By optimizing the soft water and secondary cooling water distribution of the crystallizer, the surface temperature of the billet is increased to avoid the low temperature of the plastic temperature of the billet surface. Although this method can avoid the peak temperature of VN precipitation, the reduction in cooling intensity and the decrease in pulling speed will inevitably lead to a longer residence time in the high temperature zone on the billet surface, which will still lead to a large amount of VN precipitation. In this case, straightening deformation may still cause cracks on the billet surface.

[0006] The Chinese invention patent with the authorization announcement number CN100457327C discloses a "method for controlling network cracks in continuous casting billets of high-nitrogen and high-strength weathering steel containing vanadium". The nitrogen content of the continuous casting billets of high-strength weathering steel is 0.01-0.03% and the vanadium content is 0.02-0.15%. The network cracks in the billets are eliminated by setting the cooling water volume on the wide and narrow sides of the crystallizer and the casting speed of the casting machine, increasing the billet shell surface temperature to 1050-1120°C, the vibration frequency to 110-130Hz, reducing the CaO ratio in the protective slag, and reducing the amount of cooling water used in the second cooling stage of the billet. This method does not take into account that at a nitrogen content of 0.01 to 0.03%, a large amount of high-melting-point AlN inclusions will precipitate from the liquid steel. Due to the effect of gravity, the AlN inclusions will be enriched on the inner arc side of the ingot. When the ingot shell temperature is straightened in the range of 1050 to 1120°C, the ingot shell strength is insufficient, and the AlN inclusions are enriched on the surface of the ingot shell, which may cause steel leakage.

[0007] In the above invention patents, vanadium-nitrogen microalloyed steel slabs are all produced by straight-arc slab continuous casting machines. V and N dissolved at high temperatures in the initial stage of solidification will precipitate in the form of V(CN) at the austenite grain boundaries as the temperature decreases during the solidification process. In the bending area of ​​the straight-arc slab continuous casting machine, the inner arc side and outer arc side of the ingot are subjected to compressive stress and tensile stress, respectively. In the straightening area, the inner arc side and outer arc side of the ingot are subjected to tensile stress and compressive stress, respectively. In particular, the ingot will produce stress concentration due to the notch effect of the vibration mark under the action of tensile stress, thereby accelerating the formation and expansion of cracks. The characteristics of the straight-arc slab continuous casting machine determine that when producing vanadium-nitrogen microalloyed steel, it is very easy to produce transverse cracks at the corners of the ingot. Since the transverse cracks at the corners of the ingot cannot be cleaned during production, delamination defects will occur on the surface edge of the product after defective rolling, which seriously affects the yield rate of the steel plate. Summary of the invention

[0008] The present invention provides a method for controlling surface cracks of a VN micro-alloyed steel continuous casting billet. A vertical continuous casting machine is used to produce the continuous casting billet. Compared with a traditional arc continuous casting machine, the method ensures that inclusions have sufficient time to float up and be removed in the solidifying liquid core, reduces the capture of inclusion particles by the solidifying billet shell, improves the purity and homogeneity of the solidifying billet shell, and reduces the probability of billet cracks caused by liquid phase precipitation type inclusions such as AlN. In addition, the vertical continuous casting machine does not need to straighten the billet. Compared with a traditional arc continuous casting machine, the method avoids the problem of the billet shell being subjected to deformation stress during the straightening process, and effectively avoids the occurrence of stress cracks.

[0009] In order to achieve the above object, the present invention adopts the following technical solutions:

[0010] A method for controlling surface cracks of a VN microalloyed steel continuous casting billet, wherein the VN microalloyed steel continuous casting billet is produced by a vertical slab continuous casting machine, and the following production process is controlled:

[0011] 1) Different pulling speeds are set according to the cross-sectional size of the continuous casting billet and the converter + refining smelting cycle, and the pulling speed is controlled at 0.09-0.39 m / min;

[0012] 2) Different ladle pouring times are set according to the width and thickness of the continuous casting billet, and the ladle pouring time is controlled within 54 to 137 minutes;

[0013] 3) The cooling water volume in different areas of the secondary cooling zone is set according to the casting speed, so that the stress generated in the continuous casting billet does not exceed its tensile strength, and the maximum stress is near the solidus;

[0014] 4) The chemical composition of the continuous casting protection slag is calculated by weight percentage: CaO 34%~36%; SiO2 32%~34%; MgO 0.5%~0.7%; Na2O 9%~11%; K2O 0.03%~0.07%; Al2O3 5%~7%; Fe2O3 0.5%~0.8%; F 7.5%~8.5%; C 5%~6%.

[0015] Furthermore, the chemical composition of the VN microalloyed steel continuous casting billet is C: 0.06% ~ 0.20%, Si: 0.10% ~ 0.40%, Mn: 1.0% ~ 3.0%, P ≤ 0.05%, S ≤ 0.05%, V: 0.05% ~ 0.4%, N: 0.01% ~ 0.2%, and the remainder is Fe and unavoidable impurity elements.

[0016] Furthermore, the VN microalloyed steel continuous casting billet has a thickness of 400-700 mm and a width of 2000-2600 mm.

[0017] Furthermore, the VN microalloyed steel continuous casting billet is cast using a 120-300 ton ladle, and the number of caster streams is 2.

[0018] Furthermore, the refining adopts nitrogen blowing alloying, and the refining time is determined by the nitrogen content; the drawing speed mode is determined according to the nitrogen content, and the upper and lower limits of the drawing speed are set according to the cross-sectional specifications of the continuous casting billet in each drawing speed mode; specifically as follows:

[0019] When the nitrogen content is 0.005%≤N<0.01%:200mm≤continuous casting billet thickness t<400mm, the pulling speed is 0.35~0.39m / min;400mm≤continuous casting billet thickness t<600mm, the pulling speed is 0.16~0.18m / min;600mm≤continuous casting billet thickness t≤700mm, the pulling speed is 0.11~0.12m / min;

[0020] When the nitrogen content is 0.01%≤N<0.025%:200mm≤continuous casting billet thickness t<400mm, the pulling speed is 0.31~0.34m / min;400mm≤continuous casting billet thickness t<600mm, the pulling speed is 0.14~0.15m / min;600mm≤continuous casting billet thickness t≤700mm, the pulling speed is 0.10~0.11m / min;

[0021] When the nitrogen content is 0.025%≤N<0.050%: 200mm≤continuous casting billet thickness t<400mm, the pulling speed is 0.28~0.31m / min; 400mm≤continuous casting billet thickness t<600mm, the pulling speed is 0.12~0.13m / min; 600mm≤continuous casting billet thickness t≤700mm, the pulling speed is 0.09~0.10m / min.

[0022] Furthermore, the second cooling zone is divided into zones one to seven, of which zones one to six adopt steam-water nozzle cooling, and zone seven adopts water spray cooling; the cooling water volume of each zone is: zone one 3.1-4.2 L / s; zone two 1.9-2.8 L / s; zone three 0.8-1.4 L / s; zone four 0.45-0.7 L / s; zone five 0.27-0.4 L / s; zone six 0.19-0.32 L / s; zone seven 0.12-0.17 L / s.

[0023] Furthermore, the coarse inclusions and fine inclusions of the VN microalloyed steel continuous casting billet are controlled below level 1.0.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1) The present invention adopts a vertical continuous casting machine to produce VN microalloyed steel, which ensures that inclusions have sufficient time to float up and be removed in the solidified liquid core, reduces the capture of inclusion particles by the solidified shell, improves the purity and homogeneity of the solidified shell, and reduces the probability of cracks in the casting caused by liquid phase precipitation type inclusions such as AlN;

[0026] 2) The vertical continuous casting machine has no bending-straightening process, no difference in cooling conditions between the inner and outer arcs of the ingot, no temperature difference between the inner and outer sides of the ingot, no problems such as uneven casting structure and internal stress, and effectively avoids the occurrence of stress cracks;

[0027] 3) The present invention develops a continuous casting production process for VN microalloyed steel based on a vertical continuous casting machine; this is mainly because no matter whether it is straight arc continuous casting or vertical continuous casting, the temperature of the corners of the ingot is much lower than the temperature inside the ingot. If the secondary cooling rate is not specially controlled, V(C,N) will still precipitate in the precipitation temperature range, causing V(C,N) to be segregated at the corners of the ingot. If V(C,N) cannot be fully diffused during the subsequent heating process before rolling the ingot, it will not effectively prevent the growth of recrystallized austenite grains and provide a large number of ferrite nucleation core positions; by adopting the process described in the present invention, V(C,N) of the VN microalloyed steel ingot can be evenly distributed, and the advantages of V(C,N) can be fully utilized during the rolling process, which promotes the refinement of the austenite recrystallization grains of the rolled steel plate and the refinement of the ferrite grains after the austenite phase transformation. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a low-magnification microstructure photograph of the continuous casting billet produced in Example 1 of the present invention.

[0029] Figure 2 This is a high-magnification microstructure photograph of the continuous casting billet produced in Example 1 of the present invention. DETAILED DESCRIPTION

[0030] The present invention discloses a method for controlling surface cracks of a VN microalloyed steel continuous casting billet. The VN microalloyed steel continuous casting billet is produced by a vertical slab continuous casting machine, and the following production process is controlled:

[0031] 1) Different pulling speeds are set according to the cross-sectional size of the continuous casting billet and the converter + refining smelting cycle, and the pulling speed is controlled at 0.09-0.39 m / min;

[0032] 2) Different ladle pouring times are set according to the width and thickness of the continuous casting billet, and the ladle pouring time is controlled within 54 to 137 minutes;

[0033] 3) The cooling water volume in different areas of the secondary cooling zone is set according to the casting speed, so that the stress generated in the continuous casting billet does not exceed its tensile strength, and the maximum stress is near the solidus;

[0034] 4) The chemical composition of the continuous casting protection slag is calculated by weight percentage: CaO 34%~36%; SiO2 32%~34%; MgO 0.5%~0.7%; Na2O 9%~11%; K2O 0.03%~0.07%; Al2O3 5%~7%; Fe2O3 0.5%~0.8%; F 7.5%~8.5%; C 5%~6%.

[0035] Furthermore, the chemical composition of the VN microalloyed steel continuous casting billet is C: 0.06% ~ 0.20%, Si: 0.10% ~ 0.40%, Mn: 1.0% ~ 3.0%, P ≤ 0.05%, S ≤ 0.05%, V: 0.05% ~ 0.4%, N: 0.01% ~ 0.2%, and the remainder is Fe and unavoidable impurity elements.

[0036] Furthermore, the VN microalloyed steel continuous casting billet has a thickness of 400-700 mm and a width of 2000-2600 mm.

[0037] Furthermore, the VN microalloyed steel continuous casting billet is cast using a 120-300 ton ladle, and the number of caster streams is 2.

[0038] Furthermore, the refining adopts nitrogen blowing alloying, and the refining time is determined by the nitrogen content; the drawing speed mode is determined according to the nitrogen content, and the upper and lower limits of the drawing speed are set according to the cross-sectional specifications of the continuous casting billet in each drawing speed mode; specifically as follows:

[0039] When the nitrogen content is 0.005%≤N<0.01%:200mm≤continuous casting billet thickness t<400mm, the pulling speed is 0.35~0.39m / min;400mm≤continuous casting billet thickness t<600mm, the pulling speed is 0.16~0.18m / min;600mm≤continuous casting billet thickness t≤700mm, the pulling speed is 0.11~0.12m / min;

[0040] When the nitrogen content is 0.01%≤N<0.025%:200mm≤continuous casting billet thickness t<400mm, the pulling speed is 0.31~0.34m / min;400mm≤continuous casting billet thickness t<600mm, the pulling speed is 0.14~0.15m / min;600mm≤continuous casting billet thickness t≤700mm, the pulling speed is 0.10~0.11m / min;

[0041] When the nitrogen content is 0.025%≤N<0.050%: 200mm≤continuous casting billet thickness t<400mm, the pulling speed is 0.28~0.31m / min; 400mm≤continuous casting billet thickness t<600mm, the pulling speed is 0.12~0.13m / min; 600mm≤continuous casting billet thickness t≤700mm, the pulling speed is 0.09~0.10m / min.

[0042] Furthermore, the second cooling zone is divided into zones one to seven, of which zones one to six adopt steam-water nozzle cooling, and zone seven adopts water spray cooling; the cooling water volume of each zone is: zone one 3.1-4.2 L / s; zone two 1.9-2.8 L / s; zone three 0.8-1.4 L / s; zone four 0.45-0.7 L / s; zone five 0.27-0.4 L / s; zone six 0.19-0.32 L / s; zone seven 0.12-0.17 L / s.

[0043] Furthermore, the coarse inclusions and fine inclusions of the VN microalloyed steel continuous casting billet are controlled below level 1.0.

[0044] The technical problem solved by the surface crack control method of VN microalloyed steel continuous casting billet described in the present invention is the cracks at the corners of VN microalloyed steel casting billet and the surface cracks of steel plate after rolling. The method is suitable for wide and thick VN microalloyed steel plates.

[0045] The vertical slab continuous casting machine sets different drawing speeds according to the cross-sectional size of the continuous casting billet and the converter + refining smelting cycle. Since the refining adopts nitrogen blowing alloying, the refining time is determined by the nitrogen content. Therefore, three drawing speed modes are determined according to the nitrogen content. In each drawing speed mode, the upper and lower limits of the drawing speed are set according to the cross-sectional specifications of the continuous casting billet. The overall drawing speed range is controlled at 0.09-0.39m / min to ensure that the liquid core length is within a reasonable range and the billet bulging problem will not be caused by excessive static pressure of molten steel. The three drawing speed modes are shown in Table 1.

[0046] Table 1 Casting speed mode of vertical slab continuous casting machine m / min

[0047]

[0048] The vertical slab continuous casting machine sets different ladle pouring times according to the width and thickness of the continuous casting slab, and the pouring time is controlled at 54 to 137 minutes. See Table 2 for details.

[0049] Table 2 Ladle pouring time min

[0050]

[0051] The second cooling zone has 7 sections, namely zone 1 to zone 7. According to the selected pulling speed mode, the corresponding cooling water volume is set in different areas, see Table 3.

[0052] Table 3 Cooling water volume in secondary cooling zone

[0053]

[0054] In view of the surface quality problem caused by uneven temperature distribution of large-section continuous casting billets at faster drawing speeds, which in turn leads to uneven solidification of the thickness of the meniscus billet shell, continuous casting protection slag is used to ensure uniform and sufficient lubrication of the continuous casting billet. The chemical composition of the continuous casting protection slag is shown in Table 4.

[0055] Table 4 Chemical composition of continuous casting mold slag wt%

[0056] Element CaO <![CDATA[SiO2]]> MgO <![CDATA[Na2O]]> <![CDATA[K2O]]> <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> F C content 34~36 32~34 0.5~0.7 9~11 0.03~0.07 5~7 0.5~0.8 7.5~8.5 5~6

[0057] The present invention is based on the continuous casting process principle of the vertical slab continuous casting machine as follows:

[0058] If the drawing speed of the vertical slab continuous casting machine is too slow, it is easy to cause the following results: 1) Surface quality problems may occur due to the too thick solidified shell of the meniscus; 2) The large cross-section of the ingot and the uneven temperature distribution may cause uneven solidification of the thickness of the meniscus shell, resulting in surface quality problems; 3) The spacing of the vibration marks is too close, which may cause overlap, making the surface of the ingot rough, the resistance of the ingot drawing is large, and it is easy to produce surface cracks, which may also affect the smooth demolding of the ingot. If the drawing speed of the casting machine is too fast, it is easy to cause the following results: The static pressure of the molten steel of the vertical slab continuous casting machine is greater than that of the conventional continuous casting machine, and the static pressure of the molten steel depends on the length of the liquid core. The length of the liquid core is very sensitive to the changes in the drawing speed and the thickness of the continuous casting ingot. The greater the drawing speed, the thicker the continuous casting ingot, the deeper the liquid core length, and the greater the possibility of cracks caused by bulging, the drawing speed must be limited.

[0059] After the pulling speed corresponding to various cross-sectional sizes (specifications) of the continuous casting billet is determined, the ladle pouring time corresponding to various specifications of the continuous casting billet is determined in combination with the converter + refining smelting cycle.

[0060] The secondary cooling zone is divided into seven areas. Zones 1 to 6 are cooled by steam-water nozzles, and zone 7 is cooled by water spray. The water volume in each section is set according to the specifications of the continuous casting billet to ensure that the stress generated in the continuous casting billet will not exceed its tensile strength. The maximum stress value appears near the solidus line. The shortening of the distance from the meniscus of the crystallizer reduces the static pressure of the molten steel on the billet, thereby reducing the probability of cracks and achieving the purpose of improving the quality of the continuous casting billet.

[0061] For vertical slab continuous casting machines, due to its low pulling speed, complex steel grade characteristics, high superheat and other characteristics, the adaptability requirements for continuous casting protection slag are particularly high. The VN micro-alloyed steel described in the present invention belongs to the peritectic reaction component. When the peritectic reaction occurs, volume shrinkage will occur when δ is transformed to γ, which is easy to cause deep vibration marks and depressions on the surface of the continuous casting billet. In severe cases, the shrinkage causes large stress in the primary billet shell. If the stress is not released or even cooled unevenly or the liquid level of the crystallizer fluctuates severely, longitudinal cracks will occur on the surface of the continuous casting billet. Therefore, for VN micro-alloyed steel, weak cooling is required in the crystallizer to even out the thickness of the billet shell and reduce the stress effect. At the same time, considering the slag rolling factor, the continuous casting protection slag needs to have high basicity and low crystallinity.

[0062] The following embodiments are implemented on the premise of the technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0063] [Example]

[0064] The specific implementation process of the VN microalloyed steel continuous casting billet surface crack control method of the present invention is as follows:

[0065] The chemical composition of the continuous casting slabs of each embodiment is shown in Table 5. The continuous casting process parameters of each embodiment are shown in Table 6. The secondary cooling process parameters are shown in Table 7.

[0066] The low magnification microstructure photograph of the continuous casting billet produced in Example 1 is as follows: Figure 1 As shown, high-magnification tissue photos are Figure 2 shown.

[0067] Table 5 Chemical composition of continuous casting slab (%)

[0068] Example C Si Mn P S V N 1 0.09 0.36 1.59 0.016 0.002 0.09 0.010 2 0.012 0.38 1.52 0.015 0.003 0.15 0.016 3 0.15 0.38 1.55 0.016 0.003 0.26 0.026 4 0.18 0.37 1.48 0.015 0.002 0.35 0.034

[0069] Table 6 Continuous casting process parameters

[0070] Example Continuous casting billet section specifications (mm) Pulling speed(m / min) Ladle pouring time (min) 1 400×2100 0.37 67.1 2 400×2400 0.32 66.3 3 600×2200 0.12 124.6 4 700×2500 0.10 125.3

[0071] Table 7 Secondary cooling process parameters

[0072]

[0073] In this embodiment, the total length of the second cooling zone is 12.66 meters, zones 1 to 6 are cooled by steam-water nozzles, and zone 7 is cooled by water spray.

[0074] The surface and internal cracks of the 400mm, 600mm and 700mm thick VN micro-alloyed steel continuous casting billets produced in this embodiment are pure in steel quality, and both coarse and fine inclusions are controlled below level 1.0.

[0075] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for controlling surface cracks in a VN microalloyed steel continuous casting billet, characterized in that: The VN microalloyed steel continuous casting billet is produced by a vertical slab continuous casting machine, and the following production process is controlled: 1) Different pulling speeds are set according to the cross-sectional dimensions of the continuous casting billet and the converter + refining smelting cycle, and the pulling speed is controlled at 0.09-0.39 m / min; refining adopts nitrogen blowing alloying, and the refining time is determined by the nitrogen content; the pulling speed mode is determined according to the nitrogen content, and the upper and lower limits of the pulling speed are set according to the cross-sectional specifications of the continuous casting billet in each pulling speed mode; the details are as follows: When the nitrogen content is 0.005%≤N<0.01%:200mm≤continuous casting billet thickness t<400mm, the pulling speed is 0.35~0.39m / min;400mm≤continuous casting billet thickness t<600mm, the pulling speed is 0.16~0.18m / min;600mm≤continuous casting billet thickness t≤700mm, the pulling speed is 0.11~0.12m / min; When the nitrogen content is 0.01%≤N<0.025%:200mm≤continuous casting billet thickness t<400mm, the pulling speed is 0.31~0.34m / min;400mm≤continuous casting billet thickness t<600mm, the pulling speed is 0.14~0.15m / min;600mm≤continuous casting billet thickness t≤700mm, the pulling speed is 0.10~0.11m / min; When the nitrogen content is 0.025%≤N<0.050%:200mm≤continuous casting billet thickness t<400mm, the pulling speed is 0.28~0.31m / min;400mm≤continuous casting billet thickness t<600mm, the pulling speed is 0.12~0.13m / min;600mm≤continuous casting billet thickness t≤700mm, the pulling speed is 0.09~0.10m / min; 2) Different ladle pouring times are set according to the width and thickness of the continuous casting billet, and the ladle pouring time is controlled within 54 to 137 minutes; 3) The cooling water volume in different areas of the secondary cooling zone is set according to the casting speed, so that the stress generated in the continuous casting billet does not exceed its tensile strength, and the maximum stress is near the solidus; 4) The chemical composition of the continuous casting protection slag is calculated by weight percentage: CaO 34%~36%; SiO2 32%~34%; MgO 0.5%~0.7%; Na2O 9%~11%; K2O 0.03%~0.07%; Al2O3 5%~7%; Fe2O3 0.5%~0.8%; F 7.5%~8.5%; C 5%~6%.

2. The method for controlling surface cracks of VN microalloyed steel continuous casting billet according to claim 1, characterized in that: The chemical composition of the VN microalloyed steel continuous casting billet is C: 0.06%-0.20%, Si: 0.10%-0.40%, Mn: 1.0%-3.0%, P≤0.05%, S≤0.05%, V: 0.05%-0.4%, N: 0.01%-0.2%, and the balance is Fe and unavoidable impurity elements.

3. The method for controlling surface cracks of VN microalloyed steel continuous casting billet according to claim 1, characterized in that: The VN microalloyed steel continuous casting billet has a thickness of 400-700 mm and a width of 2000-2600 mm.

4. The method for controlling surface cracks of VN microalloyed steel continuous casting billet according to claim 1, characterized in that: The VN microalloyed steel continuous casting billet is cast using a 120-300 ton steel ladle, and the number of strands of the casting machine is 2.

5. The method for controlling surface cracks of VN microalloyed steel continuous casting billet according to claim 1, characterized in that: The secondary cooling zone is divided into zones 1 to 7, of which zones 1 to 6 are cooled by steam-water nozzles, and zone 7 is cooled by water spray; the cooling water volume of each zone is: zone 1 3.1-4.2 L / s; zone 2 1.9-2.8 L / s; zone 3 0.8-1.4 L / s; zone 4 0.45-0.7 L / s; zone 5 0.27-0.4 L / s; zone 6 0.19-0.32 L / s; zone 7 0.12-0.17 L / s.

6. The method for controlling surface cracks of VN microalloyed steel continuous casting billet according to claim 1, characterized in that: The coarse inclusions and fine inclusions of the VN microalloyed steel continuous casting billet are controlled below level 1.0.

Citation Information

Patent Citations

  • Method of controlling the net crack of high-nitrogen continuous-casting slab of high strength weathering steel containing vanadium

    CN100457327C

  • A method for continuous casting of vanadium- and nitrogen-containing microalloyed peritectic steel billets

    CN107866538B

  • Production method of VN microalloyed steel and VN microalloyed crack-free continuous casting billet

    CN111996466B

  • Method for controlling the cross crack of blank angle of high nitrogen steel casting board containing vanadium

    CN101036939A

  • High strength nickel base corrosion resistance alloy and manufacturing method thereof

    CN102899582A

Cited By

  • Method for controlling surface cracks of microalloy sulfur-containing steel

    CN119304143A

  • A method for controlling surface cracks in microalloyed sulfur-containing steel

    CN119304143B