A high refractive index glass flake and preparation method thereof
By adjusting the component ratio and process flow of glass flakes, high refractive index glass flakes with a refractive index higher than 1.92 are prepared, which solves the problem of low refractive index of existing glass flakes and enables application in the field of high refractive index materials. Improves the whiteness and brightness of the material.
Patent Information
- Application Number
- CN202310226011.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-10
AI Technical Summary
The existing glass flakes have low refractive index and low whiteness, making it difficult to be well used in the field of high refractive index material applications.
The component ratio is 4 to 9% quartz sand, 1 to 5% titanium dioxide, 2 to 7% barium nitrate, 1 to 3% calcium carbonate, 1 to 3% sodium carbonate, 0.2 to 1% Magnesium oxide, 0.2~1% boric acid, 0.2~1% zinc oxide, 0.2~1 % aluminum hydroxide, 0.2-1% sodium pyroantimonate, 75-90% recycled high-refractive index glass flakes, prepared through kiln melting and hydraulic classification processes to obtain a refractive index greater than 1.92 and a density greater than 4.5g /cm3 high refractive index glass flakes.
It achieves high refractive index, low dispersion, high whiteness, and good brightness glass flakes, and the preparation process is simple and low cost. It is suitable for industrial production and is suitable for coatings, printing inks, cosmetics and other fields.
Smart Images

Figure CN116217078B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of glass, and in particular to a high-refractive-index glass flake and a preparation method thereof. Background Art
[0002] Glass flakes are glass fragments several microns thick. They are made from molten medium-alkali glass above 1200°C through blowing, cooling, crushing, screening and grinding. Glass flakes can be used as anti-corrosion coatings for fillers, with high adhesion and excellent chemical resistance and anti-aging properties. They also have the characteristics of corrosion resistance, good permeability resistance, low film shrinkage, small thermal expansion coefficient, less curing residual stress, wear resistance, simple construction and easy repair.
[0003] Conventional refractive glass flakes, here referring to glass flakes with a refractive index lower than 1.6, are widely used in chemical, metallurgical, chemical fiber, electroplating, construction and other industries. They have good anti-permeability, are unlikely to cause water vapor diffusion, have low film shrinkage, small residual stress on the bonding surface, small thermal expansion coefficient, correspondingly small bonding thermal stress, and less curing residual stress. Although their mechanical strength is not as good as that of FRP linings, they have excellent wear resistance and scratch resistance. However, due to their low refractive index and low whiteness, the light transmittance of glass flakes is very low, making it difficult to be well applied in materials that require high refractive index.
[0004] In order to make low-refractive-index glass flakes used in high-refractive-index environments, there are currently many practices. In 2006, Switzerland developed a glass flake interference pigment, which coated a high-refractive-index dielectric material on a glass substrate with an average thickness of less than 1 μm. The dielectric material is a class of materials composed of metal oxides, which are mainly used in coatings, inkjet printing, textile dyeing and cosmetics. In 2009, Japan developed a coated glass flake, which produces a metallic color by coating the surface of the glass flake with a metal. The interference color produced by the interference of reflected light can be produced by coating the surface of the glass flake with a metal oxide. Using such glass flakes, it can eventually be applied to aspects such as color and gloss of coatings and cosmetics. In 2014, North China University of Water Resources and Hydropower developed a method for preparing a glass flake polyurea anti-corrosion coating. First, remove stains, rust or other debris on the surface of the substrate; second, apply a primer to make the coating bond more firmly to the substrate; then prepare the glass flakes, and then use a spray gun to apply the anti-corrosion coating, and finally obtain a glass flake with a flatness greater than 0.5 mm.
[0005] Chinese patent application CN 1622981 A discloses a glass flake-based multilayer pigment, on which glass flakes are coated with alternating layers of high refractive index and low refractive index, and at least three coating layers. Chinese patent application CN106280550A discloses a glass flake-based anticorrosive pigment and a preparation method thereof, wherein glass flakes are treated with a series of treatment liquids to obtain a polyaniline-coated glass flake iron oxide filter cake, which is then dried to obtain the finished product. Chinese patent application CN 104312209B discloses a glass flake-based pearlescent pigment and a preparation method thereof, wherein a glass flake substrate is coated with multiple layers of different metal oxide films, and finally a glass flake-based pearlescent pigment is synthesized, which has better pearlescent brightness and brighter color, and has been widely used in high-end products.
[0006] All of the above-mentioned materials with high refractive index use glass flakes with low refractive index as the base material, and obtain materials with high refractive index through different processing methods. Glass flakes cannot be directly applied to the application field of high refractive index materials. Based on the above reasons, the present invention develops glass flakes with high refractive index, so that it can directly have high refractive index without being processed. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings of low refractive index and low whiteness of glass flakes produced by the above-mentioned existing production technology, and to provide a method for continuously producing high-refractive index, high-density short-grain glass flakes and preparation methods. The high-refractive index glass flakes obtained according to the component ratio and preparation method of the present invention have high refractive index, small dispersion, high light transmittance, high whiteness, good brightness, low glass crystallization tendency, excellent chemical stability, and the preparation process is simple and inexpensive, and are suitable for industrial production.
[0008] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a high-refractive index glass flake, in which the proportions of its components are, by mass percentage, 4-9% of quartz sand, 1-5% of titanium dioxide, 2-7% of barium nitrate, 1-3% of calcium carbonate, 1-3% of sodium carbonate, 0.2-1% of magnesium oxide, 0.2-1% of boric acid, 0.2-1% of zinc oxide, 0.2-1% of aluminum hydroxide, 0.2-1% of sodium pyroantimonate, and 75-90% of recycled materials.
[0009] The content of Fe2O3 in each component is less than 30ppm.
[0010] The quartz sand must completely pass through a 120-mesh standard sieve.
[0011] The recycled materials are large glass particles that have not formed glass flakes in the production line, or they can be glass particles formed by melting raw materials other than recycled materials in a special use scheme. The recycled materials can pass through a 5-mesh standard sieve and have a water content of less than 3%.
[0012] The glass flakes of the present invention have a refractive index greater than 1.92 and a density greater than 4.5 g / cm 3 The flake thickness is less than 20 microns and the flake diameter is 500-2000 microns.
[0013] The present invention also provides a method for preparing high refractive index glass flakes, which comprises the following steps:
[0014] Step 1) Prepare the materials: weigh each component according to the proportion of each component;
[0015] Step 2), mixing all components except the returned material uniformly to form a mixture;
[0016] Step 3), adding the recycled material to the mixture and mixing again to form a batch material;
[0017] Step 4), adding the batch material into the kiln and melting it until a homogenized glass liquid is obtained;
[0018] Step 5), flowing the glass liquid into cooling water with a certain thickness to form a glass sheet;
[0019] Step 6), by hydraulic classification, the classified glass sheets are collected in sections according to thickness;
[0020] Step 7), the collected glass sheets are subjected to heat treatment and then cooled in air to obtain glass flakes.
[0021] The specific process parameters of each step are:
[0022] Step 1, material preparation: weigh each component according to the distribution ratio of each group;
[0023] Step 2, putting the weighed quartz sand, titanium dioxide, barium nitrate, calcium carbonate, sodium carbonate, magnesium oxide, boric acid, zinc oxide, aluminum hydroxide, and sodium pyroantimonate into a V-type mixer and mixing for 30 to 60 minutes to form a mixture;
[0024] Step 3, adding the weighed recycled material to the above mixed material, mixing for 10 to 20 minutes to form a uniformly mixed batch;
[0025] Step 4: Add the batch material from the feeding port into the kiln which has been heated to 1420 degrees. The batch material goes through four stages: silicate formation, glass formation, glass clarification, and glass homogenization, and is discharged from the discharge port in the working pool of the high-temperature kiln.
[0026] Step 5, the high-temperature glass liquid flows into the room temperature water tank from the narrow slit with a width of 5-10 mm at the lower end of the discharge port under the action of gravity; at the same time, when the glass flows out, the glass is also quickly cooled by running water;
[0027] Step 6, the water in the upper part of the water tank flows from one side of the water tank to the other side together with the glass pieces to the filter screen with an inclination angle of 3° and 400 meshes, so as to achieve hydraulic classification of the glass pieces and separation of the glass pieces from the water, and the water is filtered and naturally collected in the water tank below the filter screen; the glass pieces on the filter screen are collected in sections according to the required thickness, and the large glass particles at the bottom of the water tank are fished out and dried as recycled materials for further use;
[0028] Step 7, add the collected glass flakes to a 600°C electrically heated rotary furnace, wherein the feeding speed is controlled to be 10 kg / h; the number of revolutions of the rotary tube is 25 to 35 revolutions / min, and the heating is performed for 1 hour. Collect the glass flakes coming out of the rotary furnace, put them into barrels, and cool them in air to obtain high refractive index glass flakes.
[0029] The inner wall of the kiln is made of WS41 zirconium corundum material. The material of the feed port is Pt10 alloy material. The lining material of the rotary furnace is 310S stainless steel. The barrel for collecting glass flakes is made of heat-resistant stainless steel.
[0030] The present invention uses the gas "cold burst" principle to form glass flakes. The obtained glass flakes are then naturally graded by water flow gravity, thus realizing the continuous preparation of high-density short-material high-refractive glass flakes. The prepared glass flakes have a refractive index greater than 1.92 and a density greater than 4.5g / cm 3 The flake thickness is less than 20 microns, the flake diameter is 500-2000 microns, the whiteness is high, and the brightness is high. The high refractive index glass flakes obtained according to the preparation method of the present invention have high refractive index, small dispersion, high density, high whiteness, good brightness, small glass crystallization tendency, excellent chemical stability, simple preparation process, low cost, and are suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic diagram of the production device of high refractive index glass flakes, wherein 1 is the feeding port, 2 is the kiln, 3 is the kiln working pool, 4 is the discharge port, 5 is the slit outlet of the downstream port, 6 is the cooling water pipe, 7 is the cooling water tank, 8 is a 400-mesh filter screen, and 9 is a filtered water collection tank. DETAILED DESCRIPTION
[0032] The high refractive index glass flakes of the invention have the following components in percentage by mass: 4-9% quartz sand, 1-5% titanium dioxide, 2-7% barium nitrate, 1-3% calcium carbonate, 1-3% sodium carbonate, 0.2-1% magnesium oxide, 0.2-1% boric acid, 0.2-1% zinc oxide, 0.2-1% aluminum hydroxide, 0.2-1% sodium pyroantimonate, and 75-90% recycled materials.
[0033] The content of Fe2O3 in each component is less than 30ppm. The quartz sand must pass through a 120-mesh standard sieve. The recycled material is a large-particle glass particle that does not form glass flakes in the production line, or it can be a glass particle material formed by melting raw materials other than recycled materials in a special use scheme. The recycled material particles can pass through a 5-mesh standard sieve and have a water content of less than 3%.
[0034] The glass flakes prepared by the present invention have a refractive index greater than 1.92 and a density greater than 4.5 g / cm 3 The flake thickness is less than 20 microns and the flake diameter is 500-2000 microns.
[0035] The equipment structure of the present invention for preparing glass flakes is shown in FIG. Figure 1 , including a kiln 2, on which a feed port 1 and a discharge port 4 are arranged, the feed port 1 is located above one end of the kiln 2, and the discharge port 4 is located below the other end of the kiln 2. A kiln working pool 3 is arranged in the kiln 2, and the batch material added by the feed port 1 enters the kiln working pool 3 for heating and melting, and the glass liquid formed by the complete melting reaction enters the discharge port 4 through the kiln working pool 3. The discharge end of the discharge port 4 is set as a slit 5 structure, and the width of the slit 5 is 5 to 10 mm. A cooling water trough 7 is arranged below the lower discharge port 4, and a cooling water pipe 6 is arranged between the discharge port 4 and the cooling water trough 7. When the glass liquid is discharged from the slit 5 of the discharge port 4, the cooling water pipe 6 sprays water to it to quickly cool the glass liquid. A filter screen 8 is arranged on one side of the discharge port of the cooling water trough 7, and the filter screen 8 is 400 mesh and is set at an inclination of 3°. A filtered water collection water trough 9 is arranged below the filter screen 8. The device further comprises a heating furnace (not shown), which is a rotary heating furnace.
[0036] The inner wall of the kiln 2 is made of WS41 zirconium corundum material. The material of the feed port 4 is Pt10 alloy material.
[0037] The method for preparing high refractive index glass flakes of the present invention comprises the following steps:
[0038] Step 1, material preparation: weigh each component according to the distribution ratio of each group;
[0039] Step 2, mixing the weighed quartz sand, titanium dioxide, barium nitrate, calcium carbonate, sodium carbonate, magnesium oxide, boric acid, zinc oxide, aluminum hydroxide, and sodium pyroantimonate to form a mixture;
[0040] Step 3, adding the weighed recycled material to the above mixed material, mixing for 10 to 20 minutes to form a uniformly mixed batch;
[0041] Step 4, adding the batch material from the feeding port 1 into the high temperature kiln working pool 3 in the kiln 2, the batch material goes through four stages of silicate formation, glass formation, glass clarification and glass homogenization, and is discharged from the discharge port 4 in the high temperature kiln working pool 3; the heating temperature of the kiln is 1420 degrees Celsius.
[0042] Step 5, the high-temperature glass liquid flows into the room-temperature cooling water tank 7 from the slit 5 with a width of 5-10 mm at the lower end of the feed port 4 under the action of gravity; at the same time, when the glass flows out, the flowing cooling water in the cooling water pipe 6 is used to quickly cool the glass;
[0043] Step 6, the glass entering the cooling water tank 7 forms glass sheets, and the water on the top flows together with the glass sheets from one side of the tank to the discharge port on the other side, and flows into the filter through the discharge port of the cooling water tank 7, so as to realize hydraulic classification of the glass sheets and separation of the glass sheets and water. The water is filtered through the filter and naturally collected into the filtered water collection tank 9 below the filter; the filter is set with an inclination angle of 3° and a mesh size of 400.
[0044] The glass pieces on the filter screen 8 are collected in sections according to the required thickness, and the large glass particles at the bottom of the cooling water tank 7 and the filtered water collection tank 9 are fished out and dried as recycled materials for further use;
[0045] Step 7, heat-treat the collected glass pieces, and cool them in the air to obtain glass flakes. Heating treatment: add them to a 600°C electrically heated rotary furnace, where the feeding rate is controlled at 10Kg / h; the number of revolutions of the rotary tube is 25 to 35 turns / min, and heat for 1 hour. Collect the glass pieces coming out of the rotary furnace, put them into a barrel, and cool them in the air to obtain high-refractive index glass flakes. The lining material of the rotary furnace is 310S stainless steel, and the barrel for collecting glass flakes is made of heat-resistant stainless steel.
[0046] The following is a specific description of the preferred embodiments.
[0047] Embodiment 1:
[0048] Step 1, preparing materials: weighing 4% quartz sand, 5% titanium dioxide, 7% barium nitrate, 1% calcium carbonate, 3% sodium carbonate, 1% magnesium oxide, 1% boric acid, 1% zinc oxide, 1% aluminum hydroxide, 1% sodium pyroantimonate, and 75% recycled materials respectively by mass percentage;
[0049] Step 2, putting the weighed quartz sand, titanium dioxide, barium nitrate, calcium carbonate, sodium carbonate, magnesium oxide, boric acid, zinc oxide, aluminum hydroxide, and sodium pyroantimonate into a V-type mixer and mixing for 35 minutes to form a mixture;
[0050] Step 3, adding the weighed recycled material to the above mixed material, mixing for 10 minutes to form a uniformly mixed batch;
[0051] Step 4, adding the batch material from the feeding port 1 into the kiln 2 which has been heated to 1420 degrees, and the batch material goes through four stages, namely silicate formation, glass formation, glass clarification and glass homogenization, and then is discharged from the discharge port 4 in the working pool 3 of the high-temperature kiln;
[0052] Step 5, the high-temperature glass liquid flows into the room-temperature water tank from the slit 5 with a width of 5 mm at the lower end of the feed port 4 under the action of gravity; at the same time, when the glass flows out, the cooling water in the cooling water pipe 6 is used to quickly cool the glass;
[0053] Step 6, the water in the upper part of the water tank flows from the left side to the right side of the cooling water tank 7 together with the glass pieces, with an inclination of 3° and a 400-mesh filter screen 8, to achieve hydraulic classification of the glass pieces and separation of the glass pieces from the water, and the filtered water is naturally collected in the filtered water collection tank 9 below the filter screen;
[0054] Then, the glass pieces on the filter are collected in sections according to the required thickness, and the large glass particles at the bottom of the cooling water tank 7 are fished out and dried as recycled materials for further use;
[0055] Step 7, add the collected glass flakes to a 600°C electrically heated rotary furnace, wherein the feeding speed is controlled to be 10 kg / h; the number of revolutions of the rotary tube is 25 revolutions / min, and the heating is performed for 1 hour. Collect the glass flakes coming out of the rotary furnace, put them into barrels, and cool them in air to obtain high refractive index glass flakes.
[0056] The brightness of the sample was measured using the NFZ-6 retroreflective sign measuring instrument. The light source voltage was 5.78V and the brightness of the sample was measured to be 60cd*1x -1 m -2 ; The refractive index of the obtained glass microspheres was measured to be 1.932 using a WYV-S digital V prism refractometer.
[0057] Embodiment 2:
[0058] Step 1, preparing materials: weighing 5% quartz sand, 5% titanium dioxide, 2% barium nitrate, 2% calcium carbonate, 2% sodium carbonate, 1% magnesium oxide, 1% boric acid, 1% zinc oxide, 1% aluminum hydroxide, 1% sodium pyroantimonate, and 79% recycled materials respectively by mass percentage;
[0059] Step 2, putting the weighed quartz sand, titanium dioxide, barium nitrate, calcium carbonate, sodium carbonate, magnesium oxide, boric acid, zinc oxide, aluminum hydroxide, and sodium pyroantimonate into a V-type mixer and mixing for 40 minutes to form a mixture;
[0060] Step 3, adding the weighed recycled material to the above mixed material, mixing for 15 minutes to form a uniformly mixed batch;
[0061] Step 4, adding the batch material from the feeding port 1 into the kiln 2 which has been heated to 1420 degrees, and the batch material goes through four stages, namely silicate formation, glass formation, glass clarification and glass homogenization, and then is discharged from the discharge port 4 in the working pool 3 of the high-temperature kiln;
[0062] Step 5, the high-temperature glass liquid flows into the room-temperature water tank from the 6-mm-wide slit 5 at the lower end of the feed port 4 under the action of gravity; at the same time, when the glass flows out, the cooling water in the cooling water pipe 6 is used to quickly cool the glass;
[0063] Step 6, the water in the upper part of the water tank flows from the left side to the right side of the cooling water tank 7 together with the glass pieces, with an inclination of 3° and a 400-mesh filter screen 8, to achieve hydraulic classification of the glass pieces and separation of the glass pieces from the water, and the filtered water is naturally collected in the filtered water collection tank 9 below the filter screen;
[0064] Then, the glass pieces on the filter are collected in sections according to the required thickness, and the large glass particles at the bottom of the cooling water tank 7 are fished out and dried as recycled materials for further use;
[0065] Step 7, add the collected glass flakes to a 600°C electrically heated rotary furnace, wherein the feeding speed is controlled to be 10 kg / h; the number of revolutions of the rotary tube is 30 revolutions / min, and the heating is performed for 1 hour. Collect the glass flakes coming out of the rotary furnace, put them into barrels, and cool them in air to obtain high refractive index glass flakes.
[0066] The brightness of the sample was measured using the NFZ-6 retroreflective sign measuring instrument. The light source voltage was 5.78V and the brightness of the sample was measured to be 65cd*1x -1 m -2 ; The refractive index of the obtained glass microspheres was measured to be 1.936 using a WYV-S digital V prism refractometer.
[0067] Embodiment 3:
[0068] Step 1, preparing materials: weighing 6% of quartz sand, 4% of titanium dioxide, 6% of barium nitrate, 3% of calcium carbonate, 1% of sodium carbonate, 1% of magnesium oxide, 1% of boric acid, 1% of zinc oxide, 1% of aluminum hydroxide, 1% of sodium pyroantimonate, and 76% of recycled materials respectively by mass percentage;
[0069] Step 2, putting the weighed quartz sand, titanium dioxide, barium nitrate, calcium carbonate, sodium carbonate, magnesium oxide, boric acid, zinc oxide, aluminum hydroxide, and sodium pyroantimonate into a V-type mixer and mixing for 45 minutes to form a mixture;
[0070] Step 3, adding the weighed recycled material to the above mixed material, mixing for 20 minutes to form a uniformly mixed batch;
[0071] Step 4, adding the batch material from the feeding port 1 into the kiln 2 which has been heated to 1420 degrees, and the batch material goes through four stages, namely silicate formation, glass formation, glass clarification and glass homogenization, and then is discharged from the discharge port 4 in the working pool 3 of the high-temperature kiln;
[0072] Step 5, the high-temperature glass liquid flows into the room temperature water tank from the slit 5 with a width of 7 mm at the lower end of the feed port 4 under the action of gravity; at the same time, when the glass flows out, the cooling water pipe 6 is used to quickly cool the glass;
[0073] Step 6, the water in the upper part of the water tank flows from the left side to the right side of the cooling water tank 7 together with the glass pieces, with an inclination of 3° and a 400-mesh filter screen 8, to achieve hydraulic classification of the glass pieces and separation of the glass pieces from the water, and the filtered water is naturally collected in the filtered water collection tank 9 below the filter screen;
[0074] Then, the glass pieces on the filter are collected in sections according to the required thickness, and the large glass particles at the bottom of the cooling water tank 7 are fished out and dried as recycled materials for further use;
[0075] Step 7, add the collected glass flakes to a 600°C electrically heated rotary furnace, wherein the feeding speed is controlled to be 10 kg / h; the number of revolutions of the rotary tube is 35 revolutions / min, and the heating is performed for 1 hour. Collect the glass flakes coming out of the rotary furnace, put them into barrels, and cool them in air to obtain high refractive index glass flakes.
[0076] The brightness of the sample was measured using the NFZ-6 retroreflective sign measuring instrument. The light source voltage was 5.78V and the brightness of the sample was measured to be 70cd*1x -1 m -2 ; The refractive index of the obtained glass microspheres was measured to be 1.940 using a WYV-S digital V prism refractometer.
[0077] Embodiment 4:
[0078] Step 1, preparing materials: weighing 7% quartz sand, 3% titanium dioxide, 3% barium nitrate, 2% calcium carbonate, 2% sodium carbonate, 1% magnesium oxide, 1% boric acid, 1% zinc oxide, 1% aluminum hydroxide, 1% sodium pyroantimonate, and 78% recycled materials respectively by mass percentage;
[0079] Step 2, putting the weighed quartz sand, titanium dioxide, barium nitrate, calcium carbonate, sodium carbonate, magnesium oxide, boric acid, zinc oxide, aluminum hydroxide, and sodium pyroantimonate into a V-type mixer and mixing for 50 minutes to form a mixture;
[0080] Step 3, adding the weighed recycled material to the above mixed material, mixing for 10 minutes to form a uniformly mixed batch;
[0081] Step 4, adding the batch material from the feeding port 1 into the kiln 2 which has been heated to 1420 degrees, and the batch material goes through four stages, namely silicate formation, glass formation, glass clarification and glass homogenization, and then is discharged from the discharge port 4 in the working pool 3 of the high-temperature kiln;
[0082] Step 5, the high-temperature glass liquid flows into the room temperature water tank from the 8 mm wide slit 5 at the lower end of the feed port 4 under the action of gravity; at the same time, when the glass flows out, the cooling water pipe 6 is used to quickly cool the glass;
[0083] Step 6, the water in the upper part of the water tank flows from the left side to the right side of the cooling water tank 7 together with the glass pieces, with an inclination of 3° and a 400-mesh filter screen 8, to achieve hydraulic classification of the glass pieces and separation of the glass pieces from the water, and the filtered water is naturally collected in the filtered water collection tank 9 below the filter screen;
[0084] Then, the glass pieces on the filter are collected in sections according to the required thickness, and the large glass particles at the bottom of the cooling water tank 7 are fished out and dried as recycled materials for further use;
[0085] Step 7, add the collected glass flakes to a 600°C electrically heated rotary furnace, wherein the feeding speed is controlled to be 10 kg / h; the number of revolutions of the rotary tube is 25 revolutions / min, and the heating is performed for 1 hour. Collect the glass flakes coming out of the rotary furnace, put them into barrels, and cool them in air to obtain high refractive index glass flakes.
[0086] The brightness of the sample was measured using the NFZ-6 retroreflective sign measuring instrument. The light source voltage was 5.78V and the brightness of the sample was measured to be 75cd*1x -1 m -2 ; The refractive index of the obtained glass microspheres was measured to be 1.944 using a WYV-S digital V prism refractometer.
[0087] Embodiment 5:
[0088] Step 1, preparing materials: weighing 8% quartz sand, 2% titanium dioxide, 4% barium nitrate, 2% calcium carbonate, 2% sodium carbonate, 1% magnesium oxide, 1% boric acid, 1% zinc oxide, 1% aluminum hydroxide, 1% sodium pyroantimonate, and 77% recycled materials respectively by mass percentage;
[0089] Step 2, putting the weighed quartz sand, titanium dioxide, barium nitrate, calcium carbonate, sodium carbonate, magnesium oxide, boric acid, zinc oxide, aluminum hydroxide, and sodium pyroantimonate into a V-type mixer and mixing for 55 minutes to form a mixture;
[0090] Step 3, adding the weighed recycled material to the above mixed material, mixing for 15 minutes to form a uniformly mixed batch;
[0091] Step 4, adding the batch material from the feeding port 1 into the kiln 2 which has been heated to 1420 degrees, and the batch material goes through four stages, namely silicate formation, glass formation, glass clarification and glass homogenization, and then is discharged from the discharge port 4 in the working pool 3 of the high-temperature kiln;
[0092] Step 5, the high-temperature glass liquid flows into the room temperature water tank from the 9 mm wide slit 5 at the lower end of the feed port 4 under the action of gravity; at the same time, when the glass flows out, the cooling water pipe 6 is used to quickly cool the glass;
[0093] Step 6, the water in the upper part of the water tank flows from the left side to the right side of the cooling water tank 7 together with the glass pieces, with an inclination of 3° on the 400-mesh filter 8, to achieve hydraulic classification of the glass pieces and separation of the glass pieces from the water, and the filtered water is naturally collected in the filtered water collection tank 9 below the filter;
[0094] Then, the glass pieces on the filter are collected in sections according to the required thickness, and the large glass particles at the bottom of the cooling water tank 7 are fished out and dried as recycled materials for further use;
[0095] Step 7, add the collected glass flakes to a 600°C electrically heated rotary furnace, wherein the feeding speed is controlled to be 10 kg / h; the number of revolutions of the rotary tube is 30 revolutions / min, and the heating is performed for 1 hour. Collect the glass flakes coming out of the rotary furnace, put them into barrels, and cool them in air to obtain high refractive index glass flakes.
[0096] The brightness of the sample was measured using the NFZ-6 retroreflective sign measuring instrument. The light source voltage was 5.78V and the brightness of the sample was measured to be 80cd*1x -1 m -2 ; The refractive index of the obtained glass microspheres was measured to be 1.948 using a WYV-S digital V prism refractometer.
[0097] Embodiment 6:
[0098] Step 1, preparing materials: weighing 9% quartz sand, 1% titanium dioxide, 3% barium nitrate, 1% calcium carbonate, 1% sodium carbonate, 1% magnesium oxide, 1% boric acid, 1% zinc oxide, 1% aluminum hydroxide, 1% sodium pyroantimonate, and 80% recycled materials respectively by mass percentage;
[0099] Step 2, putting the weighed quartz sand, titanium dioxide, barium nitrate, calcium carbonate, sodium carbonate, magnesium oxide, boric acid, zinc oxide, aluminum hydroxide, and sodium pyroantimonate into a V-type mixer and mixing for 60 minutes to form a mixture;
[0100] Step 3, adding the weighed recycled material to the above mixed material, mixing for 20 minutes to form a uniformly mixed batch;
[0101] Step 4, adding the batch material from the feeding port 1 into the kiln 2 which has been heated to 1420 degrees, and the batch material goes through four stages, namely silicate formation, glass formation, glass clarification and glass homogenization, and then is discharged from the discharge port 4 in the working pool 3 of the high-temperature kiln;
[0102] Step 5, the high-temperature glass liquid flows into the room-temperature water tank from the slit 5 with a width of 10 mm at the lower end of the feed port 4 under the action of gravity; at the same time, when the glass flows out, the cooling water pipe 6 is used to quickly cool the glass;
[0103] Step 6, the water in the upper part of the water tank flows from the left side to the right side of the cooling water tank 7 together with the glass pieces, with an inclination of 3° and a 400-mesh filter screen 8, to achieve hydraulic classification of the glass pieces and separation of the glass pieces from the water, and the filtered water is naturally collected in the filtered water collection tank 9 below the filter screen;
[0104] Then, the glass pieces on the filter are collected in sections according to the required thickness, and the large glass particles at the bottom of the cooling water tank 7 are fished out and dried as recycled materials for further use;
[0105] Step 7, add the collected glass flakes to a 600°C electrically heated rotary furnace, wherein the feeding speed is controlled to be 10 kg / h; the number of revolutions of the rotary tube is 35 revolutions / min, and the heating is performed for 1 hour. Collect the glass flakes coming out of the rotary furnace, put them into barrels, and cool them in air to obtain high refractive index glass flakes.
[0106] The brightness of the sample was measured using the NFZ-6 retroreflective sign measuring instrument. The light source voltage was 5.78V and the brightness of the sample was measured to be 85cd*1x -1 m -2 ; The refractive index of the obtained glass microspheres was measured to be 1.95 using a WYV-S digital V prism refractometer.
[0107] A high-refractive-index glass flake produced by the present invention is a filler for an anti-corrosion material and has excellent resistance to medium penetration in the anti-corrosion material, so that the prepared coating has antibacterial and anti-mildew effects and a long service life. The modified glass flakes with high dispersibility and high reactivity make the composite ink have excellent corrosion resistance and anti-penetration power. The prepared ink has good rheology, is easy to flow and print, has strong adhesion after drying, is heat-resistant and corrosion-resistant, and greatly improves the performance of traditional water-based polyurethane ink. At the same time, because it has excellent light stability, it can be added into the pigment for coloring. At present, glass flake materials have been widely used in coatings, printing inks, cosmetics, anti-corrosion materials and other fields.
Claims
1. A high refractive index glass flake, the components of which are distributed in the following proportions by mass: 4-9% quartz sand, 1-5% titanium dioxide, 2-7% barium nitrate, 1-3% calcium carbonate, 1-3% sodium carbonate, 0.2-1% magnesium oxide, 0.2-1% boric acid, 0.2-1% zinc oxide, 0.2-1% aluminum hydroxide, 0.2-1% sodium pyroantimonate, and 75-90% recycled materials.
2. The high refractive index glass flake according to claim 1, characterized in that: The content of Fe2O3 in each component is less than 30ppm.
3. The high refractive index glass flake according to claim 1, characterized in that: The quartz sand must completely pass through a 120-mesh standard sieve.
4. The high refractive index glass flake according to claim 1, characterized in that: The recycled material is glass particles with a water content of less than 3%.
5. The high refractive index glass flake according to claim 1, characterized in that: The glass flakes have a refractive index greater than 1.92 and a density greater than 4.5 g / cm 3 The flake thickness is less than 20 microns and the flake diameter is 500-2000 microns.
6. The method for preparing the high refractive index glass flakes according to any one of claims 1 to 5, comprising the following steps: Step 1) Prepare the materials: weigh each component according to the proportion of each component; Step 2), mixing all components except the returned material uniformly to form a mixture; Step 3), adding the recycled material to the mixture and mixing again to form a batch material; Step 4), adding the batch material into the kiln and melting it until a homogenized glass liquid is obtained; Step 5), flowing the glass liquid into cooling water with a certain thickness to form a glass sheet; Step 6), by hydraulic classification, the classified glass sheets are collected in sections according to thickness; Step 7), the collected glass sheets are subjected to heat treatment and then cooled in air to obtain glass flakes.
7. The preparation method according to claim 6, characterized in that: Step 5) The thickness of the glass liquid when it flows out is 5 to 10 mm.
8. The preparation method according to claim 6, characterized in that: Step 5) Before the glass liquid flows out of the kiln and enters the cooling water, spray cooling water to cool the glass liquid.
9. The preparation method according to claim 6, characterized in that: In step 6), the glass pieces in the cooling water flow with the water flow to a filter screen with an inclination angle of 3° for classification.
10. The preparation method according to claim 6, characterized in that: Step 7), heating temperature 600°C, heating time 1 hour.