A fuel cell housing, a method for manufacturing the fuel cell, and the fuel cell itself.
By combining conductive tape, insulating prepreg, and energy-absorbing foam layer in a sandwich structure, the shortcomings of fuel cell assembly housing in terms of heat resistance, insulation, and electromagnetic shielding are solved, achieving high strength and high insulation performance, and improving the stability and design flexibility of the housing under extreme conditions.
Patent Information
- Application Number
- CN202310262059.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-03-17
AI Technical Summary
Existing fuel cell assembly housings are inadequate in terms of heat resistance, insulation, mechanical strength, and electromagnetic shielding. In particular, traditional materials perform poorly at high temperatures and cannot meet the requirements under extreme conditions.
The fuel cell housing is manufactured using a sandwich structure, comprising a conductive tape layer, an insulating prepreg layer, and an energy-absorbing foam layer, and is formed by compression molding. The conductive tape is located on the outer layer, the insulating prepreg layer is located on the inner layer, and the energy-absorbing foam layer is located in the middle, providing high strength, heat resistance, and insulation properties.
It improves the insulation strength and electromagnetic shielding effect of the fuel cell casing, reduces the impact of folded breaks, enhances the heat resistance of the casing, reduces the design gap between the casing and the battery, and increases the design freedom of the battery structure.
Smart Images

Figure CN116231030B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of fuel cell technology, and in particular to a fuel cell housing, a preparation method thereof, and a fuel cell. Background Technology
[0002] In the early development of hydrogen fuel cells, the structure was modeled after traditional battery systems. Initially, bipolar plates were used to form individual cells, which were then fitted with housings to create battery packs. Multiple battery packs were integrated and assembled into a single housing, forming a cell-housing-air-assembly housing structure. Therefore, the cell housing was responsible for hydrogen resistance, insulation, mechanical strength, and electromagnetic shielding. Typically, cell housings were made of composite materials or ceramics, while the assembly housing was made of metals such as aluminum alloys. However, with technological advancements, the design of fuel cell cells has changed. In the past, bipolar plate packs used inlet end plates on both sides to deliver hydrogen, and top and bottom current collectors met current conductivity requirements. The function of the original cell housing was eliminated, resulting in a bipolar plate-air-assembly housing structure. Furthermore, hydrogen fuel cells typically place the DC-DC converter (DCDC) in the upper part of the housing, requiring high strength from both the upper and lower housings, making it impossible to use ordinary power battery housing materials.
[0003] The individual battery casing is cooled by a cooling water circuit and only supports a single battery unit. Its mechanical strength and heat resistance requirements (maximum 90℃) are relatively low. However, the assembly casing needs to meet the requirements of heat resistance, insulation, mechanical strength, and electromagnetic shielding. Since all bipolar plates are installed on the assembly casing, the mechanical strength requirements of the assembly casing are much greater than those of traditional individual battery casings (6-10 times or more). Furthermore, since the assembly casing does not have a water circulation cooling system, its heat resistance needs to be improved to above 120℃. While ensuring heat resistance and mechanical strength, the assembly casing still needs to meet the requirements of insulation and electromagnetic shielding.
[0004] Traditional assembly housings are made of metals such as aluminum alloys. While these materials can meet requirements for heat resistance, mechanical strength, and electromagnetic shielding, the presence of an oxide film or anodizing treatment on the aluminum alloy surface makes it difficult for insulating coatings to adhere effectively, thus affecting insulation performance. Therefore, it is of paramount importance to ensure that the assembly housing simultaneously meets the requirements for heat resistance, insulation, mechanical strength, and electromagnetic shielding.
[0005] In some related technologies, fuel cell casings employ a multi-layer structure design, with each layer's material meeting specific requirements for insulation, mechanical strength, and electromagnetic shielding. However, these solutions still have some drawbacks, including but not limited to the following:
[0006] 1. In related technologies, the individual battery casing is cooled by a cooling water circuit and only supports a single battery unit. The mechanical strength and heat resistance requirements (maximum 90℃) are relatively low. Only the second layer of the three layers can withstand mechanical forces, and it is mainly used to meet the puncture resistance function. Applying the individual battery casing material to the assembly casing cannot meet the mechanical strength and heat resistance requirements.
[0007] 2. In related technologies, only the third layer of the single-cell battery casing has high-voltage electrical insulation function. This insulation is achieved by using non-conductive polymer and glass fiber composite materials. Since the first layer is a conductive material, the electrical insulation strength is limited by the thickness of the third layer. Due to volume limitations, the thickness of the single-cell battery casing cannot be too high, so it can only meet the breakdown voltage requirement of 2500V, but the insulation resistance is low (<100MΩ). This material cannot meet the various extreme insulation requirements of the assembly when applied to the assembly casing.
[0008] 3. In related technologies, the first layer of the single-cell battery casing uses a copper grid as the base layer, and the second layer is a composite resin. The copper grid is fixed by the composite curing process, and together with the carbon fiber in the second layer, they achieve the electromagnetic shielding effect. However, the copper grid is subject to stress during the composite curing process, which can cause wrinkles and breakage points, thus reducing the electromagnetic shielding effect. Similarly, the carbon fiber in the composite, being a woven fabric, naturally has porosity, and wrinkles and breakage points can also occur during the layering process, further reducing the electromagnetic shielding effect. Therefore, this solution will further reduce the electromagnetic shielding effect when applied to larger assembly casings, failing to achieve satisfactory results. Summary of the Invention
[0009] This application provides a fuel cell housing, a manufacturing method, and a fuel cell, which can meet the requirements of heat resistance, insulation, mechanical strength, and electromagnetic shielding of the assembly housing.
[0010] In one aspect, a fuel cell housing is provided, comprising a tape layer, a first layer, a second layer and a third layer arranged sequentially.
[0011] The tape layer includes conductive tape;
[0012] The first and third layers are made of insulating prepreg;
[0013] The second layer includes energy-absorbing foam.
[0014] In some embodiments, the conductive tape includes a base tape and a reinforcing tape disposed on the base tape.
[0015] In some embodiments, the base tape is aluminum foil tape;
[0016] And / or, the reinforcing tape is made of graphite tape.
[0017] In some embodiments, the peel strength of the graphite tape is ≥5 N / cm;
[0018] And / or, the graphite type in the graphite tape is flake graphite, with a carbon content ≥94%.
[0019] In some embodiments, the insulating prepreg used in the first layer and the insulating prepreg used in the third layer may be the same or different.
[0020] In some embodiments, the insulating prepreg of the first layer comprises, by weight, 40-60 parts epoxy resin, 20-30 parts continuous glass fiber, and 20-30 parts continuous basalt fiber.
[0021] In some embodiments, the continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method.
[0022] In some embodiments, the insulating prepreg of the third layer comprises, by weight, 40-60 parts of phenolic resin, 20-30 parts of continuous alumina fiber, and 20-30 parts of continuous quartz fiber.
[0023] In some embodiments, the continuous alumina fibers and continuous quartz fibers are orthogonally woven into a preform using a mixed weaving method.
[0024] In some embodiments, the preform includes two types: 0° / 90° and -45° / 45°.
[0025] In some embodiments, the ratio of 0° / 90° preforms to -45° / 45° preforms is 1:1.
[0026] In some embodiments, the energy-absorbing foam is PET foam or PMI foam.
[0027] In some embodiments, the thickness of the energy-absorbing foam is 5 mm to 10 mm;
[0028] And / or, the compressive modulus of the energy-absorbing foam is ≥50MPa.
[0029] In a second aspect, a method for preparing a fuel cell housing as described in any of the above-mentioned methods is provided, comprising:
[0030] The insulating prepreg is processed to form a preform, the preform comprising a first layer of preform and a third layer of preform;
[0031] The first layer of preform, the energy-absorbing foam, and the third layer of preform are molded to obtain an intermediate.
[0032] The outer surface of the intermediate body is coated with conductive tape to obtain the fuel cell housing.
[0033] In some embodiments, the molding temperature is 50°C to 120°C, the pressure is 20 to 30 bar, and the time is 2 to 3 minutes.
[0034] In some embodiments, coating the outer surface of the intermediate body with conductive tape includes the following steps:
[0035] Apply base tape to the outer surface of the intermediate body so that the entire outer surface of the intermediate body is covered by base tape;
[0036] On the base tape, reinforcing tape is applied to the irregular areas on the outer surface of the intermediate body so that the entire surface of the irregular areas is covered by reinforcing tape.
[0037] In some embodiments, the insulating prepreg is processed to form a preform, including the following steps:
[0038] The insulating prepreg is placed on the roll roller, aligned, spread and stacked, and then cut into stacked blocks. The stacked blocks are then locally heated to connect the layers of material into a grippable whole structure.
[0039] The entire structure is grasped, heated on a preheating platform, then placed in a preforming mold for mold closing and cold pressing preforming. Finally, the excess edges are trimmed on the preforming fixture to obtain the preformed body.
[0040] Thirdly, a fuel cell is provided, which includes a fuel cell housing as described in any of the above.
[0041] The beneficial effects of the technical solution provided in this application include:
[0042] This application provides a fuel cell housing, a fabrication method, and a fuel cell. The tape layer includes conductive tape, which is located on the outermost layer. This ensures that the overall component meets electromagnetic shielding requirements. For irregular areas with special structures, such as grooves or holes, the amount of conductive tape applied can be increased to ensure that there are no weak areas in the electromagnetic shielding. Furthermore, the component can be repaired promptly after being bumped or damaged, resulting in low cost and convenient operation. Compared to copper grids, it does not need to be molded together with the composite substrate composed of the first, second, and third layers, reducing wrinkles and breaks and mitigating their impact on the electromagnetic shielding effect. Compared to conductive coatings, it eliminates the need for pretreatment of the composite substrate. Moreover, conductive coatings may be damaged by flying debris during use, leading to regional electromagnetic shielding failure. The conductive tape effectively solves this problem; even if damaged by flying debris, the damaged area can be repaired promptly to restore the electromagnetic shielding function.
[0043] The second layer includes energy-absorbing foam, which has high rigidity. The first and third layers are made of insulating prepreg, which has insulation, heat resistance, and high mechanical properties. The first, second, and third layers form a sandwich-like three-layer structure. All three layers can provide high strength and high modulus, and are all heat-resistant materials, which can effectively improve the overall heat resistance and strength of the composite matrix, reduce the degree of deformation under extreme high temperature environments, or the degree of vibration failure in actual use. At the same time, the overall insulation thickness includes the full thickness of the three layers, without wasting the thickness of the first, second, and third layers. This results in high insulation strength of the fuel cell shell, which can reach insulation resistance >10TΩ and breakdown voltage >100kV, far exceeding the breakdown voltage of air. Because the insulation performance of the shell is high, higher than that of air, it is not necessary to increase the design gap between the internal battery and the shell to block the passage between the battery and the outside of the shell through air. In other words, this application uses the above-mentioned sandwich-like three-layer structure to replace the role of air, thereby reducing the design gap between the shell and the battery and increasing the design freedom of the battery structure. Attached Figure Description
[0044] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0045] Figure 1 This is a schematic diagram of the fuel cell housing provided in an embodiment of this application.
[0046] In the diagram: 1. Adhesive tape layer; 2. First layer; 3. Second layer; 4. Third layer. Detailed Implementation
[0047] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0048] See Figure 1As shown in the illustration, this application provides a fuel cell housing comprising, from the outside in, a tape layer 1, a first layer 2, a second layer 3, and a third layer 4. The tape layer includes conductive tape, which is located on the outermost layer. This ensures the overall electromagnetic shielding requirements are met. For irregular areas with special structures, such as grooves or holes, the amount of conductive tape applied can be increased to ensure no weak points in the electromagnetic shielding. Furthermore, the tape can be promptly repaired after impacts, resulting in low cost and convenient operation. Compared to copper grids, it does not need to be molded together with the composite substrate formed by the first layer 2, second layer 3, and third layer 4, reducing wrinkles and breaks and mitigating their impact on the electromagnetic shielding effect. Moreover, compared to conductive coatings, no pretreatment of the composite substrate is required. Additionally, conductive coatings may be damaged by flying debris during use, leading to regional electromagnetic shielding failure. Conductive tape effectively solves this problem; even if damaged by flying debris, the damaged area can be promptly repaired to restore the electromagnetic shielding function.
[0049] The second layer 3 includes energy-absorbing foam, which has high rigidity. The first layer 2 and the third layer 4 are made of insulating prepreg, which has insulation, heat resistance, and high mechanical properties. The first layer 2, the second layer 3, and the third layer 4 form a sandwich-like three-layer structure. All three layers can provide high strength and high modulus, and are all heat-resistant materials, which can effectively improve the overall heat resistance and strength of the composite matrix, reduce the degree of deformation under extreme high temperature environments or vibration failure in actual use. At the same time, the overall insulation thickness includes the full thickness of the three layers, without wasting the thickness of the first layer 2, the second layer 3, and the third layer 4. This results in high insulation strength of the fuel cell shell, which can reach insulation resistance >10TΩ and breakdown voltage >100kV, far exceeding the breakdown voltage of air. Since the insulation performance of the shell is high, higher than that of air, it is not necessary to increase the design gap between the internal battery and the shell to block the formation of a passage between the battery and the outside of the shell through air. In other words, this application uses the above-mentioned sandwich-like three-layer structure to replace the role of air, thereby reducing the design gap between the shell and the battery and increasing the design freedom of the battery structure.
[0050] Since the first layer 2, the second layer 3, and the third layer 4 form a sandwich-like three-layer structure, when used in the assembly housing structure, the surfaces of these three layers are not all regular. Therefore, the conductive tape includes a base tape and a reinforcing tape disposed on the base tape. Specifically, the base tape is applied to the surface of the first layer 2, ensuring that the entire surface of the first layer 2 is covered without exposure. The specific number of base tape layers is determined according to actual needs; for example, at least one layer of base tape is applied. Then, reinforcing tape is applied to irregular areas such as grooves and hole connection edges, ensuring that the irregular areas are completely covered and reinforced by reinforcing tape. The specific number of reinforcing tape layers is determined according to actual needs; for example, at least two layers of reinforcing tape are applied.
[0051] The aforementioned base tape has several options. For example, as an example, the base tape can be aluminum foil tape or graphite tape. Aluminum foil tape is prone to tearing when pasted on irregular areas, such as when bent and pressed. Graphite tape is softer and less prone to tearing, so it can reinforce areas where aluminum foil tape is easily torn. Moreover, aluminum foil tape is effective but expensive, while graphite tape is less effective but cheaper, so both can be used in combination.
[0052] Similarly, the reinforcing tape has a variety of options; for example, the reinforcing tape can be graphite tape.
[0053] Furthermore, the peel strength of the graphite tape is ≥5N / cm; if the peel strength is too low, the adhesion will easily fail.
[0054] And / or, the graphite type in the graphite tape is flake graphite, with a carbon content ≥94%, as a low carbon content will weaken the conductivity.
[0055] Both the first layer 2 and the third layer 4 use insulating prepreg, which gives the fuel cell casing insulation, heat resistance and high mechanical properties. There are various options for the selection of insulating prepreg for these two layers.
[0056] For example, the insulating prepreg used in the first layer 2 is the same as the insulating prepreg used in the third layer 4.
[0057] For example, the insulating prepreg used in the first layer 2 and the insulating prepreg used in the third layer 4 are different.
[0058] Furthermore, by weight, the insulating prepreg of the first layer 2 comprises: 40-60 parts epoxy resin, 20-30 parts continuous glass fiber, and 20-30 parts continuous basalt fiber. Composites prepared with epoxy resin typically achieve an elongation at break of over 2%, which is considered relatively "tough," effectively resisting external impacts (such as gravel) when used as the outer layer of a battery casing.
[0059] The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform is impregnated with epoxy resin, stored at low temperature, and then cut and laid out before use.
[0060] The preform includes two types: 0° / 90° and -45° / 45°.
[0061] Preferably, the ratio of 0° / 90° preforms to -45° / 45° preforms is 1:1 to avoid excessive or insufficient strength in one direction, which could lead to shear failure.
[0062] In other words, to avoid excessive or insufficient strength in a certain direction, which would cause shear failure, the insulating prepreg of the first layer 2 includes two types of preforms with different layup directions: 0° / 90° and -45° / 45°. In use, the amount of 0° / 90° preforms and -45° / 45° preforms used is equal. The preforms with the two layup directions are impregnated with epoxy resin and then stacked together for cutting.
[0063] Furthermore, based on parts by weight, the insulating prepreg of the third layer 4 comprises: 40-60 parts phenolic resin, 20-30 parts continuous alumina fiber, and 20-30 parts continuous quartz fiber. Composites prepared with phenolic resin tend to have relatively high strength, but their elongation at break is typically less than 2%, making them relatively brittle. Furthermore, the inner layer uses continuous quartz fiber for better insulation and continuous alumina fiber for better heat resistance, thus improving the safety of the internal battery.
[0064] The continuous alumina fibers and continuous quartz fibers are orthogonally woven into a preform using a mixed weaving method. The preform is impregnated with phenolic resin, stored at low temperature, and then cut and laid out before use.
[0065] The preform includes two types: 0° / 90° and -45° / 45°.
[0066] Preferably, the ratio of 0° / 90° preforms to -45° / 45° preforms is 1:1 to avoid excessive or insufficient strength in one direction, which could lead to shear failure.
[0067] In other words, to avoid excessive or insufficient strength in a certain direction, which would cause shear failure, the insulating prepreg of the third layer 4 includes two types of preforms with different layup directions: 0° / 90° and -45° / 45°. In use, the amount of 0° / 90° preforms and -45° / 45° preforms used is equal. The preforms with the two layup directions are impregnated with epoxy resin and then stacked together for cutting.
[0068] The energy-absorbing foam mentioned above is made of PET (polyethylene terephthalate) foam or PMI (polymethacrylamide) foam.
[0069] The thickness of the energy-absorbing foam is 5mm to 10mm; the compression modulus of the energy-absorbing foam is ≥50MPa.
[0070] This application also provides a method for preparing a fuel cell housing, which includes the following steps:
[0071] 101: Processing the insulating prepreg to form a preform, the preform comprising a first layer 2 and a third layer 4.
[0072] Specifically, the processing of the insulating prepreg to form the preform of the first layer 2 includes the following steps:
[0073] 201: Place the first layer 2 of insulating prepreg on the roll roller, align, spread and stack it, then cut it into stacked blocks, and then use local heating to connect the layers of material in the stacked blocks into a grippable whole structure for later use.
[0074] 202: Grab the overall structure, heat it on a preheating platform, then place it in a preforming mold for mold closing and cold pressing preforming, and then trim the excess edges on the preforming fixture to obtain the first layer 2 preform.
[0075] Processing the insulating prepreg to form the preform of the third layer 4 includes the following steps:
[0076] 301: Place the third layer 4 insulating prepreg on the roll roller, align, spread and stack it, then cut it into stacked blocks, and then use local heating to connect the layers of the stacked blocks into a grippable whole structure for later use.
[0077] 302: Grab the overall structure, heat it on the preheating platform, then place it in the preforming mold for mold closing and cold pressing preforming, and then trim the excess edges on the preforming fixture to obtain the preformed body of the third layer 4.
[0078] 102: The preform of the first layer 2, the energy-absorbing foam, and the preform of the third layer 4 are placed into the press mold in sequence, and the preform of the first layer 2, the energy-absorbing foam, and the preform of the third layer 4 are molded to obtain the intermediate body.
[0079] The molding temperature is 50℃~120℃, the pressure is 20~30 bar, and the time is 2~3 min.
[0080] After the intermediate has cooled, eject it and remove the intermediate.
[0081] 103: Coat the outer surface of the intermediate body with conductive tape to obtain the fuel cell housing.
[0082] The process of coating the outer surface of the intermediate body with conductive tape includes the following steps:
[0083] 401: Apply a base tape to the outer surface of the intermediate body, at least one layer, so that the outer surface of the intermediate body is completely covered by the base tape and no part is exposed.
[0084] 402: On the base tape, apply reinforcing tape to irregular areas such as grooves and hole connection edges on the outer surface of the intermediate body, applying at least two layers to ensure that the entire surface of the irregular area is covered by reinforcing tape.
[0085] This application also provides a fuel cell, which includes the fuel cell housing provided in the above embodiments.
[0086] The present application will be described in detail below through examples and comparative examples.
[0087] Example 1
[0088] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0089] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There are two layers of aluminum foil tape and three layers of graphite tape.
[0090] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 40 parts epoxy resin, 20 parts continuous glass fiber, and 20 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with a 1:1 ratio of 0° / 90° preform to -45° / 45° preform.
[0091] The second layer 3 includes energy-absorbing foam, which is made of PET foam and has a thickness of 5 mm.
[0092] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 60 parts phenolic resin, 20 parts continuous alumina fiber, and 20 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0093] Example 2
[0094] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0095] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There are two layers of aluminum foil tape and three layers of graphite tape.
[0096] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 50 parts epoxy resin, 25 parts continuous glass fiber, and 25 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with a 1:1 ratio of 0° / 90° preform to -45° / 45° preform.
[0097] The second layer 3 includes energy-absorbing foam, which is made of PET foam and has a thickness of 8 mm.
[0098] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 50 parts phenolic resin, 25 parts continuous alumina fiber, and 25 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0099] Example 3
[0100] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0101] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There are two layers of aluminum foil tape and three layers of graphite tape.
[0102] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 60 parts epoxy resin, 30 parts continuous glass fiber, and 30 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0103] The second layer 3 includes energy-absorbing foam, which is made of PET foam and has a thickness of 10 mm.
[0104] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 40 parts phenolic resin, 30 parts continuous alumina fiber, and 30 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0105] Example 4
[0106] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0107] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There are two layers of aluminum foil tape and two layers of graphite tape.
[0108] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 50 parts epoxy resin, 20 parts continuous glass fiber, and 20 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0109] The second layer 3 includes energy-absorbing foam, which is made of PET foam and the thickness of the PMI foam is 5 mm.
[0110] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 50 parts phenolic resin, 20 parts continuous alumina fiber, and 20 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with a 1:1 ratio of 0° / 90° preform to -45° / 45° preform.
[0111] Example 5
[0112] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0113] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There are two layers of aluminum foil tape and two layers of graphite tape.
[0114] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 50 parts epoxy resin, 30 parts continuous glass fiber, and 30 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0115] The second layer 3 includes energy-absorbing foam, which is made of PET foam and has a thickness of 8 mm.
[0116] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 50 parts phenolic resin, 30 parts continuous alumina fiber, and 30 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0117] Example 6
[0118] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0119] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There are two layers of aluminum foil tape and two layers of graphite tape.
[0120] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 50 parts epoxy resin, 25 parts continuous glass fiber, and 25 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with a 1:1 ratio of 0° / 90° preform to -45° / 45° preform.
[0121] The second layer 3 includes energy-absorbing foam, which is made of PET foam and the thickness of the PMI foam is 10 mm.
[0122] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 50 parts phenolic resin, 25 parts continuous alumina fiber, and 25 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0123] Example 7
[0124] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0125] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There is one layer of aluminum foil tape and three layers of graphite tape.
[0126] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 40 parts epoxy resin, 20 parts continuous glass fiber, and 20 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with a 1:1 ratio of 0° / 90° preform to -45° / 45° preform.
[0127] The second layer 3 includes energy-absorbing foam, which is made of PET foam and has a thickness of 5 mm.
[0128] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 60 parts phenolic resin, 20 parts continuous alumina fiber, and 20 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0129] Example 8
[0130] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0131] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There is one layer of aluminum foil tape and three layers of graphite tape.
[0132] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 50 parts epoxy resin, 25 parts continuous glass fiber, and 25 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with a 1:1 ratio of 0° / 90° preform to -45° / 45° preform.
[0133] The second layer 3 includes energy-absorbing foam, which is made of PET foam and has a thickness of 8 mm.
[0134] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 50 parts phenolic resin, 25 parts continuous alumina fiber, and 25 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0135] Example 9
[0136] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0137] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There is one layer of aluminum foil tape and three layers of graphite tape.
[0138] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 60 parts epoxy resin, 30 parts continuous glass fiber, and 30 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0139] The second layer 3 includes energy-absorbing foam, which is made of PET foam and has a thickness of 10 mm.
[0140] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 40 parts phenolic resin, 30 parts continuous alumina fiber, and 30 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0141] Example 10
[0142] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0143] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There is one layer of aluminum foil tape and two layers of graphite tape.
[0144] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 50 parts epoxy resin, 20 parts continuous glass fiber, and 20 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0145] The second layer 3 includes energy-absorbing foam, which is made of PET foam and the thickness of the PMI foam is 5 mm.
[0146] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 50 parts phenolic resin, 20 parts continuous alumina fiber, and 20 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with a 1:1 ratio of 0° / 90° preform to -45° / 45° preform.
[0147] Example 11
[0148] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0149] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There is one layer of aluminum foil tape and two layers of graphite tape.
[0150] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 50 parts epoxy resin, 30 parts continuous glass fiber, and 30 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0151] The second layer 3 includes energy-absorbing foam, which is made of PET foam and has a thickness of 8 mm.
[0152] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 50 parts phenolic resin, 30 parts continuous alumina fiber, and 30 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0153] Example 12
[0154] A fuel cell housing includes a tape layer 1, a first layer 2, a second layer 3, and a third layer 4 arranged sequentially from the outside to the inside.
[0155] The tape layer 1 includes conductive tape, which includes aluminum foil tape and graphite tape. The aluminum foil tape is pasted on the first layer 2, and the graphite tape is pasted on the aluminum foil tape. There is one layer of aluminum foil tape and two layers of graphite tape.
[0156] The first layer 2 uses an insulating prepreg, which, by weight, comprises: 50 parts epoxy resin, 25 parts continuous glass fiber, and 25 parts continuous basalt fiber. The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with a 1:1 ratio of 0° / 90° preform to -45° / 45° preform.
[0157] The second layer 3 includes energy-absorbing foam, which is made of PET foam and the thickness of the PMI foam is 10 mm.
[0158] The third layer 4 uses an insulating prepreg, which, by weight, comprises: 50 parts phenolic resin, 25 parts continuous alumina fiber, and 25 parts continuous quartz fiber. The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method. The preform includes two types: 0° / 90° and -45° / 45°, with the ratio of 0° / 90° preform to -45° / 45° preform being 1:1.
[0159] Table 1
[0160]
[0161] Comparative Example 1
[0162] The fuel cell stack assembly housing is made of aluminum alloy.
[0163] Comparative Example 2
[0164] The fuel cell stack assembly housing is made of carbon fiber composite material, with a copper grid embedded in the outer layer of the housing and a conductive coating on the outside.
[0165] Example of effect
[0166] Composite fuel cell assembly shells were prepared using the formulations of Examples 1-12. The mechanical properties, electrical properties, and flame retardant properties of the shells were tested, and the results were compared with those of Comparative Examples 1 and 2. The test results are shown in Table 2 below.
[0167] Table 2
[0168]
[0169] As can be seen from the test results in Table 2, compared with commonly used aluminum alloy materials or carbon fiber composite materials, the composite material of this application performs well in terms of mechanical properties, electrical properties, and thermal runaway. This application can significantly improve heat resistance and insulation while ensuring strength and electromagnetic shielding performance.
[0170] In summary, the fuel cell housing provided in this application includes a conductive tape layer on the outermost layer. This ensures that the entire component meets electromagnetic shielding requirements. For irregular areas with special structures, such as grooves or holes, the amount of conductive tape applied can be increased to ensure that there are no weak points in the electromagnetic shielding. Furthermore, the component can be repaired promptly after impacts, resulting in low cost and convenient operation. Compared to copper grids, it does not need to be molded together with the composite substrate composed of the first, second, and third layers, reducing wrinkles and breaks and mitigating their impact on the electromagnetic shielding effect. Moreover, compared to conductive coatings, no pretreatment of the composite substrate is required. Additionally, conductive coatings may be damaged by flying debris during use, leading to regional electromagnetic shielding failure. The conductive tape effectively solves this problem; even if damaged by flying debris, the damaged area can be repaired promptly to restore the electromagnetic shielding function.
[0171] The second layer includes energy-absorbing foam, which has high rigidity. The first and third layers are made of insulating prepreg, which has insulation, heat resistance, and high mechanical properties. The first, second, and third layers form a sandwich-like three-layer structure. All three layers can provide high strength and high modulus, and are all heat-resistant materials, which can effectively improve the overall heat resistance and strength of the composite matrix, reduce the degree of deformation under extreme high temperature environments, or the degree of vibration failure in actual use. At the same time, the overall insulation thickness includes the full thickness of the three layers, without wasting the thickness of the first, second, and third layers. This results in high insulation strength of the fuel cell shell, which can reach insulation resistance >10TΩ and breakdown voltage >100kV, far exceeding the breakdown voltage of air. Because the insulation performance of the shell is high, higher than that of air, it is not necessary to increase the design gap between the internal battery and the shell to block the passage between the battery and the outside of the shell through air. In other words, this application uses the above-mentioned sandwich-like three-layer structure to replace the role of air, thereby reducing the design gap between the shell and the battery and increasing the design freedom of the battery structure.
[0172] In the description of this application, it should be noted that the terms "upper," "lower," etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application. Unless otherwise expressly specified and limited, the terms "installed," "connected," and "linked" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication between two elements. For those skilled in the art, the specific meaning of the above terms in this application can be understood according to the specific circumstances.
[0173] It should be noted that in this application, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0174] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A fuel cell housing, characterized in that, It includes, from the outside to the inside, a tape layer (1), a first layer (2), a second layer (3) and a third layer (4); The tape layer (1) includes a conductive tape, which is composed of a base tape and a reinforcing tape. The base tape is fully covered on the outer surface of the first layer (2), and the reinforcing tape is attached to the irregular area of the first layer (2) corresponding to the base tape. The base tape is made of aluminum foil tape, and the reinforcing tape is made of graphite tape. The peel strength of the graphite tape is ≥5N / cm. The graphite type in the graphite tape is flake graphite, and the carbon content is ≥94%. The first layer (2) and the third layer (4) are made of insulating prepreg; The second layer (3) includes energy-absorbing foam.
2. The fuel cell housing as described in claim 1, characterized in that: The insulating prepreg used in the first layer (2) may be the same as or different from the insulating prepreg used in the third layer (4).
3. The fuel cell housing as described in claim 1, characterized in that: The insulating prepreg of the first layer (2) comprises, by weight, 40-60 parts of epoxy resin, 20-30 parts of continuous glass fiber and 20-30 parts of continuous basalt fiber.
4. The fuel cell housing as described in claim 3, characterized in that: The continuous glass fiber and continuous basalt fiber are orthogonally woven into a preform using a mixed weaving method.
5. The fuel cell housing as described in claim 1, characterized in that: The insulating prepreg of the third layer (4) comprises, by weight, 40-60 parts of phenolic resin, 20-30 parts of continuous alumina fiber and 20-30 parts of continuous quartz fiber.
6. The fuel cell housing as described in claim 5, characterized in that: The continuous alumina fiber and continuous quartz fiber are orthogonally woven into a preform using a mixed weaving method.
7. The fuel cell housing as described in claim 4 or 6, characterized in that: The preform includes two types: 0° / 90° and -45° / 45°.
8. The fuel cell housing as described in claim 7, characterized in that: The ratio of 0° / 90° preforms to -45° / 45° preforms used is 1:
1.
9. The fuel cell housing as described in claim 1, characterized in that: The energy-absorbing foam is made of PET foam or PMI foam.
10. The fuel cell housing as claimed in claim 1, characterized in that: The thickness of the energy-absorbing foam is 5mm~10mm; And / or, the compressive modulus of the energy-absorbing foam is ≥50MPa.
11. A method for preparing a fuel cell housing as described in any one of claims 1 to 10, characterized in that, It includes: The insulating prepreg is processed to form a preform, the preform comprising a first layer (2) and a third layer (4); The preform of the first layer (2), the energy-absorbing foam and the preform of the third layer (4) are molded to obtain an intermediate body; The outer surface of the intermediate body is coated with conductive tape to obtain the fuel cell housing.
12. The method for preparing a fuel cell housing as described in claim 11, characterized in that, The molding temperature is 50℃~120℃, the pressure is 20~30 bar, and the time is 2~3 min.
13. The method for preparing a fuel cell housing as described in claim 11, characterized in that, The process of coating the outer surface of the intermediate body with conductive tape includes the following steps: Apply base tape to the outer surface of the intermediate body so that the entire outer surface of the intermediate body is covered by base tape; On the base tape, reinforcing tape is applied to the irregular areas on the outer surface of the intermediate body so that the entire surface of the irregular areas is covered by reinforcing tape.
14. The method for preparing a fuel cell housing as described in claim 11, characterized in that, Processing the insulating prepreg to form a preform includes the following steps: The insulating prepreg is placed on the roll roller, aligned, spread and stacked, and then cut into stacked blocks. The stacked blocks are then locally heated to connect the layers of material into a grippable whole structure. The entire structure is grasped, heated on a preheating platform, then placed in a preforming mold for mold closing and cold pressing preforming. Finally, the excess edges are trimmed on the preforming fixture to obtain the preformed body.
15. A fuel cell, characterized in that, It includes the fuel cell housing as described in any one of claims 1 to 10.
Citation Information
Patent Citations
Electromagnetic shielding heat-dissipation film and manufacturing method thereof
CN104981138A
Fuel cell housing
CN106104893A
Mass production method of automobile composite material battery box sandwich structure
CN111907088A