Methods of creating environmental barriers
Through DLI-MOCVD technology, environmental barrier coatings for rare earth silicates and zirconia are formed on CMC materials, solving the problem of corrosion sensitivity of ceramic matrix composite materials at high temperatures, and achieving higher oxidation and corrosion resistance , extends service life.
Patent Information
- Application Number
- CN202180065172.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-29
- Filing Date
- 2021-09-20
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-09-20
AI Technical Summary
In oxidation and high-temperature corrosion environments, ceramic matrix composites (CMC materials) are sensitive to corrosion, especially under operating conditions of aviation turbines, the existing environmental barrier coatings still have insufficient protection at high temperatures.
Direct liquid injection-metal organic chemical vapor deposition (DLI-MOCVD) technology is used to form an environmental barrier coating on CMC materials, and through rare earth silicates, zirconia and other materials, it forms a denser, more oxidative and high-temperature corrosion resistant The barrier reduces residual pores and micro-cracks, and improves composition and microstructure control.
The obtained environmental barrier coating has higher density and chemical resistance, reduces internal stress, improves resistance to high temperatures and oxidation, extends the service life of CMC materials, and maintains good results during thin layer deposition. Thermal expansion compatibility.
Smart Images

Figure CN116234784B_ABST
Abstract
Description
Technical Field
[0001] One particular field of application of the invention is the protection of at least parts of ceramic matrix composites ("CMC materials") forming hot parts of gas turbines, such as combustion chamber walls or turbine shrouds, turbine distributors or turbine blades for aircraft engines or industrial turbines. Background Art
[0002] Increasing efficiency and reducing polluting emissions lead to taking higher and higher temperatures in the combustion chamber into account.
[0003] Therefore, it has been proposed to replace metallic materials with CMC materials, in particular for the walls of combustion chambers or turbine shrouds. In fact, it is well known that CMC materials have both good mechanical properties, enabling them to be used in structural elements, and the ability to maintain these properties at high temperatures. CMC materials may include a fiber reinforcement made of refractory fibers (usually carbon or ceramic), which is densified by a ceramic matrix (for example silicon carbide).
[0004] Under the operating conditions of aircraft turbines, that is to say at high temperatures in an oxidizing and humid environment, CMC materials are very sensitive to corrosion phenomena. The reason for CMC corrosion is the oxidation of silicon carbide to silicon dioxide, which, under the action of water vapor, volatilizes in the form of silicon hydroxide Si(OH)4. Corrosion phenomena lead to the degradation of the CMC and affect its service life. In order to limit this degradation during operation, it has been considered to form an environmental barrier ("environmental barrier coating"; "EBC") on the surface of the CMC material. The environmental barrier can include a silicon tie coating and a rare earth silicate coating located on the tie coating. The tie coating can, on the one hand, improve the adhesion of the rare earth silicate coating and, on the other hand, form a protective silicon dioxide coating, the low permeability of which to oxygen helps to protect the CMC from oxidation. The rare earth silicate coating in turn can limit the diffusion of water vapor into the silicon dioxide coating formed by the oxidation of silicon, thereby limiting the degradation of said silicon dioxide coating. The environmental barrier can be deposited by thermal spraying. In particular, US2019040761 is known, which describes an EBC formed by this method.
[0005] However, there is still a need to further improve the protection of CMC materials in oxidative and high temperature corrosive environments, especially in environments greater than or equal to 800°C. Summary of the invention
[0006] The present invention relates to a method for producing a component with improved oxidation and high temperature corrosion resistance, comprising forming an environmental barrier coating on at least a portion of a ceramic matrix composite material, wherein the environmental barrier coating is formed by direct liquid injection-metal organic chemical vapor deposition.
[0007] The present invention is based on the use of a special deposition technology, namely direct liquid injection-metal organic chemical vapor deposition ("DLI-MOCVD"), which uses one or more molecular precursors to form an environmental barrier on the CMC material. Hereinafter, for the sake of brevity, this technology will be referred to as the "DLI-MOCVD technology".
[0008] DLI-MOCVD technology is used in the semiconductor field, but to the best of the inventors' knowledge, has not been used to develop environmental barriers to protect CMC materials.
[0009] The environmental barrier obtained by the DLI-MOCVD technology has fewer residual pores and microcracks, as well as better composition and microstructural control than the environmental barrier obtained by thermal spraying. In this way, the environmental barrier obtained in the context of the present invention is more impermeable (less pores) and has less internal stress related to the expansion difference between the desired barrier compound and the undesirable compound during operation (better control of composition). Compared with traditional chemical vapor deposition CVD, the use of DLI-MOCVD technology also allows better control of the composition of the deposit obtained, in particular by adjusting the amount of various precursors to adjust the composition of the deposit (if necessary). It is also possible to deposit a pure phase like thermal spraying, rather than a mixed phase of the rare earth disilicate / rare earth monosilicate type. Having a more effective environmental barrier, especially less porosity, can reduce its thickness, which promotes the compatibility of the thermal expansion coefficients between the environmental barrier and the underlying material. The production of deposits of reduced thickness is also particularly advantageous for certain components in which, despite the presence of a protective deposit, it is desirable to maintain a very thin thickness at least locally, for example in the case of the trailing edge of a blade, and for the production of fine multi-layer deposits (e.g., about 10 μm per layer), which are easily achieved by thermal spraying. In addition, the present invention has the advantage of allowing the satisfactory use of precursors in liquid or solid form, the evaporation and entrainment of which in the gaseous state may be difficult to achieve or difficult to control within the framework of conventional chemical vapor deposition (CVD) methods. The DLI-MOCVD technology also allows the use of metal chloride precursors to be omitted, which are usually generated in situ in the gaseous state in conventional CVD methods, such generation being relatively complex with respect to control and flow management and possibly producing hydrochloric acid as a reaction by-product, which is corrosive and may degrade the deposition facility.
[0010] The environmental barrier coating obtained within the scope of the present invention may have any composition. Thus, the environmental barrier coating may comprise at least one rare earth silicate, zirconium oxide stabilized with rare earth oxides or mullite (3Al2O3.2SiO2).
[0011] In an exemplary embodiment, the environmental barrier coating includes a rare earth silicate and is formed from at least an alkoxysilane silicon oxide precursor and a rare earth β-diketone rare earth oxide precursor in the presence of an oxygen supply source. In particular, the silicon oxide precursor can be di-tert-butoxy diacetoxy silane and a rare earth oxide precursor RE (thd) 3, wherein RE represents a rare earth element and the group (thd) represents 2,2,6,6-tetramethyl-3,5-heptanedioate, and the rare earth oxide precursor is, for example, Y (thd) 3 (CAS n ° 15632-39-0).
[0012] The combination of these precursors is advantageous because RE(thd)3 is readily commercially available, relatively simple to use and thermally stable, which allows deposition at high temperatures and thus high growth rates, and the decomposition temperature of di-tert-butyldiacetoxysilane is very close to that of RE(thd)3. The two precursors are also miscible, which allows them to be dissolved in the same solvent for use if desired.
[0013] The oxygen supply source may include at least one of the following gases: O2, N2O, H2O, CO2, O3.
[0014] In exemplary embodiments, the nature and / or relative proportions of the molecular precursors are altered during formation of the environmental barrier coating to impart it with a varying composition.
[0015] The DLI-MOCVD technique allows fine and continuous tuning of the composition of the environmental barrier coating during the deposition process to improve its properties. It should be noted that it is also possible to deposit several consecutive environmental barrier coatings with well-defined and different compositions.
[0016] In particular, forming the environmental barrier coating may include forming at least a first portion comprising a rare earth disilicate, and forming a second portion comprising a rare earth monosilicate over the first portion.
[0017] The fact that the monosilicates are positioned on the outside of the environmental barrier can further increase the resistance of the environmental barrier to decay, since rare earth monosilicates are less sensitive to this phenomenon than rare earth disilicates.
[0018] Alternatively, forming the environmental barrier coating includes forming at least a first portion comprising a rare earth monosilicate, and forming a second portion comprising a rare earth disilicate on the first portion.
[0019] Alternatively or in combination, forming the environmental barrier coating includes at least forming a first portion comprising a first rare earth silicate, and forming a second portion comprising a second rare earth silicate different from the first rare earth, the first and second portions superimposing.
[0020] Changing the properties of the rare earths along the environmental barrier can improve its chemical resistance. For example, the first part can contain ytterbium disilicate, or yttrium disilicate and ytterbium disilicate, while the second part can contain yttrium monosilicate or lutetium disilicate. Thus, the first part provides improved corrosion protection, while the second part provides improved resistance to calcium aluminum silicate and magnesium aluminum silicate (CMAS).
[0021] In an exemplary embodiment, the environmental barrier coating has a thickness less than or equal to 1000 μm, such as less than or equal to 700 μm.
[0022] The DLI-MOCVD technology allows reducing the thickness of the environmental barrier, as the latter has better characteristics.
[0023] The thickness of the environmental barrier coating may be greater than or equal to 200 μm, such as between 200 μm and 1000 μm, such as between 200 μm and 700 μm.
[0024] In an exemplary embodiment, the method includes depositing a bond coating comprising silicon on at least a portion of an outer surface of a ceramic matrix composite material, and depositing an environmental barrier coating on the bond coating. The bond coating may be deposited by chemical vapor deposition.
[0025] In an exemplary embodiment, the formed environmental barrier coating is also subjected to a thermal crystallization process.
[0026] Depending on the production temperature, the environmental barrier may be amorphous. This crystallization treatment can then crystallize the deposit and finely adjust the size of the grains.
[0027] The temperature applied during the crystallization heat treatment may be greater than or equal to 1250° C., for example 1350° C. This temperature may be less than or equal to 1400° C., for example if a silicon bonding coating is present, to avoid any risk of melting of the latter.
[0028] The invention also relates to a component produced by implementing the method as described above, which component is a turbine component. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A first example of a component having improved oxidation resistance and high temperature corrosion resistance that can be obtained by practicing the present invention is schematically illustrated.
[0030] Figure 2 A second example of a component having improved oxidation resistance and high temperature corrosion resistance that can be obtained by practicing the present invention is schematically illustrated. DETAILED DESCRIPTION
[0031] Figure 1An example of a component 1 comprising a CMC material 3 having an environmental barrier 2 obtainable by implementing the present invention is shown.
[0032] The CMC material 3 may comprise a fiber reinforcement, which may be made of carbon fibers (C) or ceramic fibers, such as silicon carbide fibers (SiC) or essentially made of SiC, including Si-CO or Si-CON fibers, that is to say also containing oxygen and possibly nitrogen. Such fibers are produced by the company Nippon Carbon under the name "Nicalon" or "Hi-Nicalon" or "Hi-Nicalon Type-S" or by the company Ube Industries under the name "Tyranno-ZMI". The ceramic fibers may be coated with a thin interfacial coating made of pyrolytic carbon (PyC), boron nitride (BN) or boron-doped carbon (BC, containing 5 to 20 at.% of B, supplemented by C).
[0033] The fiber reinforcement is densified by at least a portion of a ceramic (e.g., predominantly ceramic by volume) matrix. The ceramic matrix may include, for example, silicon carbide or a Si-BC ternary system. The matrix may be formed at least in part by CVI in a manner known per se. Alternatively, the matrix may be formed at least in part by a liquid process (impregnated with a precursor resin of the matrix and converted by crosslinking and pyrolysis, the process being repeatable) or by infiltration of silicon in a molten state (a "melt-infiltration" method). In the latter case, a powder is introduced into the optionally partially densified fiber reinforcement, which powder may be a powder of carbon, a ceramic (e.g., silicon carbide), or a mixture of these powders, and then infiltrated with a metal composition based on silicon in a molten state to form a SiC-Si type matrix. The fiber reinforcement may be woven or not woven, and when the fiber reinforcement is in the form of short fibers dispersed in the material 3, it does not depart from the scope of the invention. Alternatively, a particle reinforcement in the form of particles dispersed in the material 3 may be used.
[0034] The environmental barrier 2 may be formed on the entire outer surface S of the CMC material 3 or only on a portion of this surface S, for example when only a portion of the surface S needs to be protected. Figure 1 In the example shown, the environmental barrier 2 includes an environmental barrier coating 7 and a bond coating 5 present between the CMC material 3 and the coating 7. In the example shown, the bond coating 5 is in contact with the surface S of the composite material 3. Furthermore, in this example, the coating 7 is in contact with the bond coating 5.
[0035] The bond coating 5 may form in operation a protective silicon dioxide coating that is resistant to oxidation (a "TGO" coating known as "thermally grown oxide") in a manner known per se. The bond coating 5 may be made of silicon.
[0036] Coating 7 is an environmental barrier coating that provides protection against oxidation and high temperature corrosion by specifically limiting the diffusion of water vapor and oxygen to the bond coating 5 and the CMC material 3. Coating 7 may include rare earth silicates, such as rare earth monosilicates and / or rare earth disilicates, zirconia stabilized by rare earth oxides such as yttria, or mullite.
[0037] The coating 7 may include at least one rare earth element selected from yttrium Y, scandium Sc and lanthanide elements. Specifically, the rare earth element may be selected from yttrium Y and ytterbium Yb. It should be noted that if the coating 7 includes multiple rare earth elements, such as yttrium and ytterbium, it does not exceed the scope of the present invention.
[0038] The coating 7 may have an equiaxed microstructure, which improves mechanical strength and toughness. Alternatively, the coating 7 may have a columnar microstructure to improve resistance to thermal shock.
[0039] The coating 7 may have a thickness e1 greater than or equal to 50 μm, such as greater than or equal to 200 μm, such as greater than or equal to 250 μm. The thickness e1 may be between 50 μm and 1000 μm, such as between 200 μm and 1000 μm or between 250 μm and 1000 μm, such as between 200 μm and 700 μm or between 250 μm and 700 μm. The coating 7 forms a coating covering the outer surface S of the CMC material 3, and the thickness e1 is measured from the outer surface.
[0040] Details relating to the production of the environmental barrier will now be described.The paragraphs to be discussed now provide details relating to the formation of the bond coating 5.
[0041] The bond coating 5 may be formed by chemical vapor deposition from a precursor containing silicon, including, for example, silane, monochlorosilane, dichlorosilane and / or trichlorosilane. Two examples of forming the bond coating 5 by chemical vapor deposition are described below.
[0042] According to a first example, the temperature applied during the deposition of the bond coating 5 may be between 900° C. and 1150° C., for example between 1100° C. and 1150° C., and the pressure applied during the deposition may be between 15.3 kPa and 20 kPa, for example between 16.7 kPa and 18 kPa. During deposition, a precursor comprising silicon may be introduced into the reaction chamber in which the CMC material 3 is present, with a flow rate between 0.05 g / min and 0.3 g / min, for example between 0.1 g / min and 0.2 g / min. According to this first example, the bond coating 5 obtained has a crystalline microstructure. In particular, the bond coating 5 may be made of silicon, the bond coating 5 comprising, for example, columnar grains of crystalline silicon. Alternatively, the bond coating 5 may be made of a silicon alloy, for example a eutectic silicon alloy or a silicide.
[0043] According to a second example, the bonding coating 5 includes an amorphous silicon phase having crystalline silicon grains distributed inside, which grains may have an average size between 0.03 μm and 3 μm. The amorphous silicon phase may be formed of pure silicon or silicon dispersed with boron, oxygen and / or nitrogen. According to this second example, the bonding coating 5 may be formed at a deposition temperature that prevents crystallization of the deposited silicon, and then the bonding coating is heat treated at a treatment temperature higher than the temperature applied during deposition to form crystalline silicon grains distributed in the amorphous silicon phase. The temperature applied during deposition may be between 300°C and 700°C or between 700°C and 1000°C, and the pressure applied during deposition may be between 1.2 kPa and 1013 hPa. The operating conditions are selected according to the precursor used. The treatment temperature may be between 1000°C and 1400°C, for example, between 1200°C and 1350°C. During deposition, a precursor containing silicon may be introduced into the reaction chamber in which the CMC material 3 is present, with a flow rate between 0.1 g / min and 2 g / min.
[0044] When a method other than chemical vapor deposition is used to form the bond coating 5, it is within the scope of the present invention, for example, the bond coating 5 can alternatively be formed by thermal spraying from a powder or a powder mixture having a desired composition.
[0045] The description goes on to provide details regarding the production of the environmental barrier coating 7 .
[0046] In the DLI-MOCVD technique, the molecular precursors of the environmental barrier coating 7 to be obtained are present in liquid form in at least one tank, optionally dissolved in an organic solvent. Each molecular precursor can be present in a separate reservoir or, if the molecular precursors are miscible, the latter can be present in the same reservoir. Thus, the precursors can be dissolved in the same organic solvent (liquid) in the same tank. The solvent can be, for example, toluene or mesitylene.
[0047] In order to deposit the coating 7, the liquid molecular precursor is injected into the expansion chamber in the form of droplets, and the expansion chamber is heated to a certain temperature so that the precursor evaporates without causing their decomposition. For example, the expansion chamber described in the document US2009078791 can be used. The supply of liquid molecular precursor to the expansion chamber can be regulated by a liquid flow meter. A gas phase containing a mixture of gaseous molecular precursors is obtained in the expansion chamber by flash evaporation of the liquid precursor. The gas phase is entrained by a carrier gas (such as argon or nitrogen) to a reaction chamber in which the CMC material 3 is present. As described above, the CMC material 3 is heated to a temperature sufficient to allow the molecular precursor to decompose, optionally in the presence of an oxygen supply source. An environmental barrier coating 7 is formed on the CMC material 3. The reaction chamber can be a reactor with hot walls or cold walls. The latter case is conducive to the rapid formation of deposits on the CMC material 3 at high temperatures, rather than homogeneous reactions in the gas phase, while taking into account the degradation temperature of the precursor.
[0048] The composition of the coating 7 obtained depends on the molecular precursors used and their relative proportions introduced into the reaction chamber. A person skilled in the art knows how to select the molecular precursors to be implemented in the precursors known per se for the DLI-MOCVD technology to obtain the coating 7. The operating conditions for the deposition to be implemented are determined by a person skilled in the art based on experience and by known methods. For example, a person skilled in the art can perform multiple depositions by adjusting the flow rate of the molecular precursors, then characterize these depositions, and then, if necessary, improve the flow rate, temperature and pressure parameters to obtain the desired coating 7.
[0049] According to one example, the coating 7 may contain earth silicate and be formed from at least a silicon oxide molecular precursor and a rare earth oxide molecular precursor in the presence of an oxygen supply source as described above.
[0050] According to another example, the coating 7 may include mullite and be formed from at least a silicon oxide molecular precursor and an aluminum oxide molecular precursor in the presence of an oxygen supply source as described above.
[0051] Regardless of the example considered, the silicon oxide molecular precursor may be an alkoxysilane, such as tetraethyl orthosilicate (TEOS) or di-tert-butoxydiacetoxysilane (DADBS).
[0052] The aluminum oxide molecular precursor can be a complex of trimethylaluminum (TMA) and an oxygen supply source, or aluminum alkoxide (such as triisopropoxyaluminum, Al(OiPr)3), or β-diketonate aluminum (such as aluminum acetylacetonate, Al(acac)3).
[0053] According to another example, the coating 7 may include zirconium oxide stabilized by rare earth oxides (eg, yttria-zirconia) and formed from at least a zirconium oxide molecular precursor and a rare earth oxide molecular precursor in the presence of an oxygen supply source as described above.
[0054] The zirconium oxide precursor may be selected from: zirconium alkoxides or zirconium β-diketonate. As examples of usable zirconium alkoxides, tetra-tert-butoxy zirconium Zr(OtBu)4, tetra-butoxy zirconium Zr(OnBu)4 or tetra-propoxy zirconium Zr(OnPr)4 may be mentioned. As examples of usable β-diketonate zirconium, Zr(thd)4 may be mentioned.
[0055] Regardless of the example considered, the rare earth oxide molecular precursor can be selected from: rare earth alkoxides or rare earth β-diketones. As an example of a rare earth alkoxide that can be used, RE(mmp)3 can be mentioned, wherein RE represents a rare earth element and the (mmp) group represents 1-methoxy-2-methyl-2-propanolato. As an example of a rare earth β-diketone that can be used, RE(thd)3 can be mentioned, wherein RE represents a rare earth element.
[0056] As mentioned above, the molecular precursors are in the liquid state. If these precursors are in the solid state under standard temperature and pressure conditions (pressure of 1 bar and temperature of 20° C.), they can be dissolved in a solvent. For example, the rare earth oxide molecular precursor Y(thd)3 is available in solid form and can be dissolved in toluene or mesitylene or benzene. Other molecular precursors, such as alkoxysilanes, may already be in the liquid state under standard temperature and pressure conditions.
[0057] For example, the following operating conditions may be implemented during the formation of the environmental barrier coating 7:
[0058] - the temperature of the reaction chamber in which the CMC material 3 is present may be between 600° C. and 1200° C., such as between 800° C. and 1100° C., such as between 800° C. and 1000° C., and
[0059] The pressure in the reaction chamber may be less than or equal to 1000 mbar, such as less than or equal to 100 mbar, such as less than or equal to 20 mbar. The pressure in the reaction chamber may be between 0.3 mbar and 1000 mbar, such as between 2 mbar and 100 mbar, such as between 2 mbar and 20 mbar.
[0060] In the case where the coating 7 comprises a rare earth silicate, the ratio [the amount of silicon oxide molecular precursor material injected into the expansion chamber] / [the amount of rare earth oxide molecular precursor material injected into the expansion chamber] may be between 0.1 and 10, for example, between 0.2 and 5. The amount of material is measured in moles (mol). In addition, the ratio [the amount of material of the oxygen supply source implemented] / [the amount of material of the liquid precursor implemented] may be between 0.1 and 10, for example, between 0.5 and 5. In the case where the precursor is dissolved in a solvent, the amount of liquid precursor material corresponds to the amount of material of the liquid solvent containing the precursor.
[0061] Various details have just been described regarding the formation of an environmental barrier coating 7 by DLI-MOCVD techniques. Once the coating 7 is formed, it may be subjected to one or more post-treatments, which will now be described.
[0062] Therefore, the coating 7 can be decarburized to eliminate the residual carbon provided by the ligands of the molecular precursor. The decarburization process can be carried out under an oxidizing atmosphere, which can include molecular oxygen, carbon monoxide or nitrous oxide. The temperature applied during the decarburization process can be between 800°C and 1350°C, for example, between 900°C and 1100°C. The duration of the decarburization process can be between 30 minutes and 5 hours. If the duration is too long, a crystallization process can be started. Those skilled in the art will work in pairs (time, temperature), tending to increase the processing time when the temperature is low, and vice versa.
[0063] Alternatively or in combination, the coating 7 may undergo a crystallization heat treatment to reduce the proportion of amorphous phase present. The crystallization heat treatment may be carried out at a temperature greater than or equal to 1250° C., for example 1350° C., for example comprised between 1300° C. and 1350° C. The duration of the crystallization heat treatment may be greater than or equal to 5 hours, for example greater than or equal to 25 hours, for example 5 hours to 50 hours. For example, for a coating 7 of yttrium disilicate, the crystallization heat treatment may be carried out at a temperature of 1350° C. for at least 5 hours.
[0064] The component 1 thus produced may be a component for aviation or aerospace applications. The component 1 may be part of a hot part of a gas turbine or industrial turbine of an aviation or aerospace engine. The component 1 may be a component of a turbine engine. The component 1 may constitute at least a portion of a distributor, at least a portion of a nozzle, or a thermal protection coating, a wall of a combustion chamber, a sector of a turbine shroud, or a turbine engine blade.
[0065] Once obtained, component 1 is used in oxidizing and corrosive atmospheres at elevated temperatures greater than or equal to 800° C. In particular, it can be used at temperatures between 800° C. and 1500° C., or even between 800° C. and 1300° C. Component 1 can especially be used in humid air.
[0066] The example just described involves a component 1 having an environmental barrier coating 7 having a uniform composition. The environmental barrier coating may alternatively have a varying composition when the nature and / or relative proportions of the molecular precursors vary during the deposition process. A component 11 having an environmental barrier coating 17 of varying composition may be Figure 2As shown. The environmental barrier coating 17 includes two overlapping portions 17a and 17b having different compositions. The transition from portion 17a to portion 17b can be continuous. According to one example, portion 17a can include a rare earth disilicate and portion 17b can include a rare earth monosilicate. The rare earth element of the monosilicate can be the same as or different from the rare earth element of the disilicate. In the case where the monosilicate is superimposed on the disilicate, the disilicate can be yttrium disilicate and the monosilicate can be ytterbium monosilicate. Alternatively or in combination, portion 17a can include a silicate of a first rare earth and portion 17b can include a silicate of a second rare earth different from the first rare earth.
[0067] The properties of the CMC material 13 of the bonding coating 15 may be as follows: Figure 1 Just as described.
[0068] In addition, just combined Figure 1 and Figure 2 The example depicted has an environmental barrier coating 7 or 17 forming the outer surface of the coated component, the coating 7 or 17 being the coating furthest from the CMC material 3. However, the environmental barrier coating may be coated with additional coatings, such as thermal barriers, if this is not the case without departing from the scope of the invention.
[0069] Example
[0070] The inventors tested each solution separately by injection using an evaporator heated to 175° C. The reaction chamber was a cold-wall reactor in which there was a silicon substrate placed on a sample holder (“susceptor”) heated by a halogen lamp. The temperature applied was 680° C. and the pressure applied in the reaction chamber was 2.67 mbar.
[0071] The rare earth oxide precursor used was Y(thd)3 dissolved in toluene at a concentration of 0.01 M. The rate of injection of the solution into the evaporator was 0.75 g / min. The carrier gas (Ar) flow rate of the solution was 300 standard cubic centimeters per minute ("sccm").
[0072] The silicon oxide precursor used was di-tert-butoxydiacetoxysilane (DADBS), dissolved in toluene at a concentration of 0.01 M. The rate at which the solution was injected into the evaporator was 0.5 g / min. The carrier gas (Ar) flow rate of the solution was 300 sccm.
[0073] The ratio [molar amount of Y(thd)3] / [molar amount of DADBS] is equal to 1.46.
[0074] The flow rate of O2 introduced into the reaction chamber is 40% of 400 sccm, and the flow rate of N2 introduced into the reaction chamber is 60% of 400 sccm.
[0075] The ratio [molar amount of O2 injected] / [molar amount of toluene containing dissolved precursors] was 0.66. The approximate atomic composition of the deposit obtained by X-ray photoelectron spectroscopy measurements was as follows: Y: 23%, Si: 19%, O: 56%, C: 2%.
[0076] The expression “between... and...” must be understood as including the boundary.
Claims
1. A method of producing a component having improved resistance to oxidation and high temperature corrosion, comprising forming an environmental barrier coating on at least a portion of a ceramic matrix composite material, the environmental barrier coating being formed by direct liquid injection-metal organic chemical vapor deposition using one or more molecular precursors; wherein, In direct liquid injection-metal organic chemical vapor deposition, at least one molecular precursor in a liquid state is injected into an expansion chamber in the form of droplets, and the expansion chamber is heated to a certain temperature so that the at least one molecular precursor evaporates without causing its decomposition, so as to obtain a gas phase containing at least one molecular precursor in a gaseous state; and, wherein, the gas phase is entrained by a carrier gas to a reaction chamber in which a composite material is present, and the composite material is heated to a temperature sufficient to allow decomposition of at least one molecular precursor in the gas phase, so as to form an environmental barrier coating on the composite material.
2. The method according to claim 1, wherein: The environmental barrier coating includes a rare earth silicate and is formed from at least an alkoxysilane silicon oxide precursor and a rare earth β-diketone rare earth oxide precursor in the presence of an oxygen supply source.
3. The method according to claim 1, wherein: The nature and / or relative proportions of the molecular precursors are altered during formation of the environmental barrier coating to impart it with a varying composition.
4. The method according to claim 3, wherein: Forming the environmental barrier coating includes forming at least a first portion comprising a rare earth disilicate, and forming a second portion comprising a rare earth monosilicate over the first portion.
5. The method according to claim 3, wherein: Forming the environmental barrier coating includes forming at least a first portion comprising a rare earth monosilicate, and forming a second portion comprising a rare earth disilicate on the first portion.
6. The method according to claim 3, wherein: Forming the environmental barrier coating includes at least forming a first portion comprising a first rare earth silicate, and forming a second portion comprising a second rare earth silicate different from the first rare earth, the first portion and the second portion overlapping.
7. The method according to claim 1, wherein: The thickness of the environmental barrier coating is less than or equal to 1000 μm.
8. The method according to claim 1, wherein: The method includes depositing a bond coating comprising silicon on at least a portion of an exterior surface of a ceramic matrix composite material, and the environmental barrier coating is deposited on the bond coating.
9. The method according to claim 8, wherein: The bond coat is deposited by chemical vapor deposition.
10. The method according to claim 1, wherein: The formed environmental barrier coating is also subjected to a thermal crystallization treatment.
11. The method according to any one of claims 1 to 10, wherein: The component is a turbine engine component.