A hydrophobic aerogel with strong toughness and preparation method thereof
By using a combination method of metal cation solvation and surfactant in strong acid and weak alkali salts in the preparation of silica aerogels, the problems of brittleness and environmental pollution in traditional processes are solved, and high-performance and low-cost gas are achieved. Gel production, suitable for practical applications in a variety of shapes and sizes.
Patent Information
- Application Number
- CN202211632352.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-19
AI Technical Summary
In actual application, the existing silica aerogels are weak in the neck area, resulting in high brittleness and low mechanical properties. The traditional preparation process has problems such as complex process, high cost, and environmental pollution, making it difficult to achieve high efficiency, safety and low quality. Industrial production at cost.
The solvation of metal cations in strong acid and weak alkali salts is used to form hydrated ions. The hydrolysis of the silicon source is catalyzed through hydrolysis reaction, and the micelles are formed in water using surfactants to reduce the surface tension of the solvent, and drying under normal pressure conditions is achieved, so as to avoid high corrosion. A hydrolysis process is regulated to obtain high-performance aerogels.
Silicone aerogel with high thermal stability, high compression strength and good hydrophobicity was prepared. It has a green and environmentally friendly process, which simplifies the production process, reduces costs, and is suitable for practical application needs in a variety of shapes and sizes.
Smart Images

Figure CN116216727B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hydrophobic aerogel with strong toughness and a preparation method thereof, which is particularly suitable for the fields of thermal insulation, water treatment, adsorption and catalysis, and belongs to the technical field of functional materials. Background Art
[0002] Silica aerogel is a porous silicon material composed of a three-dimensional network structure. Its microstructure is similar to a pearl necklace. It has attracted much attention due to its extremely high specific surface area, low density, high porosity and low thermal conductivity. It has broad application prospects in the fields of thermal insulation, water treatment, adsorption and catalysis. However, the neck area of silica aerogel is weak, resulting in its high brittleness and low mechanical properties, which limits its use in practical scenarios.
[0003] Organic-inorganic hybridization is an effective way to strengthen the network structure of silica aerogel and improve its mechanical properties. The current common preparation strategy is to use acid or base to catalyze the organosiloxane precursor, form a wet gel after hydrolysis-condensation reaction, and then obtain the aerogel through aging, surface modification, solvent exchange and drying. The traditional drying process is a supercritical drying process, which requires expensive supercritical drying equipment, needs to be carried out under high temperature or high pressure conditions, and consumes a large amount of liquid CO2. It has the disadvantages of complex process, high cost and potential safety hazards. If the atmospheric pressure drying process is adopted, a hydrophobic modifier, such as hexamethyldisilazane or trimethylchlorosilane, is required for surface modification, and then a large amount of organic solvent is required for multiple solvent exchanges. Although the traditional atmospheric pressure drying process can also produce aerogels with good mechanical properties, its process is not environmentally friendly and has the disadvantages of being time-consuming and highly polluting.
[0004] Chinese patent CN110339788A discloses a method for preparing enhanced silica aerogel, which has a simple process and can be used for large-scale industrial production. However, its formula requires an alcohol organic solvent to form pores in the gel, and after the gel ages, a large amount of anhydrous ethanol is required to replace the solvent in the gel, and a modifier is used to modify the surface of the gel. This process consumes a large amount of organic solvent and is not environmentally friendly.
[0005] Chinese patent CN103496707A discloses a low-cost method for preparing silica aerogel in a pure water system. However, this method only does not use organic solvents, and the prepared silica aerogel is still brittle in texture, and does not improve the shortcomings of silica aerogel such as poor toughness, low strength, and poor mechanical properties.
[0006] In addition, acid is a catalyst for the hydrolysis reaction of the organosilicon source. Its type and concentration affect the sol-gel process of the silicon source and play a vital role in the microstructure, physical properties and various performances of the final aerogel material. Currently, the commonly used acids are proton acids such as hydrochloric acid, nitric acid, sulfuric acid, glacial acetic acid and hydrofluoric acid, which are highly corrosive and irritating and have certain dangers during use. Therefore, the development of safe and harmless acid catalysts and the preparation of low-cost and green and environmentally friendly organosilicon aerogels by atmospheric pressure drying method are hot topics in this field. Summary of the invention
[0007] The purpose of the present invention is to overcome the above-mentioned shortcomings and provide a hydrophobic aerogel with strong toughness and a preparation method thereof, which utilizes the solvation of metal cations in strong acid and weak base salts to form hydrated ions, which are then further hydrolyzed to provide H + To catalyze the hydrolysis reaction of the silicon source, the surfactant can quickly form micelles in water to make the silicon source miscible with water and reduce the surface tension of the solvent. Using water as a solvent, it can both participate in the hydrolysis and create pores, thereby achieving drying under normal pressure to obtain a silicone aerogel with good thermal stability. The preparation process is green, environmentally friendly and simple.
[0008] The technical solution of the present invention is a hydrophobic aerogel with strong toughness, and the formula ratio by weight is as follows: 8-13 parts of organic siloxane, 50-60 parts of deionized water, 0.01-0.03 parts of quaternary ammonium salt surfactant, 1-2 parts of acid catalyst aqueous solution and 0.6-1 part of alkaline catalyst aqueous solution.
[0009] Furthermore, the organosiloxane is one or both of methyltrimethoxysilane MTMS and methyltriethoxysilane MTES.
[0010] Furthermore, the organosiloxane is methyltrimethoxysilane MTMS and methyltriethoxysilane MTES in a molar ratio greater than or equal to 5:1.
[0011] There is the following corresponding relationship between the organosiloxane and the metal chloride:
[0012] When the organosiloxane is entirely methyltrimethoxysilane (MTMS), the metal chloride in the formula is a compound of one or two of copper chloride dihydrate, magnesium chloride hexahydrate, cobalt chloride hexahydrate, aluminum chloride hexahydrate and ferric chloride hexahydrate in any proportion;
[0013] When all the organosiloxanes are methyltriethoxysilane (MTES), the metal chloride in the formula is a composite of one or both of aluminum chloride hexahydrate and ferric chloride hexahydrate in any proportion;
[0014] When the organosiloxane is a compound of methyltrimethoxysilane (MTMS) and methyltriethoxysilane (MTES) and the molar ratio of the two is greater than or equal to 5:1, the metal chloride in the formula is a compound of one or two of copper chloride dihydrate, magnesium chloride hexahydrate, cobalt chloride hexahydrate, aluminum chloride hexahydrate and ferric chloride hexahydrate in any proportion;
[0015] When the organosiloxane is a compound of methyltrimethoxysilane (MTMS) and methyltriethoxysilane (MTES) and the molar ratio of the two is less than 5:1, the metal chloride in the formula is a composite of one or both of aluminum chloride hexahydrate and ferric chloride hexahydrate in any proportion.
[0016] Furthermore, the acid catalyst aqueous solution is specifically a 0.01-0.08 mol / L metal chloride aqueous solution;
[0017] The alkaline catalyst aqueous solution is a 0.5-2.0 mol / L ammonia aqueous solution;
[0018] Furthermore, the metal chloride is a mixture of one or two of copper chloride dihydrate, magnesium chloride hexahydrate, aluminum chloride hexahydrate, ferric chloride hexahydrate and cobalt chloride hexahydrate in any proportion.
[0019] Furthermore, the metal chloride water is specifically a mixture of one or two of aluminum chloride hexahydrate, ferric chloride hexahydrate, cupric chloride dihydrate, magnesium chloride hexahydrate and cobalt chloride hexahydrate in any proportion.
[0020] Furthermore, the quaternary ammonium salt type cationic surfactant is dodecyltrimethylammonium bromide DTAB, dodecyltrimethylammonium chloride DTAC, hexadecyltrimethylammonium bromide CTAB, hexadecyltrimethylammonium chloride CTAC, octadecyltrimethylammonium bromide STAB or octadecyltrimethylammonium chloride STAC.
[0021] The method for preparing the hydrophobic aerogel with strong toughness comprises the following specific steps by weight:
[0022] (1) Preparation of surfactant aqueous solution: 0.01-0.03 parts of quaternary ammonium salt surfactant and 50-60 parts of deionized water are mixed thoroughly and stirred for 2-120 minutes to fully dissolve the surfactant aqueous solution;
[0023] (2) Preparation of acid catalyst aqueous solution: adding metal chloride to deionized water, stirring for 2 to 120 minutes to fully dissolve it, and preparing an acid catalyst aqueous solution with a concentration of 0.01 to 0.08 mol / L;
[0024] (3) Preparation of silica sol: 1-2 parts of the acid catalyst aqueous solution described in step (2) and the surfactant aqueous solution described in step (1) are fully mixed, stirred for 2-120 minutes, and then 8-13 parts of organosiloxane are added, stirred for 0.5-24 hours to obtain silica sol;
[0025] (4) Preparation of silica gel: add 0.6 to 1 part of an aqueous solution of an alkaline catalyst to the silica sol described in step (3), stir for 0.1 to 5 minutes, pour into a mold, and let stand at room temperature to obtain a silica gel;
[0026] (5) Preparation of strong and tough aerogel: The silica gel described in step (4) is aged at room temperature ±50°C for 0 to 48 hours, and then placed in an oven at 60 to 105°C for drying for 6 to 48 hours to obtain a strong and tough hydrophobic aerogel.
[0027] Furthermore, the time interval from the cessation of stirring of the acid catalyst aqueous solution in step (2) to the mixing with the surfactant aqueous solution in step (1) is no more than 48 hours.
[0028] Furthermore, the time interval from stopping stirring of the silica sol in step (3) to compounding with aqueous ammonia is no more than 6 hours.
[0029] Furthermore, in step (5), a blast function is turned on inside the oven.
[0030] The method of the present invention abandons the use of conventional highly polluting and highly corrosive acids such as hydrochloric acid, nitric acid, sulfuric acid and glacial acetic acid, and aims to utilize non-toxic and harmless hydrated metal chlorides, utilize the metal cations thereof to hydrolyze and consume hydroxide ions, and ionize hydrogen ions to promote the hydrolysis reaction of siloxane.
[0031] At the same time, different metal ions have different hydrolysis degrees. Based on this, different metal chlorides can be used to regulate the hydrolysis process of organosiloxane, thereby obtaining aerogel materials with finer internal structures and better performance. While the structural properties can be regulated, it also brings difficulties in the ratio. When the concentration or ratio of metal chloride is too small, the H + The concentration required for catalyzing the hydrolysis of organosiloxane cannot be reached. When the concentration is too high, due to the excessive amount of metal hydroxide obtained by hydrolysis, the silicone hydrogel is prone to cracking during the drying process, resulting in poor formability and aerogel density will increase significantly after drying.
[0032]
[0033] Beneficial effects of the present invention:
[0034] (1) The preparation method of the present invention is green, clean and pollution-free. The preparation method of the present invention utilizes the hydrolysis reaction of metal cations in inorganic chloride to provide a catalyst H for the hydrolysis reaction of the silicon precursor. + , avoiding the dangers of using conventional strong corrosive acids. In addition, the present invention uses surfactant / water as a solvent, replacing the disadvantage of having to use alcohol or alkane organic solvents in traditional processes, and can prepare strong and tough aerogel by drying at normal pressure.
[0035] (2) The prepared aerogel has high thermal stability and a thermal decomposition temperature of 550-700°C, which is higher than the thermal decomposition temperature of traditional polymethylsilsesquioxane aerogel (~450°C).
[0036] (3) The prepared aerogel has high compressive strength (≥0.3MPa) and high maximum compression deformation (≥55%).
[0037] (4) Small shrinkage and high formability enable the preparation of aerogels with various irregular shapes, which are suitable for practical application needs of different sizes and shapes.
[0038] (5) It has very good hydrophobicity and can serve for a long time in a humid environment.
[0039] Compared with the traditional method for preparing silica aerogel, the production process of the present invention is simple, does not require organic solvents, strong corrosive acids and expensive professional drying equipment, has a high safety factor, is energy-saving and environmentally friendly, reduces the production cost of aerogel, and is conducive to market promotion and mass and industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 These are appearance pictures of aerogels of different shapes prepared in Example 1 of the present invention.
[0041] Figure 2 These are appearance pictures of aerogels of different shapes prepared in Example 2 of the present invention.
[0042] Figure 3 These are appearance pictures of aerogels of different shapes prepared in Example 2 of the present invention.
[0043] Figure 4 This is a picture of water droplets falling on the surface of the aerogel prepared in Example 1 of the present invention.
[0044] Figure 5 The water contact angle photos of the aerogels prepared in Examples 1-4 of the present invention;
[0045] a. Example 4; b. Example 3; c. Example 1; d. Example 2.
[0046] Figure 6This is a picture of water droplets falling on the surface of the aerogel prepared in Example 3 of the present invention.
[0047] Figure 7 This is a photo of the aerogel prepared in Example 5 of the present invention floating on the water surface.
[0048] Figure 8 These are stress-strain curves of the aerogels prepared in Examples 1-4 of the present invention.
[0049] Fig. 9 The thermogravimetric curves of the aerogels prepared in Examples 1-4 of the present invention.
[0050] Fig.10 The maximum compressive strain and compressive strength of the aerogel prepared in the embodiment of the present invention are compared with the aerogel prepared in the reference literature.
[0051] Fig.11 The figure is a comparison of the initial decomposition temperature and the maximum thermal weight loss rate at 800° C. between the aerogel prepared in the embodiment of the present invention and the aerogel prepared in the reference literature. DETAILED DESCRIPTION
[0052] The present invention is further explained below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art are all within the scope of the claims attached to this application.
[0053] The stress-strain curve in the embodiment of the present invention is obtained by compressing a sample with a long diameter of 25 cm×15 cm at a rate of 1 mm / min using a universal testing machine.
[0054] Example 1
[0055] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker, and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water;
[0056] (2) In another beaker, 0.16 g of aluminum chloride hexahydrate (AlCl3·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared AlCl3 aqueous solution was added to the beaker in step (1), and magnetically stirred for 3 to 5 minutes;
[0057] (3) Then, 5 g of methyltriethoxysilane was added and magnetic stirring was performed. The mixed solution changed from turbid to clear and transparent within 20 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0058] (4) Add 0.4 mL of 1 mol / L ammonia water to the silica hydrosol, stir for 30 seconds, pour into a mold and let stand at room temperature. After 11 minutes, a completely gelled silica hydrogel is obtained;
[0059] (5) The silica hydrogel was aged at room temperature for 3 h and then dried in an 80°C forced air drying oven for 18 h to obtain a hydrophobic aerogel with strong toughness.
[0060] Example 2
[0061] (1) At room temperature, add 25 g of deionized water and 0.01 g of CTAB into a beaker and stir magnetically for 5 to 10 min until cetyltrimethylammonium bromide is fully dissolved in the deionized water.
[0062] (2) In another beaker, 0.18 g of ferric chloride hexahydrate (FeCl3·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared FeCl3 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0063] The remaining steps are the same as steps (3)-(5) of Example 1.
[0064] Example 3
[0065] (1) At room temperature, add 25 g of deionized water and 0.01 g of CTAB into a beaker and stir magnetically for 5 to 10 min until cetyltrimethylammonium bromide is fully dissolved in the deionized water.
[0066] (2) In another beaker, 0.17 g of copper chloride dihydrate (CuCl2·2H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared CuCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0067] (3) Then, 5 g of methyltrimethoxysilane was added and magnetic stirring was performed. The mixed solution changed from turbid to clear and transparent within 3 minutes. Stirring was continued for 1 hour to obtain a fully hydrolyzed silica hydrosol.
[0068] The remaining steps are the same as steps (4) and (5) of Example 1.
[0069] Example 4
[0070] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0071] (2) In another beaker, 0.2 g of magnesium chloride hexahydrate (MgCl2·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared MgCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0072] The rest of the steps are the same as steps (3) to (5) in Example 3.
[0073] Example 5
[0074] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0075] (2) In another beaker, 0.24 g of cobalt chloride hexahydrate (CoCl2·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared CoCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0076] The rest of the steps are the same as steps (3) to (5) in Example 3.
[0077] Example 6
[0078] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0079] (2) In another beaker, 0.17 g of copper chloride dihydrate (CuCl2·2H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared CuCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0080] (3) Then, 3.41 g of methyltrimethoxysilane and 0.89 g of methyltriethoxysilane (molar ratio 5:1) were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0081] The remaining steps are the same as steps (4) and (5) of Example 1.
[0082] Example 7
[0083] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0084] (2) In another beaker, 0.17 g of copper chloride dihydrate (CuCl2·2H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared CuCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0085] (3) Then, 2.72 g of methyltrimethoxysilane and 1.78 g of methyltriethoxysilane (molar ratio 2:1) were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0086] The remaining steps are the same as steps (4) and (5) of Example 1.
[0087] Example 8
[0088] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0089] (2) In another beaker, 0.17 g of copper chloride dihydrate (CuCl2·2H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared CuCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0090] (3) Then, 2.04 g of methyltrimethoxysilane and 2.67 g of methyltriethoxysilane (molar ratio 1:1) were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0091] The remaining steps are the same as steps (4) and (5) of Example 1.
[0092] Example 9
[0093] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0094] (2) In another beaker, 0.17 g of copper chloride dihydrate (CuCl2·2H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared CuCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0095] (3) Then, 1.36 g of methyltrimethoxysilane and 3.57 g of methyltriethoxysilane (molar ratio 1:2) were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0096] The remaining steps are the same as steps (4) and (5) of Example 1.
[0097] Example 10
[0098] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker, and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water;
[0099] (2) In another beaker, 0.16 g of aluminum chloride hexahydrate (AlCl3·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared AlCl3 aqueous solution was added to the beaker in step (1), and magnetically stirred for 3 to 5 minutes;
[0100] (3) Then, 5 g of methyltrimethoxysilane was added and magnetic stirring was performed. The mixed solution changed from turbid to clear and transparent within 3 min. Stirring was continued for 1 h to obtain a fully hydrolyzed silica hydrosol.
[0101] (4) Add 0.4 mL of 1 mol / L ammonia water to the silica hydrosol, stir for 30 seconds, pour into a mold and let stand at room temperature. After 11 minutes, a completely gelled silica hydrogel is obtained;
[0102] (5) The silica hydrogel was aged at room temperature for 3 h and then dried in an 80°C forced air drying oven for 18 h to obtain a hydrophobic aerogel with strong toughness.
[0103] Embodiment 11
[0104] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0105] (2) In another beaker, 0.18 g of ferric chloride hexahydrate (FeCl3·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared FeCl3 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0106] The remaining steps are the same as steps (3) to (5) of Example 10.
[0107] Example 12
[0108] (1) At room temperature, add 25 g of deionized water and 0.01 g of dodecyltrimethylammonium bromide (DTAB) into a beaker and stir magnetically for 5 to 10 min until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0109] (2) In another beaker, 0.17 g of copper chloride dihydrate (CuCl2·2H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared CuCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0110] (3) Then, 4.09 g of methyltrimethoxysilane and 0.67 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 minutes. Stirring was continued for 3 hours to obtain a fully hydrolyzed silica hydrosol.
[0111] The remaining steps are the same as steps (4) and (5) of Example 1.
[0112] Embodiment 13
[0113] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0114] (2) In another beaker, 0.2 g of magnesium chloride hexahydrate (MgCl2·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared MgCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0115] (3) Then, 4.09 g of methyltrimethoxysilane and 0.67 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 minutes. Stirring was continued for 3 hours to obtain a fully hydrolyzed silica hydrosol.
[0116] The rest of the steps are the same as steps (4) and (5) of Example 1.
[0117] Embodiment 14
[0118] (1) At room temperature, 25 g of deionized water and 0.01 g of dodecyltrimethylammonium chloride (DTAC) were added to a beaker. After magnetic stirring for 5 to 10 min, hexadecyltrimethylammonium bromide was fully dissolved in the deionized water.
[0119] (2) In another beaker, 0.2 g of magnesium chloride hexahydrate (MgCl2·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared MgCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0120] (3) Then, 3.41 g of methyltrimethoxysilane and 0.89 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0121] The rest of the steps are the same as steps (4) and (5) of Example 1.
[0122] Embodiment 15
[0123] (1) At room temperature, 25 g of deionized water and 0.01 g of cetyltrimethylammonium chloride (CTAC) were added into a beaker. After magnetic stirring for 5 to 10 min, cetyltrimethylammonium bromide was fully dissolved in the deionized water.
[0124] (2) In another beaker, 0.2 g of magnesium chloride hexahydrate (MgCl2·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared MgCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0125] (3) Then, 2.72 g of methyltrimethoxysilane and 1.78 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0126] The rest of the steps are the same as steps (4) and (5) of Example 1.
[0127] Example 16
[0128] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker, and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water;
[0129] (2) In another beaker, 0.16 g of aluminum chloride hexahydrate (AlCl3·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared AlCl3 aqueous solution was added to the beaker in step (1), and magnetically stirred for 3 to 5 minutes;
[0130] (3) Then, 3.41 g of methyltrimethoxysilane and 0.89 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0131] The rest of the steps are the same as steps (4) and (5) of Example 1.
[0132] Embodiment 17
[0133] (1) At room temperature, add 25 g of deionized water and 0.01 g of octadecyltrimethylammonium bromide (STAB) into a beaker, and stir magnetically for 5 to 10 min until the octadecyltrimethylammonium bromide is fully dissolved in the deionized water;
[0134] (2) In another beaker, 0.16 g of aluminum chloride hexahydrate (AlCl3·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared AlCl3 aqueous solution was added to the beaker in step (1), and magnetically stirred for 3 to 5 minutes;
[0135] (3) Then, 2.72 g of methyltrimethoxysilane and 1.78 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0136] The rest of the steps are the same as steps (4) and (5) of Example 1.
[0137] Embodiment 18
[0138] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker, and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water;
[0139] (2) In another beaker, 0.16 g of aluminum chloride hexahydrate (AlCl3·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared AlCl3 aqueous solution was added to the beaker in step (1), and magnetically stirred for 3 to 5 minutes;
[0140] (3) Then, 2.04 g of methyltrimethoxysilane and 2.67 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0141] The rest of the steps are the same as steps (4) and (5) of Example 1.
[0142] Embodiment 19
[0143] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water.
[0144] (2) In another beaker, 0.18 g of ferric chloride hexahydrate (FeCl3·6H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared FeCl3 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0145] (3) Then, 2.72 g of methyltrimethoxysilane and 1.78 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0146] The remaining steps are the same as steps (4) and (5) of Example 1.
[0147] Embodiment 20
[0148] (1) At room temperature, 25 g of deionized water and 0.01 g of octadecyltrimethylammonium chloride (STAC) were added to a beaker. After magnetic stirring for 5 to 10 min, the hexadecyltrimethylammonium bromide was fully dissolved in the deionized water.
[0149] (2) In another beaker, 0.1 g of magnesium chloride hexahydrate (MgCl2·6H2O), 0.085 g of cupric chloride dihydrate (CuCl2·2H2O) and 20 g of deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared MgCl2 aqueous solution was added to the beaker described in step (1) and magnetically stirred for 3 to 5 minutes.
[0150] (3) Then, 2.72 g of methyltrimethoxysilane and 1.78 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0151] The rest of the steps are the same as steps (4) and (5) of Example 1.
[0152] Embodiment 21
[0153] (1) At room temperature, add 25 g of deionized water and 0.01 g of hexadecyltrimethylammonium bromide into a beaker, and stir magnetically for 5 to 10 minutes until the hexadecyltrimethylammonium bromide is fully dissolved in the deionized water;
[0154] (2) In another beaker, 0.11 g aluminum chloride hexahydrate (AlCl3·6H2O), 0.06 g ferric chloride hexahydrate (FeCl3·6H2O) and 20 g deionized water were mixed and stirred evenly, and then 0.5 mL of the prepared AlCl3 aqueous solution was added to the beaker in step (1), and magnetic stirring was performed for 3 to 5 minutes;
[0155] (3) Then, 2.72 g of methyltrimethoxysilane and 1.78 g of methyltriethoxysilane were added and magnetically stirred. The mixed solution changed from turbid to clear and transparent within 30 min. Stirring was continued for 3 h to obtain a fully hydrolyzed silica hydrosol.
[0156] The rest of the steps are the same as steps (4) and (5) of Example 1.
[0157] Application Example 1
[0158] The aerogel samples prepared in Examples 1-21 were subjected to performance tests, and the relevant data are shown in Table 1.
[0159] The aerogel samples prepared in Examples 1-6, 10-14 and 16-21 all have good formability and can be formed in different molds without missing corners. Compared with aerogels in other documents that can only be made into rectangular and cylindrical shapes, the aerogels described in this patent can be made into a variety of shapes, with small shrinkage and better formability.
[0160] Table 1 Performance data of Examples 1-21 of the present invention
[0161]
[0162]
[0163] Note: ρ = bulk density, χ = linear shrinkage, θ = water contact angle, E = elastic modulus, σ max = compression strength, ε = maximum compression deformation, λ = thermal conductivity (indoor environment: 24±5℃, 30%-60%RH, 1atm), “-” means that the aerogel is easy to crack and it is difficult to make a block sample with a size greater than or equal to 105*105*15mm, so the thermal conductivity is difficult to measure.
[0164] The stress-strain curves of the aerogels prepared in Examples 1-4 of the present invention are as follows: Figure 8 The thermal weight loss curves of the aerogels prepared in Examples 1-4 of the present invention are shown in Fig. 9 shown.
[0165] After combining various experimental data, we found that:
[0166] (1) Copper chloride dihydrate, magnesium chloride hexahydrate, aluminum chloride hexahydrate, iron chloride hexahydrate and cobalt chloride hexahydrate are suitable for the MTMS system (the silicon source can be fully dissolved in the metal chloride aqueous solution and can subsequently form an aerogel with good mechanical properties);
[0167] (2) Aluminum chloride hexahydrate and ferric chloride hexahydrate are suitable for the MTES system (the silicon source can be fully dissolved in the metal chloride aqueous solution, and aerogels with good mechanical properties can be formed subsequently), while copper chloride dihydrate, magnesium chloride hexahydrate and cobalt chloride hexahydrate are not suitable for the MTES system (the silicon source cannot be fully dissolved in the metal chloride aqueous solution, and the aerogels obtained subsequently have poor mechanical properties, large linear shrinkage and poor formability);
[0168] (3) When MTMS and MTES are compounded in a molar ratio of greater than or equal to 5:1, copper chloride dihydrate, magnesium chloride hexahydrate, cobalt chloride hexahydrate, aluminum chloride hexahydrate and ferric chloride hexahydrate are all applicable, and the mechanical properties of the aerogels prepared are comparable to those of aerogels prepared from pure MTMS or pure MTES silicon sources;
[0169] (4) When MTMS and MTES are compounded at a molar ratio of less than 5:1, copper chloride dihydrate, magnesium chloride hexahydrate, and cobalt chloride hexahydrate are not suitable for the system, and the aerogel obtained has poor mechanical properties, poor formability, and large linear shrinkage;
[0170] (5) When MTMS and MTES are compounded in a molar ratio of less than 5:1, aluminum chloride hexahydrate and ferric chloride hexahydrate are suitable for the system, and the mechanical properties of the aerogels prepared are comparable to those of the aerogels prepared from pure MTES silicon source.
[0171] In general, under the solubilizing effect of surfactants, MTMS, MTES and their composite silicon sources can be prepared through sol-gel and atmospheric pressure drying processes in an aqueous solvent using aqueous solutions of different metal chlorides as acid catalysts to obtain an aerogel with strong toughness, hydrophobicity, formability and thermal insulation.
[0172] According to the method described in the present invention, an organosilicon aerogel with excellent hydrophobicity (>145°), excellent and controllable compression performance (compression modulus of 0.026-0.300 MPa, maximum deformation of 58.5%-87.0%, maximum compressive strength of 0.10-0.58 MPa) and low thermal conductivity (33.55-49.86 mW / (m·K)) can be prepared in a relatively short time (≤20 h), which has comprehensive advantages over the prior art.
[0173] Application Example 2
[0174] The molding photos of the aerogel prepared in Example 1 in different molds are shown in Figure 1 The molding photos of the aerogel prepared in Example 2 in different molds are shown in Figure 2 and Figure 3 .
[0175] The picture of water droplets falling on the surface of the aerogel prepared in Example 1 of the present invention is as follows Figure 4 The water contact angle photos of the aerogels prepared in Examples 1-4 are shown in Figure 5 The picture of water droplets falling on the surface of the aerogel prepared in Example 3 of the present invention is shown in FIG. Figure 6 The photo of the aerogel prepared in Example 5 floating on the water surface is shown in Figure 7 shown.
[0176] It can be seen from the above experimental results that the hydrophobicity of the aerogel prepared in the embodiment of the present invention has reached or is close to reaching super-hydrophobicity, and has a wide range of hydrophobic application scenarios.
[0177] Application Example 3
[0178] The maximum compressive strain and compressive strength, as well as the thermogravimetric comparison, were performed between the aerogels described in other technical documents and the aerogels prepared in the present invention. The specific references for the aerogels are as follows:
[0179] 1.1.He,F.,et al.,Fabrication and simulation analysis of flexiblepolymethylsilsesquioxane(PMSQ)aerogels by using dimethyl sulfoxide(DMSO)assolvent.Materials&Design,2019.173:p.107777.
[0180] 2. Li,
[0181] 3. Zhu, J., H. Ren and Y. Bi, Facile fabrication of machinable low-densitymoisture-resistant silica aerogels. Journal of Porous Materials, 2019.26(2):p.399-407.
[0182] 4.Peng, F., et al., Afacile method to fabricate monolithic alumina–silica aerogels with high surface areas and good mechanicalproperties. Journal of the European Ceramic Society, 2020.40(6):p.2480-2488.
[0183] 5.Lei,C.,et al.,Tailoring structural and physical properties ofpolymethylsilsesquioxane aerogels by adjusting NH3·H2Oconcentration.Microporous and Mesoporous Materials,2018.258:p.236-243.
[0184] 6.Yun,S.,H.Luo and Y.Gao,Low-density,hydrophobic,highly flexibleambient-pressure-dried monolithic bridged silsesquioxane aerogels.Journal ofmaterials chemistry.A,Materials for energy and sustainability,2015.3(7):p.339-3398.
[0185] 7.Ding,J.,et al.,Flexible and super hydrophobicpolymethylsilsesquioxane based silica aerogel for organic solvent adsorptionvia ambient pressure drying technique.Powder Technology,2020.373:p.716-726.
[0186] 8.Guo,T.,et al.,Facile synthesis of highly flexiblepolymethylsilsesquioxane aerogel monoliths with low density,low thermalconductivity and superhydrophobicity.Vacuum,2021.183:p.109825.
[0187] 9.Yang,Z.,et al.,Hyperelastic and hydrophobic silica aerogels withenhanced compressive strength by using VTES / MTMS as precursors.Journal ofNon-Crystalline Solids,2019.525:p.119677.
[0188] 10.Bhagat,S.D.,et al.,Methyltrimethoxysilane based monolithic silicaaerogels via ambient pressure drying.Microporous and Mesoporous Materials,2007.100(1-3):p.350-355.
[0189] 11.Yun,S.,et al.,Facile synthesis of large-sized monolithicmethyltrimethoxysilane-based silica aerogel via ambient pressuredrying.Journal of Sol-Gel Science and Technology,2017.83(1):p.53-63.
[0190] 12.Chen,Y.,et al.,Synthesis of highly flexible silica aerogels byphotoacids generation.Journal of Porous Materials,2018.25(4):p.1027-1034.
[0191] 13.Guo,X.,et al.,Facile Synthesis of Flexible MethylsilsesquioxaneAerogels with Surface Modifications for Sound-Absorbance,Fast Dye Adsorptionand Oil / Water Separation.Molecules,2018.23(4):p.945.
[0192] 14. Cheng, X., et al., Rapid synthesis of ambient pressure dried monolithic silica aerogels using water as the only solvent. Materials Letters, 2017.204: p.157-160.
[0193] 15. Zhang,
[0194] The formulation of the above reference and the properties of the resulting aerogel block are shown in Table 2.
[0195] Table 2 The formulations of references and the properties of the aerogel blocks obtained
[0196]
[0197]
[0198] Note: max = compressive strength, ε = maximum compression deformation, T dec= initial decomposition temperature, ω = maximum thermal weight loss rate at 800°C. TEOS = tetraethoxysilane, MTMS = methyltrimethoxysilane, MTES = methyltriethoxysilane, ASB = alumina, VTES = vinyltriethoxysilane, EDDET = 2,2'-(1,2-ethylenedioxy)diethanethiol, DMDMS = dimethoxydimethylsilane, TESEA = 2-(3-(triethoxysilyl)propylcarbamoyloxy)ethyl acrylate, PDMS = polydimethylsiloxane, PAC = polyimide, DMSO = dimethyl sulfoxide sulfoxide), EtOH = ethanol, DMK = acetone, CTAB = cetyltrimethylammonium bromide, CTAC = n-hexadecyltrimethylammonium chloride, HEA = 2-hydroxyethylacrylate, PAG = triarylsulfonium hexafluoroantimonatesalt, BA = Brunstig acid acid), OA = oxalic acid, AA = acetic acid, HCl = hydrochloric acid, HNO3 = nitric acid.
[0199] Fig.10 The maximum compressive strain and compressive strength of the aerogel prepared in the embodiment of the present invention are compared with the aerogel prepared in the reference literature. Fig.10It can be seen that the maximum compressive strain of the aerogels prepared in Examples 1-5 of the present invention, especially Example 2, is much higher than that of the aerogels reported in the literature, and at the same time has the highest compressive strength (0.58MPa), and has the characteristics of toughness. The aerogel prepared in Reference 1 has a higher maximum compressive strain (~96.0%), but its compressive strength is lower (0.15MPa). The aerogel prepared in Reference 9 has a higher compressive strength (0.571MPa), but its maximum compressive strain is lower (~55%). Therefore, the aerogels prepared in the references cannot be called tough aerogels.
[0200] Fig.11 The comparison of the initial decomposition temperature and the maximum thermal weight loss rate at 800°C between the aerogel prepared in the embodiment of the present invention and the aerogel prepared in the reference is shown in FIG. Fig.11 It can be seen that the initial decomposition temperature of the aerogels prepared in Examples 1-4 of the present invention is between 570 and 670°C, which is much higher than the initial decomposition temperature (300 to 600°C) of the aerogels prepared in the reference. At the same time, the maximum thermal weight loss rate of the aerogels prepared in Examples 1-4 of the present invention at 800°C is less than 20%, which is also lower than the maximum thermal weight loss rate (8% to 90%) of the aerogels prepared in the reference at 800°C. Therefore, the aerogels prepared in the present invention have very good thermal stability.
[0201] Description of reference numerals: Fig.10 and Fig.11 The numbers inside the symbols represent the serial numbers of the references or embodiments of the present invention. The initial decomposition temperature refers to the temperature at which the thermal weight loss measured by thermogravimetry and differential thermal analyzer in N2 atmosphere obviously occurs. The maximum thermal weight loss rate at 800°C refers to the weight loss ratio of the sample caused by heating at 800°C measured by thermogravimetry and differential thermal analyzer in N2 atmosphere.
Claims
1. A method for preparing a hydrophobic aerogel having strong toughness, characterized in that The specific steps by weight are as follows: (1) Preparation of surfactant aqueous solution: Take 0.01-0.03 parts of quaternary ammonium salt surfactant and 50-60 parts of deionized water, mix them thoroughly, and stir for 2-120 min to fully dissolve them to prepare a surfactant aqueous solution; (2) Preparation of acid catalyst aqueous solution: Add metal chloride to deionized water and stir for 2 to 120 min to fully dissolve it to prepare an acid catalyst aqueous solution with a concentration of 0.01 to 0.08 mol / L; (3) Preparation of silica sol: 1-2 parts of the acid catalyst aqueous solution described in step (2) and the surfactant aqueous solution described in step (1) are fully mixed, stirred for 2-120 min, and then 8-13 parts of organosiloxane are added, stirred for 0.5-24 h, to obtain silica sol; (4) Preparation of silica gel: add 0.6-1 part of the alkaline catalyst aqueous solution to the silica sol described in step (3), stir for 0.1-5 min, pour into a mold, and let stand at room temperature to obtain silica gel; (5) Preparation of strong and tough aerogel: The silica gel described in step (4) is aged at room temperature ±50°C for 0 to 48 hours, and then placed in an oven at 60 to 105°C for drying for 6 to 48 hours to obtain a strong and tough hydrophobic aerogel; The organosiloxane is one or both of methyltrimethoxysilane MTMS and methyltriethoxysilane MTES; The acid catalyst aqueous solution is specifically a 0.01-0.08 mol / L metal chloride aqueous solution; the metal chloride is a mixture of one or two of copper chloride dihydrate, magnesium chloride hexahydrate, aluminum chloride hexahydrate, iron chloride hexahydrate and cobalt chloride hexahydrate in any proportion; The alkaline catalyst aqueous solution is a 0.5-2.0 mol / L ammonia aqueous solution; The quaternary ammonium salt surfactant is dodecyltrimethylammonium bromide DTAB, dodecyltrimethylammonium chloride DTAC, hexadecyltrimethylammonium bromide CTAB, hexadecyltrimethylammonium chloride CTAC, octadecyltrimethylammonium bromide STAB or octadecyltrimethylammonium chloride STAC.
2. The method for preparing a hydrophobic aerogel having strong toughness as claimed in claim 1, characterized in that: The time interval from the cessation of stirring of the acid catalyst aqueous solution in step (2) to the mixing with the surfactant aqueous solution in step (1) shall not exceed 48 hours.
3. The method for preparing a hydrophobic aerogel with strong toughness as claimed in claim 1, characterized in that: The time interval from stopping stirring of the silica sol in step (3) to compounding with ammonia water is no more than 6 hours.
4. The method for preparing a hydrophobic aerogel having strong toughness as claimed in claim 1, characterized in that: In step (5), the blowing function is turned on inside the oven.
5. The method for preparing a hydrophobic aerogel with strong toughness as claimed in claim 1, characterized in that: The organosiloxane is a mixture of methyltrimethoxysilane MTMS and methyltriethoxysilane MTES, wherein the molar ratio of MTMS:MTES is greater than or equal to 5:
1.
6. A hydrophobic aerogel with strong toughness prepared by the method according to any one of claims 1 to 5.