Comprehensive recovery method for lithium, aluminum and fluorine in electrolytic aluminum waste residues

By employing electro-controlled ion exchange technology, using lithium-selective and fluorine-selective membrane electrodes, combined with hydrochloric acid-aluminum source mixed leaching and two-stage alkaline precipitation treatment, the problems of low recovery rates of lithium, aluminum, and fluorine in electrolytic aluminum waste residue and equipment blockage have been solved, achieving efficient and green recovery of lithium, aluminum, and fluorine and obtaining high value-added products.

CN118929705APending Publication Date: 2024-11-12SHANXI KEHUA TECH SERVICE CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410921187.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In existing technologies, the recovery of lithium, aluminum, and fluorine from electrolytic aluminum waste has several problems, including crystal blockage of equipment during the evaporation and concentration process of high-salt filtrate, the presence of many impurities in the lithium concentrate affecting crystallization efficiency, and high fluorine content in the tail liquid. Furthermore, traditional electro-controlled ion exchange technology has failed to effectively address the relationship between the target ion content and the membrane electrode loading.

Method used

Using electro-controlled ion exchange technology, lithium and fluorine are extracted and enriched from high-salt filtrate by assembling lithium-selective membrane electrodes and fluorine-selective membrane electrodes, respectively. Combined with hydrochloric acid-aluminum source mixed leaching and two-stage alkaline precipitation treatment, the precise recovery of lithium, aluminum and fluorine is achieved. The content of target ions in the treatment solution is optimized by using a specific combination of anion and cation membrane electrodes and loading ratio.

Benefits of technology

It achieves a lithium recovery rate of ≥95% and a fluorine and aluminum recovery rate of ≥90%, obtaining high-value-added products such as subcrystal, aluminum hydroxide, lithium carbonate, and sodium fluoride. It solves the problems of equipment blockage and the influence of impurity ions, improves crystallization efficiency, and the process is green, efficient, and generates no hydrofluoric acid gas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929705A_ABST
    Figure CN118929705A_ABST
Patent Text Reader

Abstract

The invention discloses a comprehensive recovery method for lithium, aluminum and fluorine in electrolytic aluminum waste residues, and belongs to the field of solid waste resource recycling. According to the method, through hydrochloric acid-aluminum source mixed leaching, two-stage alkali precipitation treatment, lithium brine concentration through electric control selection and tail liquid fluorine ion removal, accurate recycling of fluorine, aluminum and lithium elements in the solid waste is achieved, the obtained product comprises subcryolite, aluminum hydroxide, lithium carbonate and sodium fluoride, the lithium recycling rate is larger than or equal to 95%, and the fluorine and aluminum recycling rate is larger than or equal to 90%. The technical scheme provided by the invention is low in energy consumption, environment-friendly, free of hydrogen fluoride gas output, safe in production process and relatively low in equipment requirement, and has good economic benefits and environmental benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a comprehensive recovery method of lithium, aluminum and fluorine in electrolytic aluminum waste slag, belonging to the field of solid waste resource recovery and utilization. Background Art

[0002] With the rapid development of my country's electronics industry, especially the accelerated industrialization of smart phones, new energy vehicles and new energy power equipment, the demand for lithium resources has increased exponentially. At present, the development of lithium resources in my country mainly includes lithium extraction from ore and lithium extraction from salt lake brine. In recent years, with the continuous improvement of my country's industrial production level, a large amount of solid waste has been generated, occupying a large area and causing serious impacts on the environment and ecology. Nowadays, the research and development of new energy and new materials is accelerating, and lithium-containing solid waste, especially lithium-containing electrolytic aluminum slag, has become a usable resource. Its resource recycling is expected to alleviate the shortage of lithium resources in my country.

[0003] In the prior art, Lin Yan of Kunming University of Science and Technology disclosed a method for recovering lithium from aluminum electrolysis solid waste in Chinese patent CN115872423A. The patent proposes to achieve accurate recovery of fluorine, aluminum and lithium in aluminum electrolysis solid waste by mixed leaching of sulfuric acid and aluminum salt and two-stage graded precipitation, and obtain high value-added products such as sub-cryosphere, aluminum fluoride and lithium carbonate respectively; however, the large amount of acid and alkali introduced in the previous process makes the salt content of the filtrate too high, and the evaporation and concentration process causes excessive crystals to block the feed pump, affecting the production of the process section; in addition, the lithium concentrated solution obtained in the previous process contains a large amount of interfering ions, which affects the crystallization efficiency of the lithium carbonate process; the high fluorine-containing tail liquid after crystallization precipitation is difficult to handle. Chinese patent CN116005006A discloses a method for extracting lithium from waste aluminum slag, which achieves the purpose of extracting lithium from solid fluorine by introducing calcium oxide in the acid leaching process; however, the added value of the calcium fluoride product separated in the process is low, and the fluorine and aluminum elements in the solid waste cannot be well separated and recovered. In addition, there are still problems such as salt crystals clogging equipment during evaporation and concentration, the large number of impurity ions in the obtained lithium-containing concentrated solution affecting the crystallization efficiency, and a high fluorine content in the precipitated tail liquid. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a comprehensive recovery method for lithium, aluminum and fluorine in electrolytic aluminum waste slag, especially to accurately recover lithium, aluminum and fluorine elements in electrolytic aluminum waste slag, and to develop green, clean and efficient resource recovery technology based on the chemical properties of solid waste materials.

[0005] In order to overcome the problem of large amounts of crystals precipitating out and clogging equipment during the evaporation and concentration process of high-salt filtrate in the traditional process, the present invention introduces an electrically controlled ion exchange technology, and selectively extracts and enriches lithium directly from the high-salt filtrate by assembling a lithium selective membrane electrode; at the same time, in order to solve the problem of high fluorine content in the tail liquid of lithium extraction in the traditional process, an electrically controlled ion exchange technology is introduced, and fluorine is enriched from the tail liquid of lithium extraction by assembling a fluorine ion selective membrane electrode, and finally a high value-added sodium fluoride product is obtained. In the prior art, the traditional electrically controlled ion exchange technology mainly focuses on the study of electroactive ion exchange materials and membrane component systems, and the quantitative relationship between the loading ratio of the active substances of the anionic membrane electrode and the target ion content in the treatment solution is not given. However, the present invention provides a specific recovery method, and determines the quantitative relationship between the loading ratio and the target ion content in the treatment solution under different anionic membrane electrode combinations.

[0006] The present invention provides a method for comprehensive recovery of lithium, aluminum and fluorine elements in electrolytic aluminum waste slag, which realizes accurate recovery of fluorine, aluminum and lithium elements in solid waste through hydrochloric acid-aluminum source mixed leaching, two-stage alkaline precipitation treatment, electronically controlled selective concentration of lithium brine and electronically controlled removal of tail liquid fluoride ions. The obtained products include sub-cryolite, aluminum hydroxide, lithium carbonate and sodium fluoride, with a lithium recovery rate of ≥95%, and a fluorine and aluminum recovery rate of ≥90%. The method specifically comprises the following steps: Step 1: Dry and grind the electrolytic aluminum waste slag to 100-200 mesh; Step 2: The ground waste slag powder in step 1 is fully stirred with dilute hydrochloric acid and an aluminum source for 4-6 hours at a reaction temperature of 80-100°C to obtain a mixture A; Step 3: The mixture A is filtered to obtain a filtrate B and a filter residue C. The filter residue C is washed three times and then dried and packaged to obtain sub-cryolite; the filtrate B is adjusted to a pH value of 5-6 by adding alkali solution, and filtered to obtain a filtrate D and a filter residue E; the filtrate D is adjusted to a pH value of 7 by adding sodium carbonate to remove calcium and magnesium, and filtered to obtain a filtrate F and a calcium residue; Step 4: The filtrate F is subjected to lithium extraction and concentration by an electrically controlled ion exchange device equipped with a lithium selective membrane electrode to obtain a receiving liquid G and a treated tail liquid H; a saturated sodium carbonate solution is added to the receiving liquid G, and crude lithium carbonate crystals are obtained by filtration, and a lithium carbonate product is obtained by washing and drying; the treated tail liquid H is subjected to fluorine removal by an electrically controlled ion exchange device equipped with a fluorine selective membrane electrode to obtain a sodium fluoride solution and a treated tail liquid L, and the treated tail liquid L is returned to the receiving liquid G for further lithium extraction.

[0007] Specifically, in the step 2, the mass fraction of the dilute hydrochloric acid is 30% - 35%, the mass ratio of the dilute hydrochloric acid to the waste residue is 1-1.5:1, and water needs to be added to mix with the waste residue powder before adding the dilute hydrochloric acid, and the mass ratio of the added water to the waste residue powder is 4:1-1.5; the aluminum source used is one of aluminum chloride, aluminum hydroxide, and aluminum oxide; in the step 2, the dilute hydrochloric acid is first mixed with the waste residue, and the aluminum source is started to be added after acid leaching for 0.5-1 h, and the aluminum source is added in multiple times until the pH is 1.5-2.0 and then stopped.

[0008] In the step 3, the alkali solution is composed of sodium hydroxide and sodium carbonate, sodium hydroxide is added to adjust the pH value to 3, and then sodium carbonate is added to adjust the pH value to 5-6.

[0009] The lithium selective membrane electrode used in the electric controlled ion exchange device equipped with the lithium selective membrane electrode in step 4 is one of λ-MnO2 and FePO4 membrane electrodes, and the counter electrode is a chloride ion imprinted polypyrrole membrane (PPy-Cl - ), one of the porous carbon electrodes, the mass of lithium in the treatment solution: the mass of the porous carbon electrode: the mass of the λ-MnO2 membrane electrode is 0.09 kg: 8 kg: 6 kg, the mass of lithium in the treatment solution: PPy-Cl - Membrane electrode mass: λ-MnO2 membrane electrode mass is 0.036 kg: 10 kg: 1kg. The fluorine-selective membrane electrode used in the electrically controlled ion exchange device equipped with fluorine-selective membrane electrode is a carbon nanotube @ nickel manganese double metal hydroxide (CNTs@NiMn-LDH) composite membrane electrode, and the counter electrode is a nickel ferrocyanide (NiHCF) membrane electrode. The fluorine mass in the treated liquid: CNTs@NiMn-LDH mass: NiHCF membrane electrode mass is 0.2 kg: 2 kg: 10 kg.

[0010] The electrically controlled ion exchange in step 4 comprises four cyclic operation steps, which are ion selective adsorption, membrane electrode rinsing, desorption concentration, and treatment liquid addition in sequence; deionized water is used for rinsing, wherein the rinsing liquid of the electrically controlled lithium extraction section is mixed with the tail liquid of the adsorption section and enters the electrically controlled defluorination section, and the rinsing liquid of the defluorination section is mixed with the tail liquid of the adsorption section and returns to the lithium precipitation section; the desorption liquid used in the lithium extraction and concentration stage is a 0.5-1 g / L lithium chloride solution; the desorption liquid used in the defluorination and concentration stage is a 1-2 g / L sodium fluoride solution; and the volume of the desorption liquid is half of the volume of the treatment liquid.

[0011] Furthermore, the electrically controlled ion exchange device operates at normal temperature and pressure, and the feed water needs to be filtered to remove organic substances.

[0012] The present invention relates to a partially formulatable ion selective separation mechanism in the electrically controlled ion exchange: .

[0013] Beneficial effects of the present invention: (1) The technical solution of the present invention can achieve high added value and accurate recovery of lithium, aluminum and fluorine elements in electrolytic aluminum waste slag. The whole process is green and efficient, and no hydrofluoric acid gas or high-fluorine tail liquid is generated. It effectively solves the storage problem of waste aluminum electrolyte and obtains high added value products such as sub-cryolite, aluminum hydroxide, lithium carbonate and sodium fluoride.

[0014] (2) The present invention uses an electrically controlled ion exchange section equipped with a lithium selective membrane electrode to replace the traditional evaporation and concentration section, thereby obtaining high-purity lithium brine and solving the problems of large crystallization volume and equipment clogging in the traditional evaporation and concentration process. In addition, the high-purity lithium brine reduces the amount of lithium carbonate solution added in the subsequent lithium carbonate crystallization process, thereby improving the crystallization efficiency.

[0015] (3) The present invention solves the problem of excessively high fluorine content in the tail liquid after lithium carbonate crystallization by adopting a post-treatment section equipped with an electrically controlled ion exchange technology equipped with a fluorine-selective membrane electrode, and simultaneously obtains a high-purity sodium fluoride concentrate.

[0016] (4) The present invention is a clean, green and efficient technology with considerable profits, low energy consumption, no hydrogen fluoride gas output, safe production process, and low equipment requirements. It has good economic, environmental and social benefits and is conducive to promoting the sustainable development of my country's electrolytic aluminum industry, lithium resource development and fluorine product manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A schematic diagram of the process flow of the comprehensive recovery method of solid waste containing lithium, aluminum and fluorine elements of the present invention; Figure 2 Schematic diagram of detailed operation steps of the electronically controlled lithium extraction process of the present invention, with λ-MnO2 / PPy-Cl - Take membrane pairs as an example; Figure 3 Schematic diagram of detailed operation steps of the electrically controlled defluorination section of the present invention, taking the CNTs@NiMn-LDH / NiHCF membrane pair as an example. DETAILED DESCRIPTION

[0018] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] The solid waste components containing lithium, aluminum and fluorine elements used in the following embodiments include: Na3AlF6 50-75%, AlF3 10-15%, Al2O3 5-10%, LiF 8-10%, and CaF2 2-5%.

[0020] Embodiment 1: In this embodiment, the components of the electrolytic aluminum waste slag are Na3AlF6 60%, AlF3 15%, Al2O3 10%, LiF 10%, and CaF2 5%. The detailed implementation steps are as follows: (1) 100 g of solid waste containing lithium, aluminum and fluorine elements was crushed, dried to constant weight, and ground to 200 mesh for later use; (2) Acid leaching: dilute 35% hydrochloric acid with water to a 25% hydrochloric acid solution, then add the powder obtained in step (1) to the prepared 350 mL acid solution, heat to 90 °C and stir to leach for 2 h, then add 20 g aluminum chloride and stir to leach for 1 h, measure the pH, if the pH is greater than 2, filter to obtain filter residue A and filtrate A; if the pH is less than 1, continue to add aluminum chloride to adjust the pH to 2, and then filter; (3) After washing three times, the filter residue was dried at 100 °C to constant weight to obtain 55 g of cryolite product.

[0021] (4) The first washing water is mixed with filtrate A to obtain filtrate B, the second washing water is used as washing water for the next process, and the third washing water is used as hydrochloric acid dilution water in step 1.

[0022] (5) Primary neutralization: Add 5 g of NaOH to the filtrate B obtained in step (4) to adjust the pH to 3, then add 15 g of Na2CO3 to adjust the pH to 5, raise the temperature to 80 °C and stir to react for 2 h to generate aluminum fluoride and aluminum hydroxide precipitates, which are then filtered to obtain filter residue C and filtrate C.

[0023] (6) The filter residue C is washed, dried at 100 °C to constant weight, and reused as an aluminum source in step (2).

[0024] (7) Secondary neutralization: sodium carbonate was added to the filtrate C obtained in step (5) to adjust the pH to 7, and calcium and magnesium ions were removed from the filtrate C. 500 mL of filtrate D and filter residue D were obtained by filtration. The lithium ion content in the filtrate D was found to be 1000 ppm by testing.

[0025] (8) Electro-controlled lithium extraction: The filtrate D is passed into a reactor equipped with λ-MnO2 / PPy-Cl - The electrically controlled ion exchange device of the membrane electrode pair, in which the λ-MnO2 membrane electrode loading is 13.5 g, and the PPy-Cl -The membrane electrode mass is 138.5 g. The selective adsorption stage is operated with constant current discharge, the applied current is -30 mA / g, and the system cutoff voltage is 0.3 V. The rinsing stage uses deionized water to rinse repeatedly for 0.5 h. The desorption stage is desorbed at a constant pressure, the cell voltage is 1.2 V, the operation time is 60 min, and the desorption liquid is 1 g / L LiCl solution. After adsorption, the tail liquid E is obtained, and the fluoride ion content is 100 ppm. The main components of the lithium-containing mother liquor obtained after the desorption stage are as follows (the content of other elements has not reached the detection limit):

[0026] (9) Electrically controlled defluorination: The tail liquid E is passed into an electrically controlled ion exchange device equipped with a CNTs@NiMn-LDH / NiHCF membrane electrode pair. The mass of the CNTs@NiMn-LDH membrane electrode is 100 mg, and the mass of the NiHCF membrane electrode is 500 mg. The operating voltage in the selective adsorption stage is 0.6 V, and the operation time is 40 min. The rinsing stage is repeatedly rinsed with deionized water for 0.5 h. The cell voltage in the desorption stage is 1.0 V, and the operation time is 1 h. The desorption liquid is 1 g / L NaF solution. The tail liquid F obtained after adsorption is returned to the electrically controlled lithium extraction section. The main components of the fluorine-containing mother liquor obtained after desorption are as follows (the content of other elements does not reach the detection limit):

[0027] The main components of tail liquid F are as follows (the contents of other elements do not reach the detection limit):

[0028] (10) Lithium precipitation: The lithium-containing mother liquor in step (8) is used as the base liquid, and solid sodium carbonate is added while stirring, wherein the amount of solid sodium carbonate added is 133 g. After the addition is completed, the mixture is reacted at 85°C for 2 h, and crude lithium carbonate is obtained by filtration. The crude lithium carbonate is washed and dried to obtain a lithium carbonate product with a content of 99.5%.

[0029] Embodiment 2: In this embodiment, the components of the electrolytic aluminum waste slag are Na3AlF665%, AlF315%, Al2O35%, LiF 10%, and CaF25%. The detailed implementation steps are as follows: (1) 100 g of solid waste containing lithium, aluminum and fluorine elements was crushed, dried to constant weight, and ground to 200 mesh for later use; (2) Acid leaching: dilute 30% hydrochloric acid with water to a 25% hydrochloric acid solution, then add the powder obtained in step (1) to the prepared 400 mL acid solution, heat to 80 °C and stir to leach for 2 h, then add 20 g aluminum chloride and stir to leach for 0.5 h, measure the pH, if the pH is greater than 2, filter to obtain filter residue A and filtrate A; if the pH is less than 1, continue to add aluminum chloride to adjust the pH to 2, and then filter; (3) After washing three times, the filter residue was dried at 100 °C to constant weight to obtain 58 g of cryolite product.

[0030] (4) The first washing water is mixed with filtrate A to obtain filtrate B, the second washing water is used as washing water for the next process, and the third washing water is used as hydrochloric acid dilution water in step 1.

[0031] (5) Primary neutralization: Add 8 g of NaOH to the filtrate B obtained in step (4) to adjust the pH to 3, then add 12 g of Na2CO3 to adjust the pH to 5, raise the temperature to 80 °C and stir to react for 2 h to generate aluminum fluoride and aluminum hydroxide precipitates, which are then filtered to obtain filter residue C and filtrate C.

[0032] (6) The filter residue C is washed, dried at 100 °C to constant weight, and reused as an aluminum source in step (2).

[0033] (7) Secondary neutralization: sodium carbonate was added to the filtrate C obtained in step (5) to adjust the pH to 7, and calcium and magnesium ions were removed from the filtrate C. 700 mL of filtrate D and filter residue D were obtained by filtration. The lithium ion content of the filtrate D was 800 ppm.

[0034] (8) Electrically controlled lithium extraction: The filtrate D was passed into an electrically controlled ion exchange device equipped with a λ-MnO2 / activated carbon membrane electrode pair, where the λ-MnO2 membrane electrode loading was 36 g, and the PPy-Cl - The membrane electrode mass is 48 g. The constant voltage operation voltage in the selective adsorption stage is 1.0 V, the operation time is 20 min, the rinsing stage is repeatedly rinsed with deionized water for 0.5 h, the cell voltage in the desorption stage is 1.2 V, the operation time is 40 min, and the desorption liquid is 1 g / L LiCl solution. After adsorption, the tail liquid E is obtained, and the fluoride ion content is 80 ppm. The main components of the lithium-containing mother liquor obtained after the desorption stage are as follows (the content of other elements has not reached the detection limit):

[0035] (9) Electrically controlled defluorination: The tail liquid E is passed into an electrically controlled ion exchange device equipped with a CNTs@NiMn-LDH / NiHCF membrane electrode pair. The mass of the CNTs@NiMn-LDH membrane electrode is 80 mg, and the mass of the NiHCF membrane electrode is 480 mg. The operating voltage in the selective adsorption stage is 0.6 V, and the operating time is 40 min. The rinsing stage is repeatedly rinsed with deionized water for 0.5 h. The cell voltage in the desorption stage is 1.0 V, and the operating time is 1 h. The desorption liquid is 1 g / L NaF solution. The tail liquid F obtained after adsorption is returned to the electrically controlled lithium extraction section. The main components of the fluorine-containing mother liquor obtained after desorption are as follows (the content of other elements does not reach the detection limit):

[0036] The main components of tail liquid F are as follows (the contents of other elements do not reach the detection limit):

[0037] (10) Lithium precipitation: The lithium-containing mother liquor in step (8) is used as the base liquid, and solid sodium carbonate is added while stirring, wherein the amount of solid sodium carbonate added is 180 g. After the addition is completed, the mixture is reacted at 85°C for 3 h, and crude lithium carbonate is obtained by filtration. The crude lithium carbonate is washed and dried to obtain a lithium carbonate product with a content of 99.5%.

[0038] Embodiment 3: In this embodiment, the components of the electrolytic aluminum waste slag are Na3AlF675%, AlF310%, Al2O35%, LiF8%, and CaF22%. The detailed implementation steps are as follows: (1) 100 g of solid waste containing lithium, aluminum and fluorine elements was crushed, dried to constant weight, and ground to 200 mesh for later use; (2) Acid leaching: dilute 35% hydrochloric acid with water to a 25% hydrochloric acid solution, then add the powder obtained in step (1) to the prepared 400 mL acid solution, heat to 100 °C and stir to leach for 3 h, then add 20 g aluminum chloride and stir to leach for 2 h, measure the pH, if the pH is greater than 2, filter to obtain filter residue A and filtrate A; if the pH is less than 1, continue to add aluminum chloride to adjust the pH to 2, and then filter; (3) After washing three times, the filter residue was dried at 100 °C to constant weight to obtain 60 g of cryolite product.

[0039] (4) The first washing water is mixed with filtrate A to obtain filtrate B, the second washing water is used as washing water for the next process, and the third washing water is used as hydrochloric acid dilution water in step 1.

[0040] (5) Primary neutralization: Add 10 g of NaOH to the filtrate B obtained in step 4 to adjust the pH to 3, then add 10 g of Na2CO3 to adjust the pH to 5, heat to 80 °C and stir to react for 3 h to generate aluminum fluoride and aluminum hydroxide precipitates, which are then filtered to obtain filter residue C and filtrate C.

[0041] (6) The filter residue C is washed, dried at 100 °C to constant weight, and reused as an aluminum source in step (2).

[0042] (7) Secondary neutralization: Sodium carbonate was added to the filtrate C obtained in step 5 to adjust the pH to 7, and calcium and magnesium ions were removed from the filtrate C. 1000 mL of filtrate D and filter residue D were obtained by filtration. The lithium ion content in the filtrate D was found to be 1000 ppm by testing.

[0043] (8) Electro-controlled lithium extraction: The filtrate D is passed into a reactor equipped with λ-MnO2 / PPy-Cl - The electronically controlled ion exchange device of the membrane electrode pair, in which the λ-MnO2 membrane electrode loading is 27 g, and the PPy-Cl - The membrane electrode mass is 277 g. The selective adsorption stage is operated with constant current discharge, the applied current is -30 mA / g, and the system cutoff voltage is 0.3 V. The rinsing stage is repeatedly rinsed with deionized water for 0.5 h. The desorption stage is operated with constant current charging, the applied current is 30 mA / g, the system cutoff voltage is 1.2 V, and the desorption liquid is 0.5 g / L LiCl solution. After adsorption, the tail liquid E is obtained, and the fluoride ion content is 100 ppm. The main components of the lithium-containing mother liquor obtained after the desorption stage are as follows (the content of other elements has not reached the detection limit):

[0044] (9) Electrically controlled defluorination: The tail liquid E is passed into an electrically controlled ion exchange device equipped with a CNTs@NiMn-LDH / NiHCF membrane electrode pair. The mass of the CNTs@NiMn-LDH membrane electrode is 200 mg, and the mass of the NiHCF membrane electrode is 1000 mg. The operating voltage in the selective adsorption stage is 0.6 V, and the operating time is 40 min. The rinsing stage is repeatedly rinsed with deionized water for 0.5 h. The cell voltage in the desorption stage is 1.0 V, and the operating time is 1 h. The desorption liquid is 1 g / L NaF solution. The tail liquid F obtained after adsorption is returned to the electrically controlled lithium extraction section. The main components of the fluorine-containing mother liquor obtained after desorption are as follows (the content of other elements does not reach the detection limit):

[0045] The main components of tail liquid F are as follows (the contents of other elements do not reach the detection limit):

[0046] (10) Lithium precipitation: The lithium-containing mother liquor in step (8) is used as the base liquid, and solid sodium carbonate is added while stirring, wherein the amount of solid sodium carbonate added is 300 g. After the addition is completed, the mixture is reacted at 85°C for 2 h, and crude lithium carbonate is obtained by filtration. The crude lithium carbonate is washed and dried to obtain a lithium carbonate product with a content of 99.5%.

[0047] Embodiment 4: In this embodiment, the components of the electrolytic aluminum waste slag are Na3AlF6 60%, AlF3 15%, Al2O3 10%, LiF 10%, and CaF2 5%. The detailed implementation steps are as follows: (1) 200 g of solid waste containing lithium, aluminum and fluorine elements was crushed, dried to constant weight, and ground to 200 mesh for later use; (2) Acid leaching: dilute 35% hydrochloric acid with water to a 25% hydrochloric acid solution, then add the powder obtained in step (1) to the prepared 700 mL acid solution, heat to 90 °C and stir to leach for 2 h, then add 40 g aluminum chloride and stir to leach for 1 h, measure the pH, if the pH is greater than 2, filter to obtain filter residue A and filtrate A; if the pH is less than 1, continue to add aluminum chloride to adjust the pH to 2, and then filter; (3) After washing three times, the filter residue was dried at 100 °C to constant weight to obtain 105 g of cryolite product.

[0048] (4) The first washing water is mixed with filtrate A to obtain filtrate B, the second washing water is used as washing water for the next process, and the third washing water is used as hydrochloric acid dilution water in step 1.

[0049] (5) Primary neutralization: Add 10 g NaOH to the filtrate B obtained in step 4 to adjust the pH to 3, then add 30 g Na2CO3 to adjust the pH to 5, heat to 80 °C and stir to react for 2 h to generate aluminum fluoride and aluminum hydroxide precipitates, which are then filtered to obtain filter residue C and filtrate C.

[0050] (6) The filter residue C is washed, dried at 100 °C to constant weight, and reused as an aluminum source in step (2).

[0051] (7) Secondary neutralization: Sodium carbonate was added to the filtrate C obtained in step 5 to adjust the pH to 7, and calcium and magnesium ions were removed from the filtrate C. 800 mL of filtrate D and filter residue D were obtained by filtration. The lithium ion content in the filtrate D was tested to be 1000 ppm.

[0052] (8) Electro-controlled lithium extraction: The filtrate D is passed into a reactor equipped with λ-MnO2 / PPy-Cl - The electrically controlled ion exchange device of the membrane electrode pair, in which the λ-MnO2 membrane electrode loading is 24.3 g, and the PPy-Cl -The membrane electrode mass is 250 g. The selective adsorption stage is operated with constant current discharge, the applied current is -30 mA / g, and the system cutoff voltage is 0.3 V. The rinsing stage uses deionized water to rinse repeatedly for 0.5 h. The desorption stage is desorbed at a constant pressure, the cell voltage is 1.2 V, the operation time is 60 min, and the desorption liquid is 1 g / L LiCl solution. After adsorption, the tail liquid E is obtained, and the fluoride ion content is 100 ppm. The main components of the lithium-containing mother liquor obtained after the desorption stage are as follows (the content of other elements has not reached the detection limit):

[0053] (9) Electrically controlled defluorination: The tail liquid E is passed into an electrically controlled ion exchange device equipped with a CNTs@NiMn-LDH / NiHCF membrane electrode pair. The mass of the CNTs@NiMn-LDH membrane electrode is 180 mg, and the mass of the NiHCF membrane electrode is 900 mg. The operating voltage in the selective adsorption stage is 0.6 V, and the operating time is 40 min. The rinsing stage is repeatedly rinsed with deionized water for 0.5 h. The cell voltage in the desorption stage is 1.0 V, and the operating time is 1 h. The desorption liquid is 1 g / L NaF solution. The tail liquid F obtained after adsorption is returned to the electrically controlled lithium extraction section. The main components of the fluorine-containing mother liquor obtained after desorption are as follows (the content of other elements does not reach the detection limit):

[0054] The main components of tail liquid F are as follows (the contents of other elements do not reach the detection limit):

[0055] (10) Lithium precipitation: The lithium-containing mother liquor in step (8) is used as the base liquid, and solid sodium carbonate is added while stirring, wherein the amount of solid sodium carbonate added is 300 g. After the addition is completed, the mixture is reacted at 85°C for 2 h, and crude lithium carbonate is obtained by filtration. The crude lithium carbonate is washed and dried to obtain a lithium carbonate product with a content of 99.5%.

Claims

1. A method for comprehensive recovery of lithium, aluminum and fluorine elements from electrolytic aluminum waste slag, characterized in that: Through hydrochloric acid-aluminum source mixed leaching, two-stage alkaline precipitation treatment, electronically controlled selective concentration of lithium brine and electronically controlled removal of fluoride ions in tail liquid, accurate recovery of fluorine, aluminum and lithium elements in solid waste is achieved. The products obtained include sub-cryospar, aluminum hydroxide, lithium carbonate and sodium fluoride. The lithium recovery rate is ≥95%, and the fluorine and aluminum recovery rates are ≥90%.

2. The method for comprehensive recovery of lithium, aluminum and fluorine elements from electrolytic aluminum waste slag according to claim 1, characterized in that: The following steps are involved: Step 1: Dry and grind the electrolytic aluminum waste slag to 100-200 mesh; Step 2: The ground waste slag powder in step 1 is fully stirred with dilute hydrochloric acid and an aluminum source for 4-6 hours at a reaction temperature of 80-100°C to obtain a mixture A; Step 3: The mixture A is filtered to obtain a filtrate B and a filter residue C. The filter residue C is washed three times and then dried and packaged to obtain sub-cryolite; the filtrate B is adjusted to a pH value of 5-6 by adding alkali solution, and filtered to obtain a filtrate D and a filter residue E; the filtrate D is adjusted to a pH value of 7 by adding sodium carbonate to remove calcium and magnesium, and filtered to obtain a filtrate F and a calcium residue; Step 4: The filtrate F is subjected to lithium extraction and concentration by an electrically controlled ion exchange device equipped with a lithium selective membrane electrode to obtain a receiving liquid G and a treated tail liquid H; a saturated sodium carbonate solution is added to the receiving liquid G, and crude lithium carbonate crystals are obtained by filtration, and a lithium carbonate product is obtained by washing and drying; the treated tail liquid H is subjected to fluorine removal by an electrically controlled ion exchange device equipped with a fluorine selective membrane electrode to obtain a sodium fluoride solution and a treated tail liquid L, and the treated tail liquid L is returned to the receiving liquid G for further lithium extraction.

3. The method for comprehensive recovery of lithium, aluminum and fluorine elements from electrolytic aluminum waste slag according to claim 2, characterized in that: In the step 2, the mass fraction of the dilute hydrochloric acid is 30% - 35%, the mass ratio of the dilute hydrochloric acid to the waste residue is 1-1.5:1, and water needs to be added to mix with the waste residue powder before adding the dilute hydrochloric acid, and the mass ratio of the added water to the waste residue powder is 4:1-1.

5.

4. The method for comprehensive recovery of lithium, aluminum and fluorine elements from electrolytic aluminum waste slag according to claim 3, characterized in that: In step 2, dilute hydrochloric acid is first mixed with the waste residue, and aluminum source is added after acid leaching for 0.5-1 h. The aluminum source is added in multiple times and the addition is stopped when the pH reaches 1.5-2.

0.

5. The method for comprehensive recovery of lithium, aluminum and fluorine elements from electrolytic aluminum waste slag according to claim 4, characterized in that: The aluminum source used is one of aluminum chloride, aluminum hydroxide and aluminum oxide.

6. The method for comprehensive recovery of lithium, aluminum and fluorine elements from electrolytic aluminum waste slag according to claim 2, characterized in that: In the step 3, the alkali solution is composed of sodium hydroxide and sodium carbonate, sodium hydroxide is added to adjust the pH value to 3, and then sodium carbonate is added to adjust the pH value to 5-6.

7. The method for comprehensive recovery of lithium, aluminum and fluorine elements from electrolytic aluminum waste slag according to claim 2, characterized in that: The lithium selective membrane electrode used in the electrically controlled ion exchange device equipped with a lithium selective membrane electrode in step 4 is one of λ-MnO2 and FePO4 membrane electrodes, and its counter electrode is one of chloride ion imprinted polypyrrole membrane and porous carbon electrode.

8. The method for comprehensive recovery of lithium, aluminum and fluorine elements from electrolytic aluminum waste slag according to claim 7, characterized in that: The mass of lithium in the treatment solution is: The mass of the porous carbon electrode is: 0.09 kg : 8 kg : 6 kg, the mass of lithium in the treatment solution is: PPy-Cl - Membrane electrode mass: The mass of λ-MnO2 membrane electrode is 0.036 kg: 10 kg: 1 kg.

9. The method for comprehensive recovery of lithium, aluminum and fluorine elements from electrolytic aluminum waste slag according to claim 2, characterized in that: The fluorine-selective membrane electrode used in the electrically controlled ion exchange device equipped with a fluorine-selective membrane electrode in step 4 is a carbon nanotube@nickel manganese double metal hydroxide composite membrane electrode, and the counter electrode is a nickel ferrocyanide membrane electrode. The mass of fluorine in the treatment liquid: the mass of CNTs@NiMn-LDH: the mass of NiHCF membrane electrode is 0.2 kg: 2 kg: 10 kg.

Citation Information

Cited By

  • Harmless fluorine removal method for electrolytic aluminum waste residues

    CN120169786A

  • A harmless defluorination method for electrolytic aluminum waste slag

    CN120169786B

  • Electrolytic aluminum waste residue comprehensive treatment and lithium recovery method

    CN121250100A