Resin composition
By using copolymers derived from α-olefins with more than 3 carbon atoms in combination with thermoplastic resins, and using a specific catalyst system for solution polymerization, the problem of bleeding during the molding process of thermoplastic resins is solved and excellent compatibility of the resin composition is achieved. properties and high performance of the molded body.
Patent Information
- Application Number
- CN202180067384.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-10-06
AI Technical Summary
Existing thermoplastic resins are prone to leakage problems during the molding process. Especially when liquid polyolefin is used as a plasticizer, the compatibility of polypropylene and other resins is poor, resulting in problems such as leakage in the molded body.
A copolymer derived from α-olefin with 3 or more carbon atoms is combined with a thermoplastic resin. The molecular weight and structural characteristics of the copolymer are ensured through methods such as gel permeation chromatography and differential scanning calorimetry to form excellent compatibility. The resin composition, including polypropylene and α-olefin copolymer, uses a bridged metallocene compound and an organoaluminum oxy compound as a catalyst for solution polymerization to prepare a resin composition with good compatibility.
It achieves excellent compatibility between thermoplastic resin and α-olefin copolymer, avoids bleeding problems, improves the mechanical properties, heat resistance and processability of the molded body, and ensures the stability and performance of the molded body.
Smart Images

Figure BDA0004154194860000031 
Figure BDA0004154194860000101 
Figure BDA0004154194860000161
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition having good moldability and capable of suppressing the occurrence of bleed-out in a molded body. Background Art
[0002] In the past, thermoplastic resins were used for various purposes in the form of molded bodies such as films, sheets, and fibers by extrusion molding. In order to obtain molded bodies with good mechanical properties by extrusion molding, resins with low melt flow rate (MFR) are usually used, but resins with low MFR cause many problems in moldability: poor meshing into the screw in the extruder, poor melting of the resin, instability of the ejection amount due to high extrusion torque, and limitation of the extrusion speed. In addition, the above-mentioned problems may also occur depending on the physical properties of the resin, deviations in shape, specifications of the extruder, etc. Therefore, in recent years, in order to solve such problems, there has been a growing demand for improved moldability.
[0003] As a common method for improving the moldability during extrusion molding, there is a method of adding a molding aid to a resin and molding it. For example, a method of applying a molding aid such as oil or polyethylene wax to a thermoplastic resin to be molded and molding it has been studied (for example, Patent Documents 1 and 2).
[0004] In addition, attempts have been made to mix liquid polyolefin as a plasticizer into a thermoplastic resin.
[0005] However, liquid polyolefin has poor compatibility with polypropylene and the like. Therefore, when liquid polyolefin is blended with thermoplastic resins such as polypropylene and molded, there is a problem that bleeding occurs in the obtained molded product.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Publication No. 5-80492
[0009] Patent Document 2: Japanese Patent Application No. 2003-528948 Summary of the invention
[0010] Problems to be solved by the invention
[0011] An object of the present invention is to provide a resin composition having good compatibility and not causing problems such as bleeding into a molded article.
[0012] Means for solving problems
[0013] The present invention relates to, for example, the following [1] to [5].
[0014] [1] A resin composition comprising 25 to 99.99% by mass of a thermoplastic resin (A) having a weight average molecular weight (Mw) of 50,000 or more in terms of polystyrene as measured by gel permeation chromatography (GPC), and 0.01 to 15% by mass of a copolymer (B) containing a structural unit derived from an α-olefin having 3 or more carbon atoms, wherein the copolymer (B) satisfies the following requirements (b-1) to (b-3): (b-1) a kinematic viscosity at 100° C. of 10 to 5,000 mm / s; 2 / s. (b-2) The content of structural units derived from α-olefins having 3 or more carbon atoms is in the range of 60 to 85 mol%. (b-3) The weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography (GPC) is 1,000 to 30,000, and the molecular weight distribution (Mw / Mn) is 2.5 or less.
[0015] [2] The resin composition according to [1], wherein the thermoplastic resin (A) is a polyolefin.
[0016] [3] The resin composition according to [1] or [2], wherein the α-olefin having 3 or more carbon atoms is propylene.
[0017] [4] The resin composition according to any one of [1] to [3], wherein the thermoplastic resin (A) is polypropylene.
[0018] [5] A method for producing the resin composition according to [1], comprising the following steps:
[0019] Step (1), carrying out the following method (α) to obtain, as the above-mentioned copolymer (B), a copolymer (B) that further satisfies the following requirements (b-4) and (b-5), and
[0020] In step (2), the thermoplastic resin (A), the copolymer (B) and any additives are melt-kneaded to obtain a resin composition.
[0021] (b-4) 1 The methyl index determined by H-NMR was in the range of 60 to 130%.
[0022] (b-5) When differential scanning calorimetry (DSC) is performed in the temperature range of -100°C to 150°C, no melting peak is observed.
[0023] Method (α): A method comprising the step of solution polymerizing ethylene and an α-olefin having 3 or more carbon atoms in the presence of the following catalyst system,
[0024] The catalyst system comprises:
[0025] a bridged metallocene compound (a) represented by the following formula 1, and
[0026] At least one compound (b) selected from the group consisting of an organoaluminum oxy-compound (b1) and a compound (b2) that reacts with the bridged metallocene compound (a) to form an ion pair.
[0027] [Chemical formula 1]
[0028]
[0029] [In Formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 Each is independently a hydrogen atom, a hydrocarbon group or a silicon-containing hydrocarbon group, and multiple adjacent groups may be connected to each other to form a ring structure.
[0030] R 6 and R 11 are the same groups as each other, being hydrogen atoms, hydrocarbon groups or silicon-containing hydrocarbon groups,
[0031] R 7 and R 10 are the same groups as each other, being hydrogen atoms, hydrocarbon groups or silicon-containing hydrocarbon groups,
[0032] R 6 and R 7 It can be bonded with hydrocarbons having 2 to 3 carbon atoms to form a ring structure.
[0033] R 10 and R 11 It can be bonded with hydrocarbons having 2 to 3 carbon atoms to form a ring structure.
[0034] R 6 , R 7 , R 10 and R 11 Not all hydrogen atoms at the same time;
[0035] Y is a carbon atom or a silicon atom;
[0036] R 13 and R 14 are each independently aryl;
[0037] M is Ti, Zr or Hf;
[0038] Q is independently a halogen atom, a hydrocarbon group, an anionic ligand or a neutral ligand capable of coordinating a lone pair of electrons;
[0039] j is an integer from 1 to 4.]
[0040] Effects of the Invention
[0041] The resin composition of the present invention has good compatibility. A thermoplastic resin such as polypropylene and an α-olefin copolymer as a plasticizer are mixed in an excellent compatible state, so that problems such as bleeding do not occur. DETAILED DESCRIPTION
[0042] Hereinafter, the present invention will be described in detail.
[0043] The resin composition according to the present invention contains the following thermoplastic resin (A) and the following copolymer (B).
[0044] [Thermoplastic resin (A)]
[0045] The thermoplastic resin (A) used in the present invention is not particularly limited, and examples thereof include polyolefins such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene, polybutene, cyclic olefin polymers, ethylene-propylene copolymers, and cyclic olefin copolymers; styrene polymers such as polystyrene, acrylonitrile-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, styrene-butadiene copolymers, and styrene-isoprene copolymers, and their hydrogenated products; polyvinyl chloride and polyvinylidene chloride; vinyl carboxylic acid polymers and vinyl carboxylic acid ester polymers such as polyacrylic acid, polymethacrylic acid, polymethyl acrylate, polymethyl methacrylate, and polyethyl methacrylate; ethylene-methacrylic acid copolymers, ethylene-methacrylate copolymers, ethylene-vinyl acetate copolymers, and ethylene-vinyl alcohol copolymers; polycarbonates and polymethacrylates; polyesters such as polyethylene terephthalate and polybutylene terephthalate; nylon 6, nylon 11, nylon 12, nylon 46, nylon 66, and nylon M XD6, wholly aromatic polyamide, semi-aromatic polyamide and other polyamides; polyacetal, and blends of these resins, etc.
[0046] Among these thermoplastic resins, polyolefins are preferred, low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene, and ethylene-propylene copolymers are more preferred, and polypropylene is particularly preferred. The polypropylene may be a polypropylene elastomer.
[0047] When the thermoplastic resin (A) is the above-mentioned polyolefin, the thermoplastic resin (A) has particularly excellent compatibility with the copolymer (B) described below, and a good resin composition free from deterioration in mechanical properties and bleed-out to the surface can be obtained.
[0048] The weight average molecular weight (Mw) of the thermoplastic resin (A) measured by gel permeation chromatography (GPC) in terms of polystyrene is 50,000 or more. The weight average molecular weight (Mw) is preferably 60,000 to 2,000,000, and more preferably 80,000 to 1,000,000. When the weight average molecular weight (Mw) of the thermoplastic resin (A) is 50,000 or more, a resin composition having excellent compatibility with the copolymer (B) can be obtained.
[0049] When the thermoplastic resin (A) is polypropylene, the MFR (JIS K7210; 230°C test load 2.16 kgf) of the polypropylene is preferably in the range of 0.1 to 60 g / 10 min, more preferably in the range of 0.3 to 20 g / 10 min, particularly preferably in the range of 0.3 to 10 g / 10 min.
[0050] When the MFR of the polypropylene is within the above range, a molded product excellent in mechanical properties, heat resistance, chemical resistance, etc. can be obtained.
[0051] <Content of thermoplastic resin (A)>
[0052] The content of the thermoplastic resin (A) in the entire resin composition of the present invention is 25 to 99.99 mass %, preferably 90 to 99.99 mass %, more preferably 96.2 to 99.8 mass %, particularly preferably 97 to 99.4 mass %, and more preferably 98 to 99.4 mass %.
[0053] If the content of the thermoplastic resin (A) in the resin composition as a whole is less than the lower limit, the properties of the thermoplastic resin (A) are impaired, and a molded product excellent in mechanical properties, heat resistance, chemical resistance, etc. may not be obtained. On the other hand, if the content of the thermoplastic resin (A) in the resin composition as a whole exceeds the upper limit, problems such as poor moldability, unstable ejection amount, and limited extrusion speed may occur.
[0054] [Copolymer (B)]
[0055] The copolymer (B) contains a structural unit derived from an α-olefin having at least 3 carbon atoms. The copolymer (B) satisfies the requirements (b1-1) to (b1-3) described below.
[0056] Examples of the α-olefin having 3 or more carbon atoms include linear α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tricene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene, and branched α-olefins such as 3-methyl-1-pentene, 4-methyl-1-pentene, 8-methyl-1-nonene, 7-methyl-1-decene, 6-methyl-1-undecene, and 6,8-dimethyl-1-decene. These α-olefins may be used alone or in combination of two or more.
[0057] The α-olefin having 3 or more carbon atoms is preferably an α-olefin having 3 to 20 carbon atoms, more preferably an α-olefin having 3 to 8 carbon atoms, and particularly preferably propylene.
[0058] <Requirement (b-1)>
[0059] The kinematic viscosity of the copolymer (B) at 100°C is 10 to 5,000 mm 2 / s.
[0060] The kinematic viscosity is preferably 10 to 3,500 mm 2 / s, more preferably 50 to 3500 mm 2 / s, more preferably 50 to 2,500 mm 2 / s, particularly preferably 50 to 700 mm 2 / s.
[0061] In the present invention, the kinematic viscosity at 100° C. is measured in accordance with ASTM D 445.
[0062] The kinematic viscosity of the copolymer (B) at 100°C is less than 10 mm 2 / s, similar to the softening agent such as the commonly used process oil, the content of the low molecular weight component with high fluidity and volatility increases, and sometimes the amount of bleeding and volatilization from the resin composition or its molded body increases, which is not preferred. If the kinematic viscosity of the copolymer (B) at 100°C is higher than 5,000 mm 2 / s, the fluidity deteriorates. Therefore, when the copolymer (B) is mixed with the thermoplastic resin (A), the adhesion sometimes increases and the processability decreases, which is not preferred. In other words, if the kinematic viscosity of the copolymer (B) at 100°C is within the above range, a resin composition or a molded product thereof having excellent heat aging resistance and processability can be obtained, which is preferred.
[0063] <Requirement (b-2)>
[0064] The content of the structural unit derived from the α-olefin having 3 or more carbon atoms in the copolymer (B) is within a range of 60 to 85 mol%.
[0065] The above content refers to the molar ratio of the structural unit derived from the α-olefin having 3 or more carbon atoms in all the structural units contained in the copolymer (B).
[0066] The content of the structural unit derived from the α-olefin having 3 or more carbon atoms in the copolymer (B) is preferably 63 to 83 mol%, more preferably 67 to 80 mol%.
[0067] In the resin composition of the present invention, since the content of the structural unit derived from α-olefin having 3 or more carbon atoms in the copolymer (B) is as high as 60 mol%, the compatibility between the thermoplastic resin (A) such as polyolefin and the copolymer (B) is excellent, and problems such as bleed-out will not occur. In addition, since the content of the structural unit derived from α-olefin having 3 or more carbon atoms in the copolymer (B) is 85 mol% or less, the crystallinity is low, and therefore, the copolymer is well compatible with the thermoplastic resin (A) such as polyolefin.
[0068] The content of structural units other than structural units derived from α-olefins having 3 or more carbon atoms contained in the copolymer (B) is in the range of 15 to 40 mol %, preferably 17 to 37 mol %, more preferably 20 to 33 mol %.
[0069] One embodiment of the copolymer (B) includes a copolymer of ethylene and an α-olefin having 3 or more carbon atoms.
[0070] <Requirement (b-3)>
[0071] The weight average molecular weight (Mw) of the copolymer (B) in terms of polystyrene measured by gel permeation chromatography (GPC) is 1,000 to 30,000, and the molecular weight distribution (Mw / Mn) is 2.5 or less.
[0072] The weight average molecular weight (Mw) of the copolymer (B) is preferably 1,500 to 25,000, more preferably 1,700 to 20,000.
[0073] If the weight average molecular weight is less than the aforementioned lower limit, the mobility of the copolymer (B) in the resin composition becomes high, so it is easy to ooze out. If the weight average molecular weight of the copolymer (B) is greater than the aforementioned upper limit, a sufficient flowability improvement effect cannot be obtained, and there is a situation where the moldability is not improved, the compatibility with the thermoplastic resin (A) deteriorates, resulting in a decrease in mechanical properties and bleeding.
[0074] The molecular weight distribution (Mw / Mn) of the copolymer (B) is preferably 2.3 or less, more preferably 2.1 or less.
[0075] When the molecular weight distribution of the copolymer (B) becomes broad (Mw / Mn becomes large), it is not preferable because a large number of low-molecular weight or high-molecular weight components are contained, which may cause bleeding or deterioration of mechanical properties.
[0076] The weight average molecular weight and molecular weight distribution of the copolymer (B) can be measured by gel permeation chromatography (GPC) calibrated using a standard substance (monodisperse polystyrene) having a known molecular weight.
[0077] The copolymer (B) may satisfy the following requirements (b-4) and (b-5) in addition to the above requirements (b-1) to (b-3). The copolymer (B) satisfying the requirements (b-4) and (b-5) can be produced by, for example, the method (α) described below.
[0078] <Requirement (b-4)>
[0079] The copolymer (B) is composed of 1 The methyl index determined by H-NMR was in the range of 60 to 130%.
[0080] The methyl index is preferably in the range of 70 to 125%, more preferably in the range of 80 to 120%.
[0081] If the copolymer (B) is composed of 1 When the methyl index measured by H-NMR is within the above range, a resin composition having good mechanical properties can be obtained. The reason why a resin composition having good mechanical properties can be obtained is believed to be because the methyl groups in the copolymer (B) enhance the interaction with the molecules of the thermoplastic resin (A).
[0082] Here, the methyl index is measured by dissolving the copolymer (B) in deuterated chloroform. 1 H-NMR and based on CHCl in deuterated chloroform 3 The ratio of the integrated value of the peak located in the range of 0.50 to 1.15 ppm to the integrated value of the peak located in the range of 0.50 to 2.20 ppm, using the solvent peak appearing at 7.24 ppm as a reference.
[0083] The methyl index is an index representing the ratio of the side chains in the copolymer (B). Therefore, if the methyl index is above the above lower limit, the side chains of the copolymer (B) are fully present, and thus, the molecular chains are not easily oriented to each other, and have molecular mobility, and good fluidity, softness, and lightness can be obtained, so it is preferred. On the other hand, if the methyl index of the copolymer (B) is below the above upper limit, the side chains of the copolymer (B) will not be too densely present, and the molecular mobility will not be reduced, and good fluidity, softness, and lightness can be maintained, so it is preferred.
[0084] If the methyl index is greater than the above-mentioned upper limit, the branched structure of the copolymer (B) becomes more, and therefore, when exposed to high temperature, the decomposition of the molecular chain becomes easy to proceed, and there is a concern that the heat resistance is reduced. In other words, it is believed that if the methyl index of the copolymer (B) is within the above-mentioned range, while maintaining the heat resistance, the copolymer (B) shows excellent molecular mobility, and it is easy to obtain a resin composition showing good fluidity, lightness, flexibility, and heat resistance, and therefore it is preferred.
[0085] <Requirement (b-5)>
[0086] When the copolymer (B) was subjected to differential scanning calorimetry (DSC) in the temperature range of -100°C to 150°C, no melting peak was observed.
[0087] The details of the differential scanning calorimetry are as follows.
[0088] Using a differential scanning calorimeter (e.g., Seiko Instruments Inc X-DSC-7000), a sample of about 8 mg of the copolymer is placed in a simple and airtight aluminum sample pan, placed in a DSC unit, and heated from room temperature to 150°C at 10°C / min under a nitrogen atmosphere. Then, after holding at 150°C for 5 minutes, the temperature is lowered at 10°C / min to cool the DSC unit to -100°C (cooling process). Then, after holding at -100°C for 5 minutes, the temperature is raised to 150°C at 10°C / min. The temperature at which the enthalpy curve obtained during the heating process shows a maximum value is taken as the melting point (Tm), and the sum of the endothermic heat accompanying the melting is taken as the melting heat (ΔH). When no melting peak is observed or the melting heat (ΔH) value is less than 1 J / g, it is considered that no melting point (Tm) is observed. The method for determining the melting point (Tm) and the melting heat (ΔH) refers to JIS K7121.
[0089] The method for producing the copolymer (B) is not particularly limited, and examples thereof include a method using a vanadium-based catalyst composed of a vanadium compound and an organic aluminum compound as described in Japanese Patent Publication No. 2-1163 and Japanese Patent Publication No. 2-7998. In addition, as a method for producing a copolymer with high polymerization activity, a method using a catalyst system composed of a metallocene compound such as zirconocene and an organic aluminum oxide compound (aluminoxane) as described in Japanese Patent Publication No. 61-221207, Japanese Patent Publication No. 7-121969, and Japanese Patent No. 2796376 can be adopted. This method can reduce the chlorine content of the obtained copolymer and the 2,1-insertion of α-olefins, and is therefore more preferred.
[0090] In the method using a vanadium-based catalyst, more chlorine compounds are used in the co-catalyst than in the method using a metallocene-based catalyst, so there is a high possibility that a trace amount of chlorine remains in the obtained copolymer (B). On the other hand, in the method using a metallocene-based catalyst, substantially no chlorine remains, so it is possible to prevent the deterioration of the resin composition caused by chlorine, which is preferred from this point of view. The chlorine content is preferably less than 100 ppm, more preferably less than 50 ppm, further preferably less than 20 ppm, and particularly preferably less than 5 ppm. The chlorine content can be quantified using various known methods. For example, there are the following methods: Using Thermo Fisher Scientific Inc.ICS-1600, ethylene·α-olefin copolymer is placed in a sample boat, and the mixture is stirred at 40 °C for 2 hours at 40 °C. 2 In the air flow, combustion and decomposition are carried out under the condition that the combustion furnace is set to 900°C. The gas generated at this time is absorbed into the absorption liquid and quantified by ion chromatography.
[0091] As a method using a metallocene-based catalyst, the following method (α) can be mentioned.
[0092] <Method (α)>
[0093] A method (α) comprising the step of solution polymerizing ethylene and an α-olefin having 3 or more carbon atoms in the presence of the following catalyst system, wherein the catalyst system comprises:
[0094] a bridged metallocene compound (a) represented by the following formula 1, and
[0095] At least one compound (b) selected from the group consisting of an organoaluminum oxy-compound (b1) and a compound (b2) that reacts with the bridged metallocene compound (a) to form an ion pair.
[0096] [Chemical formula 2]
[0097]
[0098] [In Formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 Each is independently a hydrogen atom, a hydrocarbon group or a silicon-containing hydrocarbon group, and multiple adjacent groups may be connected to each other to form a ring structure.
[0099] R 6 and R 11 are the same groups as each other, being hydrogen atoms, hydrocarbon groups or silicon-containing hydrocarbon groups,
[0100] R 7 and R 10 are the same groups as each other, being hydrogen atoms, hydrocarbon groups or silicon-containing hydrocarbon groups,
[0101] R 6 and R 7 It can be bonded with hydrocarbons having 2 to 3 carbon atoms to form a ring structure.
[0102] R 10 and R 11 It can be bonded with hydrocarbons having 2 to 3 carbon atoms to form a ring structure.
[0103] R 6 , R 7 , R 10 and R 11 Not all hydrogen atoms at the same time;
[0104] Y is a carbon atom or a silicon atom;
[0105] R 13 and R 14 are each independently aryl;
[0106] M is Ti, Zr or Hf;
[0107] Q is independently a halogen atom, a hydrocarbon group, an anionic ligand or a neutral ligand capable of coordinating a lone pair of electrons;
[0108] j is an integer from 1 to 4.]
[0109] Here, the hydrocarbon group has 1 to 20 carbon atoms, preferably 1 to 15, and more preferably 4 to 10 carbon atoms, and refers to, for example, an alkyl group, an aryl group, etc., and the aryl group has 6 to 20 carbon atoms, preferably 6 to 15 carbon atoms.
[0110] Examples of the silicon-containing hydrocarbon group include alkyl groups or aryl groups having 3 to 20 carbon atoms and containing 1 to 4 silicon atoms, and more specifically, trimethylsilyl groups, tert-butyldimethylsilyl groups, triphenylsilyl groups, and the like.
[0111] In the bridged metallocene compound represented by Formula 1, the cyclopentadienyl group may be substituted or unsubstituted.
[0112] In the bridged metallocene compound represented by Formula 1,
[0113] (i) The substituent (R) preferably bonded to the cyclopentadienyl group 1 , R 2 , R 3 and R 4 ) is a hydrocarbon group,
[0114] (ii) more preferably the substituent (R 1 , R 2 , R 3 and R 4 ) is a hydrocarbon group having 4 or more carbon atoms,
[0115] (iii) The substituent (R) most preferably bonded to the 3-position of the cyclopentadienyl group 2 or R 3 ) is a hydrocarbon group having 4 or more carbon atoms (e.g., n-butyl).
[0116] In R 1 , R 2 , R 3 and R 4 When at least two of the substituents are substituents (ie, not hydrogen atoms), the substituents may be the same or different, and it is preferred that at least one of the substituents is a hydrocarbon group having 4 or more carbon atoms.
[0117] In the metallocene compound represented by Formula 1, R bonded to the fluorene group 6 and R 11 Same, R 7 and R 10 Same, but R 6 , R 7 , R 10 and R 11 In the high temperature solution polymerization of poly-α-olefin, in order to improve the polymerization activity, it is preferred that R 6 and R 11 None of them is a hydrogen atom, and R 6 , R 7 , R 10 and R 11 For example, R bonded to the 2- and 7-positions of the fluorenyl group 6 and R 11 are the same hydrocarbon groups having 1 to 20 carbon atoms, preferably all tert-butyl groups, R 7 and R 10They are the same hydrocarbon groups having 1 to 20 carbon atoms, and preferably all of them are tert-butyl groups.
[0118] The main chain part (bonding part, Y) connecting the cyclopentadienyl group and the fluorenyl group is a bridging part containing two covalent bonds of one carbon atom or silicon atom as a structural bridging part that imparts steric rigidity to the aforementioned bridged metallocene compound represented by Formula 1. The bridging atom (Y) in the bridging part has two aromatic groups (R 13 and R 14 ). Therefore, the cyclopentadienyl group and the fluorenyl group are bonded via a covalent bond bridge portion containing an aryl group. Examples of aryl groups include phenyl, naphthyl, anthracenyl, and substituted aryl groups (in which one or more aromatic hydrogen atoms (sp 2 Examples of the substituents of the substituted aryl group include hydrocarbon groups having 1 to 20 carbon atoms, silicon-containing hydrocarbon groups having 1 to 20 carbon atoms, and halogen atoms, and preferably phenyl groups. In the bridged metallocene compound represented by Formula 1, R is preferably selected from the viewpoint of ease of production. 13 With R 14 same.
[0119] In the bridged metallocene compound represented by Formula 1, Q is preferably a halogen atom or a hydrocarbon group having 1 to 10 carbon atoms. Examples of the halogen atom include fluorine, chlorine, bromine, or iodine, and examples of the hydrocarbon group having 1 to 10 carbon atoms include methyl, ethyl, n-propyl, isopropyl, 2-methylpropyl, 1,1-dimethylpropyl, 2,2-dimethylpropyl, 1,1-diethylpropyl, 1-ethyl-1-methylpropyl, 1,1,2,2-tetramethylpropyl, sec-butyl, tert-butyl, 1,1-dimethylbutyl, 1,1,3-trimethylbutyl, neopentyl, cyclohexylmethyl, cyclohexyl, and 1-methyl-1-cyclohexyl. In addition, when j is an integer greater than 2, Q may be the same or different.
[0120] Examples of such bridged metallocene compounds (a) include:
[0121] Vinyl [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -fluorenyl) zirconium dichloride, vinyl [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, vinyl [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, vinyl [η 5-(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzofluorenyl)zirconium dichloride, vinyl [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, vinyl [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, vinyl [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, vinyl [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, vinyl [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride,
[0122] Vinyl [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -fluorenyl) zirconium dichloride, vinyl [η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, vinyl [η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, vinyl [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzofluorenyl)zirconium dichloride, vinyl[η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, vinyl[η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, vinyl[η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, vinyl[η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, vinyl [η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride,
[0123] Vinyl [η 5 -(3-n-butylcyclopentadienyl)](η 5 -fluorenyl) zirconium dichloride, vinyl [η 5-(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, vinyl [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, vinyl [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzofluorenyl)zirconium dichloride, vinyl[η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, vinyl[η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, vinyl[η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, vinyl[η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, vinyl [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride,
[0124] Diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -fluorenyl) zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5-(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride,
[0125] Diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](η 5 -fluorenyl) zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride,
[0126] Diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](η 5 -fluorenyl) zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene[η 5-(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene[η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride,
[0127] di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](η 5 -fluorenyl) zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride,
[0128] di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)](η 5 -fluorenyl) zirconium dichloride, di(p-tolyl)methylene[η 5-(3-tert-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride,
[0129] di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)](η 5 -fluorenyl) zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5-(3-n-butylcyclopentadienyl)](2,7-diphenyl-3,6-di-tert-butylfluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, etc.
[0130] Examples include compounds in which the zirconium atom of these compounds is replaced by a hafnium atom, compounds in which the chlorine ligand is replaced by a methyl group, and the like, but the bridged metallocene compound (a) is not limited to these examples.
[0131] As the organoaluminum oxy-compound (b1) used in the catalyst system in the method (α), existing aluminoxanes can be used. For example, linear or cyclic aluminoxanes represented by the following formulae 2 to 5 can be used. The organoaluminum oxy-compound may contain a small amount of an organoaluminum compound.
[0132] [Chemical formula 3]
[0133]
[0134] In formulae 2 to 4, R is independently a hydrocarbon group having 1 to 10 carbon atoms, Rx is independently a hydrocarbon group having 2 to 20 carbon atoms, and m and n are independently an integer of 2 or more, preferably 3 or more, more preferably 10 to 70, and most preferably 10 to 50.
[0135] [Chemical formula 4]
[0136]
[0137] In formula 5, R c is a hydrocarbon group having 1 to 10 carbon atoms, R d Each of the following is independently a hydrogen atom, a halogen atom or a hydrocarbon group having 1 to 10 carbon atoms.
[0138] In Formula 2 or Formula 3, R is a methyl group (Me) of an organic aluminum oxy-compound conventionally called "methylaluminoxane".
[0139] The aforementioned methylaluminoxane can be easily obtained and has high polymerization activity, so it is usually used as an active agent in polyolefin polymerization. However, methylaluminoxane is difficult to dissolve in saturated hydrocarbons, so it has been used in the form of a solution of aromatic hydrocarbons such as toluene or benzene, which is not desirable in terms of environmental protection. Therefore, in recent years, as an aluminoxane dissolved in saturated hydrocarbons, a flexible body of methylaluminoxane represented by formula 4 has been developed and used. The modified methylaluminoxane represented by formula 4 is prepared using trimethylaluminum and alkylaluminum other than trimethylaluminum, such as trimethylaluminum and triisobutylaluminum, as shown in the specification of U.S. Patent No. 4960878 and the specification of U.S. Patent No. 5041584. Rx is an isobutyl aluminoxane commercially available in the form of a saturated hydrocarbon solution and under the trade name of MMAO and TMAO. (Refer to Tosoh Finechem Corporation, Tosoh Research & Technology Review, Vol 47, 55 (2003)).
[0140] As the compound (b2) (ii) contained in the above-mentioned catalyst system and reacting with the above-mentioned bridged metallocene compound to form an ion pair (hereinafter referred to as "ionic compound" as needed), Lewis acids, ionic compounds, boranes, borane compounds, carborane compounds, which are described in Korean Patent Gazette No. 10-0551147, Japanese Patent Publication No. 1-501950, Japanese Patent Publication No. 3-179005, Japanese Patent Publication No. 3-179006, Japanese Patent Publication No. 3-207703, Japanese Patent Publication No. 3-207704, U.S. Patent No. 5321106, etc. can be used. If necessary, heteropoly compounds, isopoly compounds, etc. can be used, and ionic compounds described in Japanese Patent Publication No. 2004-51676 can be used. The above-mentioned ionic compounds can be used alone or in combination of two or more. In more detail, as examples of Lewis acids, BR can be mentioned. 3 The compound represented by (R is a fluoride, a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms (such as methyl), a substituted or unsubstituted aryl group having 6 to 20 carbon atoms (such as phenyl), etc.), for example, trifluoroboron, triphenylboron, tri(4-fluorophenyl)boron, tri(3,5-difluorophenyl)boron, tri(4-fluorophenyl)boron, tri(pentafluorophenyl)boron, and tri(p-tolyl)boron. If the above-mentioned ionic compound is used, its usage amount and sludge generation amount are relatively small compared with organic aluminum oxide compounds, which is economically advantageous. In the present invention, as the above-mentioned ionic compound, it is preferred to use a compound represented by the following formula 6.
[0141] [Chemical formula 5]
[0142]
[0143] In Formula 6, R e+ is H + , a carbonium cation, an oxonium cation, an ammonium cation, a phosphonium cation, a tropylium cation, or a ferrocenium cation having a transition metal. R f to R i are each independently an organic group, preferably a hydrocarbon group having 1 to 20 carbon atoms, more preferably an aryl group such as a pentafluorophenyl group. Examples of the aforementioned carbonium cation include tris(methylphenyl)carbonium cation, tris(dimethylphenyl)carbonium cation, etc. Examples of the aforementioned ammonium cation include dimethylanilinium cation, etc.
[0144] As the compound represented by the above Formula 6, preferably, N,N-dialkylanilinium salts can be mentioned. Specifically, N,N-dimethylanilinium tetraphenylborate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, N,N-diethylanilinium tetraphenylborate, N,N-diethylanilinium tetrakis(pentafluorophenyl)borate, N,N-diethylanilinium tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, N,N-2,4,6-pentamethylanilinium tetraphenylborate, N,N-2,4,6-pentamethylanilinium tetrakis(pentafluorophenyl)borate, etc.
[0145] The aforementioned catalyst system used in Method (α) further contains (c) an organoaluminum compound as needed. The aforementioned organoaluminum compound functions to activate the aforementioned bridged metallocene compound, the aforementioned organoaluminum oxide compound, the aforementioned ionic compound, etc. As the aforementioned organoaluminum compound, preferably, an organoaluminum represented by the following Formula 7 and a complex alkylate of a Group 1 metal and aluminum represented by the following Formula 8 can be used.
[0146] R a m Al(OR b ) n H p X q …(Formula 7)
[0147] In Formula 7, R a and R b are each independently a hydrocarbon group having 1 to 15 carbon atoms, preferably a hydrocarbon group having 1 to 4 carbon atoms. X is a halogen atom. m is an integer of 0 < m ≤ 3, n is an integer of 0 ≤ n ≤ 3, p is an integer of 0 < p ≤ 3, q is an integer of 0 ≤ q < 3, and m + n + p + q = 3.
[0148] M 2 AlR a4 …(Equation 8)
[0149] In formula 8, M 2 Indicates Li, Na or K, R a It is a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms.
[0150] Examples of the organoaluminum compound represented by Formula 7 include easily available trimethylaluminum and triisobutylaluminum. Examples of the alkyl complex compound of Group 1 metal and aluminum represented by Formula 8 include LiAl(C 2 H 5 ) 4 、LiAl(C 7 H 15 ) 4 Etc. A compound similar to the compound represented by Formula 7 can be used. For example, (C 2 H 5 ) 2 AlN(C 2 H 5 )Al(C 2 H 5 ) 2 In this way, an organic aluminum compound is formed by at least two aluminum compounds being bonded via a nitrogen atom.
[0151] In the method (α), the amount of the bridged metallocene compound (a) represented by formula 1 is preferably 5 to 50% by weight relative to the total catalyst composition. In addition, preferably, (i) the amount of the organoaluminum oxy-compound (b1) is 50 to 500 equivalents relative to the number of moles of the bridged metallocene compound used, (ii) the amount of the compound (b2) that reacts with the bridged metallocene compound to form an ion pair is 1 to 5 equivalents relative to the number of moles of the bridged metallocene compound used, and the amount of the organoaluminum compound (c) is 5 to 100 equivalents relative to the number of moles of the bridged metallocene compound used.
[0152] The catalyst system used in the method (α) may have, for example, the following [1] to [4].
[0153] [1] a bridged metallocene compound (a) represented by formula 1, and (i) an organoaluminum oxy-compound (b1)
[0154] [2] A bridged metallocene compound (a) represented by Formula 1, (i) an organoaluminum oxy-compound (b1), and an organoaluminum compound (c).
[0155] [3] A bridged metallocene compound (a) represented by formula 1, a compound (b2) that reacts with the bridged metallocene compound to form an ion pair, and an organoaluminum compound (c).
[0156] [4] A bridged metallocene compound (a) represented by formula 1, (i) an organoaluminum oxy-compound (b1), and (ii) a compound (b2) that reacts with the bridged metallocene compound to form an ion pair.
[0157] The bridged metallocene compound represented by Formula 1 (component (a)), (i) the organoaluminum oxy-compound (component (b1)), (ii) the compound (b2) that reacts with the bridged metallocene compound to form an ion pair, and / or the organoaluminum compound (component (c)) can be introduced into the starting raw material monomer (a mixture of ethylene and an α-olefin having 3 to 20 carbon atoms) in any order. For example, components (a), (b) and / or (c) are introduced into a polymerization reactor filled with the raw material monomers alone or in any order. Alternatively, at least two of components (a), (b) and / or (c) are mixed as needed, and the mixed catalyst composition is introduced into the polymerization reactor filled with the raw material monomers.
[0158] In the method (α), the copolymer (B) is prepared by solution polymerization of ethylene and an α-olefin having 3 or more carbon atoms, for example, 3 to 20 carbon atoms, under the catalyst system. As the α-olefin having 3 to 20 carbon atoms, one or more of linear α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, etc., branched α-olefins such as isobutylene, 3-methyl-1-butene, 4-methyl-1-pentene, and mixtures thereof can be used. Preferably, one or more α-olefins having 3 to 6 carbon atoms can be used, and propylene can be more preferably used. The solution polymerization can be carried out by using an inert solvent such as propane, butane, hexane, or the olefin monomer itself as a medium. In the method (α), the copolymerization temperature is usually 80 to 150°C, preferably 90 to 120°C, and the copolymerization pressure is usually atmospheric pressure to 500kgf / cm 2 , preferably atmospheric pressure to 50kgf / cm 2 , which may vary depending on the reaction materials, reaction conditions, etc.
[0159] The polymerization can be carried out in a batch mode, a semi-continuous mode or a continuous mode, and is preferably carried out in a continuous mode.
[0160] 〈Other methods〉
[0161] Copolymer (B) can be a non-modified product, or it can also be a modified product to which certain polar groups are given by graft modification. As a vinyl compound with a polar group for modification, vinyl compounds with oxygen-containing groups such as acids, anhydrides, esters, alcohols, epoxides, ethers, vinyl compounds with nitrogen-containing groups such as isocyanates and amides, vinyl compounds with silicon-containing groups such as vinyl silanes, etc. can be used. In addition, copolymer (B) can also be a modified product obtained by chlorinating a portion using the method described in Japanese Patent Publication No. 2020-97743.
[0162] Among them, vinyl compounds having oxygen-containing groups are preferred, and specifically, unsaturated epoxide monomers, unsaturated carboxylic acids and derivatives thereof are preferred. As unsaturated epoxide monomers, there are unsaturated glycidyl ethers, unsaturated glycidyl esters (e.g., glycidyl methacrylate), etc. As the aforementioned unsaturated carboxylic acids, there are acrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, nadic acid TM (endo-cis-bicyclo[2,2,1]hept-5-ene-2,3-dicarboxylic acid), etc.
[0163] In addition, examples of the derivatives of the unsaturated carboxylic acid include halide compounds, amide compounds, imide compounds, anhydrides, and ester compounds of the unsaturated carboxylic acid, etc. Specifically, maleic acid chloride, maleimide, maleic anhydride, citraconic anhydride, monomethyl maleate, dimethyl maleate, glycidyl maleate, etc.
[0164] Among them, unsaturated dicarboxylic acids and their anhydrides are more preferred, and maleic acid, nadic acid TM, and their anhydrides are particularly preferably used.
[0165] It should be noted that the position where the vinyl compound having a polar group or its derivative is grafted to the copolymer (B) is not particularly limited, and the unsaturated carboxylic acid or its derivative may be bonded to any carbon atom of the copolymer (B).
[0166] When the thermoplastic resin (A) has a polar group, by providing the copolymer (B) with the polar group, good compatibility between the copolymer (B) and the thermoplastic resin (A) can be obtained, and reduction in mechanical properties of the resin composition and bleed-out can be suppressed.
[0167] The copolymer (B) as the modified product as described above can be produced by various conventionally known methods, for example, the following method.
[0168] Method (1) is to mix the unmodified copolymer (B) using an extruder, a batch reactor or the like, and add a vinyl compound having a polar group or a derivative thereof to carry out graft copolymerization.
[0169] Method (2) is to dissolve the unmodified copolymer (B) in a solvent, add a vinyl compound having a polar group or a derivative thereof, and carry out graft copolymerization.
[0170] In any of the above methods, it is preferred that the graft reaction be carried out in the presence of a radical initiator in order to efficiently carry out graft copolymerization of the graft monomer of the vinyl compound having a polar group or a derivative thereof.
[0171] As the radical initiator, for example, organic peroxides and azo compounds can be used. Examples of the organic peroxides include benzoyl peroxide, dichlorobenzoyl peroxide, and dicumyl peroxide, and examples of the azo compounds include azobisisobutyronitrile and dimethyl azoisobutyrate.
[0172] Specifically, as such a radical initiator, dialkyl peroxides such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 1,4-bis(tert-butylperoxyisopropyl)benzene are preferably used.
[0173] These radical initiators are used in an amount of usually 0.001 to 1 part by mass, preferably 0.003 to 0.5 part by mass, and more preferably 0.05 to 0.3 part by mass, based on 100 parts by mass of the copolymer (B).
[0174] The reaction temperature in the grafting reaction using the above-mentioned radical initiator or the grafting reaction performed without using the radical initiator is usually set in the range of 60 to 350°C, preferably 120 to 300°C.
[0175] The graft amount of the vinyl compound having a polar group in the modified copolymer obtained as described above is usually 0.01 to 15% by mass, preferably 0.05 to 10% by mass, when the mass of the modified copolymer is 100% by mass.
[0176] <Content of copolymer (B)>
[0177] The content of the copolymer (B) in the entire resin composition of the present invention is 0.01 to 15% by mass, preferably 0.1 to 13% by mass, more preferably 0.5 to 12% by mass, particularly preferably 1 to 10% by mass.
[0178] If the content of the copolymer (B) in the resin composition as a whole is less than the aforementioned lower limit, the fluidity improvement effect brought by the copolymer (B) cannot be fully presented. On the other hand, if the content of the copolymer (B) in the aforementioned resin composition as a whole exceeds the aforementioned upper limit, the mechanical strength of the resin composition is reduced and oozes out sometimes, so it is not preferred. In other words, if the content of the copolymer (B) is within the aforementioned range, it is easy to obtain a resin composition having no oozing out, excellent mechanical strength and moldability, and is therefore preferred. The aforementioned effect is particularly useful for thermoplastic resins (A) with low MFR having excellent mechanical strength, because it is possible to improve moldability while maintaining the mechanical strength that is a characteristic thereof.
[0179] [Other ingredients]
[0180] The resin composition of the present invention may contain additives such as antioxidants, ultraviolet absorbers, stabilizers such as light stabilizers, metal soaps, fillers, flame retardants, antibacterial agents, antifungal agents, pigments, etc., as needed.
[0181] Examples of the stabilizer include antioxidants such as hindered phenol compounds, phosphite compounds, and thioether compounds; ultraviolet absorbers such as benzotriazole compounds and benzophenone compounds; and light stabilizers such as hindered amine compounds.
[0182] Examples of the metal soap include stearates such as magnesium stearate, calcium stearate, barium stearate, and zinc stearate.
[0183] Examples of the filler include glass fiber, silica fiber, metal fiber (stainless steel, aluminum, titanium, copper, etc.), natural fiber (wood flour, wood fiber, bamboo, bamboo fiber, cotton, cellulose, nanocellulose, wool, wheat straw, hemp, flax, kenaf, kapok, jute, ramie, sisal, henequen, corn, nut shell, wood pulp, rayon, cotton yarn, etc.), carbon black, graphite, activated carbon, graphite, carbon nanotube, carbon nanofiber, carbon nanohorn, graphene nanoplatelet, nanoporous carbon, carbon fiber, silica, glass beads, silicates (calcium silicate, talc, clay, etc.), metal oxides (iron oxide, titanium oxide, magnesium oxide, aluminum oxide, etc.), metal carbonates (calcium carbonate, barium carbonate, etc.), sulfates (calcium sulfate, barium sulfate, etc.), various metal powders (magnesium, silicon, aluminum, titanium, copper, etc.), mica, glass flakes, pumice powder, pumice balls (pumice) balloon), aluminum hydroxide, magnesium hydroxide, basic magnesium carbonate, dolomite, calcium titanate, calcium sulfite, asbestos, montmorillonite, bentonite, molybdenum sulfide, organic fillers (lignin, starch, etc.), and products containing the same. In particular, for fillers having anisotropy in structure such as glass fiber, silica fiber, metal fiber, natural fiber, carbon nanotube, carbon nanofiber, carbon nanohorn, carbon fiber, etc., the filler is broken by shearing during kneading, thereby reducing anisotropy and its characteristics are easily impaired, but the copolymer (B) reduces shearing during kneading due to the fluidity improvement effect, making it easy to maintain anisotropy, so it is useful.
[0184] Examples of the flame retardant include halogenated diphenyl ethers such as decabromodiphenyl ether and octabromodiphenyl ether, halogenated polycarbonates, inorganic compounds such as antimony trioxide, antimony tetroxide, antimony pentoxide, sodium pyroantimonate, and aluminum hydroxide, and phosphorus compounds. In addition, compounds such as tetrafluoroethylene may be added as flame retardant aids to prevent dripping.
[0185] Examples of the aforementioned antibacterial and antifungal agents include organic compounds such as imidazole compounds, thiazole compounds, nitrile compounds, halogenated alkyl compounds, and pyridine compounds; and inorganic substances and compounds such as silver, silver compounds, zinc compounds, copper compounds, and titanium compounds.
[0186] As the pigment, pigments conventionally used for coloring synthetic resins can be used. Specifically, metals such as aluminum, silver, and gold; carbonates such as calcium carbonate and barium carbonate; ZnO, TiO 2 etc. oxides; Al 2 O 3 ·nH 2 O, Fe 2 O 3 ·nH 2O and other hydroxides; CaSO 4 ,BaSO 4 Sulfate; Bi(OH) 2 NO 3 Nitrates such as PbCl 2 Chloride; CaCrO 4 、BaCrO 4 Chromates; CoCrO 4 Chromites, manganates and permanganates; Cu(BO) 2 etc. borate; Na 2 U 2 O 7 6H 2 O and other uranates; K 3 Co(NO 2 ) 6 ·3H 2 O and other nitrites; SiO 2 Silicates such as CuAsO 3 ·Cu(OH) 2 Arsenates and arsenites; Cu(C 2 H 3 O 2 ) 2 ·Cu(OH) 2 acetate; (NH 4 ) 2 MnO 2 (P 2 O 7 ) 2 Phosphates such as aluminates, molybdates, zincates, antimonates, tungstate selenides, titanates, ferric cyanides, phthalates, CaS, ZnS, CdS, black lead, carbon black, etc. inorganic pigments, cochineal lake, madder red lake, etc. natural organic pigments, naphthol green Y, naphthol green B, etc. nitroso pigments; naphthol yellow S, Pigment Chlorine 2G, etc. nitro pigments; Permanent Red 4R; Hanza Yellow, Brilliant Carmine 68, Scarlet 2R, etc. azo pigments; malachite green, rhodamine B, etc. basic dye lakes, acid green lake, azure lake, etc. acid dye lakes, alizarin lake, purpurin lake, etc. mordant dye lakes, thioindigo B, Indanthrene Orange, etc. vat dye pigments, phthalocyanine blue, phthalocyanine green, etc. phthalocyanine pigments, etc. organic pigments, etc.
[0187] The above-mentioned additives can be used in any ratio and by any adding method within the range that does not impair the effects of the present invention.
[0188] [Resin composition]
[0189] The resin composition according to the present invention is characterized in that it contains a thermoplastic resin (A) and a copolymer (B) as essential components and may contain the above-mentioned other components within a range not impairing the effects of the invention.
[0190] The composition and molecular weight of the resin composition of the present invention are not particularly limited as long as they are within the scope of the present invention. From the perspective of obtaining good moldability and mechanical properties, the proportion of components with a molecular weight of less than 5,000 observed by gel permeation chromatography (GPC) is preferably 0.7 to 4.5% relative to the overall components of the resin composition, more preferably 1.0 to 4.5%, further preferably 1.2 to 4.5%, and particularly preferably 1.3 to 3.0%. Components with a molecular weight of less than 5,000 improve the moldability of the resin composition, but on the other hand, they can cause problems such as reduced mechanical properties and oozing out. If the proportion of components with a molecular weight of less than 5,000 in the resin composition is within the aforementioned range, it is preferred that the effect of improving moldability is easily obtained while suppressing problems such as reduced mechanical properties and oozing out.
[0191] [Method for producing resin composition]
[0192] The resin composition of the present invention is produced by melt-kneading a thermoplastic resin (A), a copolymer (B) and, if necessary, additives. As a method for melt-kneading, a single-screw extruder, a twin-screw extruder, etc. can be used.
[0193] Regarding the method of adding the copolymer (B) to the thermoplastic resin (A), various methods can be used within the scope that does not impair the effect of the invention. For example, there can be mentioned: a method of dry-mixing the thermoplastic resin (A) and the copolymer (B) using a high-speed mixer such as a Henschel mixer, a roller, etc., and then melt-kneading; when the thermoplastic resin (A) is melt-kneaded, the copolymer (B) is directly added from the open part, or the copolymer (B) is inserted using a side feeder or a liquid feed pump, thereby melt-kneading.
[0194] The temperature during melt kneading is not particularly limited as long as it is a temperature at which the thermoplastic resin (A) etc. melts. For example, when the thermoplastic resin (A) is polypropylene, it is usually in the range of 190 to 300°C, preferably in the range of 200 to 250°C.
[0195] <Method for producing a masterbatch using a copolymer (B)>
[0196] As a method for producing the resin composition of the present invention, a copolymer (B) and a thermoplastic resin (A) may be melt-kneaded to produce a masterbatch containing the copolymer (B), and a thermoplastic resin (A) may be further added to the masterbatch containing the copolymer (B), and the two may be melt-kneaded to produce the resin composition.
[0197] The thermoplastic resin (A) used in the production of the masterbatch containing the copolymer (B) and the thermoplastic resin (A) further added to the masterbatch after the production of the masterbatch may be the same resin or different resins.
[0198] The method for producing the masterbatch containing the copolymer (B) is not particularly limited, and examples thereof include a method for producing the masterbatch by melt-kneading the copolymer (B) and the thermoplastic resin (A) and additives as required using a single screw extruder, a twin screw extruder, a plastomill, a Brabender mixer, a kneader, a roll mixer, a Banbury mixer, etc. Among them, from the perspective of easy mass production and easy acquisition of a pellet-shaped masterbatch, a method using a single screw extruder or a twin screw extruder is preferred, and from the perspective of improving the compatibility of the copolymer (B) and inhibiting bleeding, a method using a twin screw extruder is particularly preferred.
[0199] The temperature during melt kneading in the production of the masterbatch is not particularly limited as long as it is a temperature at which the thermoplastic resin (A) etc. melts. For example, when the thermoplastic resin (A) is polypropylene, it is usually in the range of 190 to 300°C, preferably in the range of 200 to 250°C.
[0200] The amount of the copolymer (B) contained in the masterbatch containing the copolymer (B) used in the present invention is not particularly limited, but is generally in the range of 0.1 to 100 parts by mass, preferably in the range of 0.1 to 20 parts by mass, more preferably in the range of 0.5 to 10 parts by mass, and particularly preferably in the range of 3 to 10 parts by mass, relative to 100 parts by mass of the thermoplastic resin (A) contained in the masterbatch containing the copolymer (B).
[0201] If the copolymer (B) is mixed with a mass of more than the lower limit of the aforementioned range, the components of the thermoplastic resin (A) are easily softened and melted by the copolymer (B), and when the masterbatch containing the copolymer (B) and the further added thermoplastic resin (A) are melt-kneaded by an extruder, a good fluidity improvement effect can be obtained, which is preferred. In addition, if the copolymer (B) is mixed with a mass below the upper limit of the aforementioned range, the oozing of the copolymer (B) can be suppressed, and a masterbatch containing the copolymer (B) that is not sticky can be obtained, which is preferred.
[0202] The method for melt-kneading the masterbatch containing the copolymer (B) and the thermoplastic resin (A) added to the masterbatch is not particularly limited, and for example, the same method as the melt-kneading method in the method for producing the masterbatch containing the copolymer (B) can be used.
[0203] As the ratio of the amount of the masterbatch containing the copolymer (B) to the thermoplastic resin (A) added to the masterbatch, the masterbatch containing the copolymer (B) is preferably 1 to 110 parts by mass, more preferably 15 to 110 parts by mass, and particularly preferably 15 to 50 parts by mass, relative to 100 parts by mass of the thermoplastic resin (A) added to the masterbatch. If the ratio of the amount of the masterbatch containing the copolymer (B) to the thermoplastic resin (A) added to the masterbatch is less than the lower limit of the aforementioned range, the content of the copolymer (B) in the resin composition decreases, and it is sometimes difficult to show the effect of improving the moldability. On the other hand, if the ratio of the amount of the masterbatch containing the copolymer (B) to the thermoplastic resin (A) added to the masterbatch is greater than the upper limit of the aforementioned range, the content of the copolymer (B) increases, which easily causes a decrease in mechanical properties.
[0204] When the resin composition according to the present invention is used as an adhesive or a coating agent, it can be kneaded using various organic solvents that can dissolve the thermoplastic resin (A) and the copolymer (B).
[0205] [Molding body]
[0206] The resin composition can be used to obtain a molded body comprising the resin composition. The molded body can be obtained, for example, by melt-mixing the thermoplastic resin (A) and the copolymer (B). At this time, as described above, a masterbatch containing the copolymer (B) can be manufactured, and the thermoplastic resin (A) is further added to the masterbatch and melt-mixed. In addition, the resin composition can be molded immediately after melt-mixing to obtain a molded body.
[0207] Examples of the molding method include T-die molding, blow molding, injection molding, and other known molding methods.
[0208] For example, when polypropylene is used as the thermoplastic resin (A) and is molded into an extruded sheet or film by T-die extrusion molding or the like, a molded body can be obtained by extrusion molding at a temperature of usually 170 to 300° C., preferably 180 to 270° C., and more preferably 190 to 250° C. Alternatively, a stretched film can be obtained by stretching a film extruded from an extruder by, for example, a tenter method (longitudinal and transverse stretching, transverse and longitudinal stretching), a simultaneous biaxial stretching method, or a uniaxial stretching method.
[0209] When polypropylene is used as the thermoplastic resin (A) and the molded article of the present invention is obtained by extrusion blow molding, the molded article can be obtained by extruding the mold in the form of a tubular parison at a resin temperature of 170 to 240° C. from a die, then holding the parison in the mold having the desired shape, blowing air therein, and attaching the parison to the mold at a resin temperature of 160 to 230° C., etc. In addition, during extrusion blow molding, stretching at an appropriate ratio can be performed.
[0210] When polypropylene is used as the thermoplastic resin (A) and injection molding is performed, the cylinder temperature during injection molding is usually in the range of 180 to 400° C., preferably 200 to 300° C., more preferably 200 to 250° C., the injection pressure is usually in the range of 10 to 200 MPa, preferably 20 to 150 MPa, and the mold temperature is usually in the range of 20 to 200° C., preferably 20 to 80° C., more preferably 20 to 60° C.
[0211] Example
[0212] Hereinafter, the present invention will be described by way of examples, but the present invention is not limited to these examples at all.
[0213] In the following Examples and Comparative Examples, various physical properties were measured or evaluated by the following methods.
[0214] [Kinematic viscosity]
[0215] The kinematic viscosity was measured at 100° C. using a fully automatic viscometer CAV-4 manufactured by Canon Corporation in accordance with ASTM D 445.
[0216] [Propylene content]
[0217] For the α-olefin copolymer, an ECP500 nuclear magnetic resonance apparatus manufactured by JEOL Ltd. was used, and as the solvent, a mixed solvent of o-dichlorobenzene / deuterated benzene (80 / 20 volume %) was used. The sample concentration was 55 mg / 0.6 mL, the measurement temperature was 120° C., and the observed nuclei were 13 C (125 MHz), the sequence was single pulse proton decoupling, the pulse width was 4.7 μs (45° pulse), the repetition time was 5.5 s, the accumulation number was more than 10,000 times, and 27.50 ppm was used as the reference value of chemical shift for measurement.
[0218] The propylene content was determined as described above. 13C-NMR spectrum: determined based on reports by GJ Ray (Macromolecules, 10, 773 (1977)), JC Randall (Macromolecules, 15, 353 (1982)), K. Kimura (Polymer, 25, 4418 (1984)), and others.
[0219] [Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn)]
[0220] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the copolymer (B) were measured using the following high-performance GPC measuring device. A monodisperse polystyrene with a known molecular weight was used as a standard substance for calibration. The molecular weight distribution (Mw / Mn) was calculated from the obtained molecular weights.
[0221] Measuring device: HLC8320GPC manufactured by Tosoh Corporation
[0222] Mobile phase: THF (manufactured by Wako Pure Chemical Industries, Ltd., stabilizer-free, grade for liquid chromatography)
[0223] Column: Two TSKgel Super MultiporeHZ-M manufactured by Tosoh Corporation were connected in series.
[0224] Sample concentration: 5 mg / mL
[0225] Mobile phase flow rate: 0.35 mL / min
[0226] Measurement temperature: 40℃
[0227] Standard sample for calibration curve: PStQuick MP-M manufactured by Tosoh Corporation
[0228] The molecular weight of the polyethylene wax used in the comparative example was measured using the following measuring device, and calibration was performed using monodisperse polystyrene with a known molecular weight as a standard substance.
[0229] Measuring device: HLC-8321GPC / HT manufactured by Tosoh Corporation
[0230] Mobile phase: o-dichlorobenzene
[0231] Column: 2 TSKgel GMH6-HT and 2 TSKgel GMH6-HTL manufactured by Tosoh Corporation connected in series
[0232] Sample concentration: 0.1 mg / mL
[0233] Mobile phase flow rate: 1.0 mL / min
[0234] Measuring temperature: 140℃
[0235] Standard sample for calibration curve: Monodisperse polystyrene #3std set manufactured by Tosoh Corporation
[0236] [B value]
[0237] o-Dichlorobenzene / Benzene-d 6 The results were obtained by using a spectral analyzer (4 / 1 [vol / vol%]) as the measuring solvent, under the conditions of a measuring temperature of 120°C, a spectral width of 250 ppm, a pulse repetition time of 5.5 seconds, and a pulse width of 4.7 sec (45° pulse) (100 MHz, ECX400P, JEOL Ltd.), or a measuring temperature of 120°C, a spectral width of 250 ppm, a pulse repetition time of 5.5 seconds, and a pulse width of 5.0 sec (45° pulse) (125 MHz, Bruker BioSpinAVANCEIIIcryo-500). 13 The B value was calculated from the C-NMR spectrum based on the following formula (1). The peaks were assigned with reference to the above-mentioned known documents.
[0238] B=P O1-O2 / (2×P O1 ×P O2 ) (1)
[0239] In the above formula (1), P O1 represents the molar fraction of the structural unit derived from the first olefin, P O2 represents the molar fraction of the structural unit derived from the second olefin, P O1-O2 It represents the molar fraction of the "first olefin-second olefin" chain of all dyad chains.
[0240] [Unsaturated bond amount]
[0241] o-dichlorobenzene-d 4 The measurement was performed under the measurement conditions of a measurement temperature of 120° C., a spectrum width of 20 ppm, a pulse repetition time of 7.0 seconds, and a pulse width of 6.15 μsec (45° pulse) as the measurement solvent. 1 H-NMR spectrum (400 MHz, JEOL ECX400P). Using the solvent peak (o-dichlorobenzene 7.1 ppm) as a chemical shift standard, the amount of unsaturated bonds per 1000 carbon atoms (units / 1000C) was calculated from the ratio of the integral value of the main peak observed at 0 to 3 ppm and the peak from unsaturated bonds observed at 4 to 6 ppm.
[0242] [Chlorine content]
[0243] The copolymer samples were loaded into sample boats using Thermo Fisher Scientific Inc. ICS-1600 and heated in an Ar / O atmosphere. 2 In the air flow, combustion and decomposition are carried out under the condition that the combustion furnace is set at 900°C. The gas generated at this time is absorbed into the absorption liquid, and the chlorine content is quantified by ion chromatography.
[0244] [density]
[0245] The density was measured in accordance with JIS K7112 (density gradient tube method).
[0246] [Melting point]
[0247] Using Seiko Instruments Inc X-DSC-7000, a sample of about 8 mg of the copolymer was placed in a simple and sealed aluminum sample pan, and placed in a DSC unit. The DSC unit was heated from room temperature to 150°C at 10°C / min under a nitrogen atmosphere. Then, after being kept at 150°C for 5 minutes, the temperature was lowered at 10°C / min, and the DSC unit was cooled to -100°C (cooling process). Then, after being kept at -100°C for 5 minutes, the temperature was raised to 150°C at 10°C / min, and the temperature at which the enthalpy curve obtained during the heating process showed a maximum value was taken as the melting point (Tm), and the sum of the endothermic heat accompanying the melting was taken as the melting heat (ΔH). When no melting peak is observed or the melting heat (ΔH) value is less than 1J / g, it is considered that no melting point (Tm) is observed. The method for determining the melting point (Tm) and the melting heat (ΔH) is based on JIS K7121.
[0248] [Methyl index]
[0249] The nuclear magnetic resonance apparatus EX270 manufactured by JEOL Ltd. was used. The solvent was deuterated chloroform. The sample concentration was 55 mg / 0.6 mL. The measurement temperature was room temperature. The observation nucleus was 1 H (270 MHz), single pulse as sequence, 6.5 μs (45° pulse) as pulse width, 5.5 s as repetition time, 16 accumulation times, and chemical shift reference value based on CHCl in deuterated chloroform. 3 The solvent peak was 7.24 ppm and measured.
[0250] The 1The ratio of the integral value of the peak in the range of 0.50 to 1.15 ppm to the integral value of the peak in the range of 0.50 to 2.20 ppm in the spectrum obtained by H-NMR spectrum is used as a methyl index. Here, the peak based on α-olefin (co)polymer is roughly included in the range of 0.50 to 2.20 ppm. In this range, the peak based on methyl is likely to be included in the range of 0.50 to 1.15 ppm.
[0251] Thermoplastic resin (A)
[0252] As the thermoplastic resin (A), polypropylene F113G manufactured by Prime Polymer Co., Ltd. (hereinafter referred to as thermoplastic resin (a)) was used.
[0253] Copolymer (B) and other copolymers
[0254] As the copolymer (B), a copolymer (b-1) produced by the following production method was used. As other copolymers, copolymers (b-2) and (b-3) produced by the following production method were used.
[0255] [Method for producing copolymer (b-1)]
[0256] 250 mL of decane was charged into a glass polymerization vessel having an internal volume of 1 L and fully purged with nitrogen. After the temperature in the system was raised to 130° C., ethylene at a flow rate of 15 L / hr, propylene at a flow rate of 85 L / hr, and hydrogen at a flow rate of 100 L / hr were continuously supplied into the polymerization vessel, and the mixture was stirred at a stirring speed of 600 rpm. Next, 0.2 mmol of triisobutylaluminum was charged into the polymerization vessel, and then 2.022 mmol of MMAO and [methylphenylmethylene (η 5 -cyclopentadienyl)(η 5-2,7-di-tert-butylfluorenyl)] 0.00670mmol of zirconium dichloride was pre-mixed for more than 15 minutes and loaded into a polymerizer to start polymerization. Then, ethylene, propylene and hydrogen were continuously supplied and polymerization was carried out at 130°C for 15 minutes. After the polymerization was stopped by adding a small amount of isobutyl alcohol into the system, the unreacted monomers were purged. The obtained polymer solution was washed 3 times with 100mL of 0.2mol / l hydrochloric acid, then washed 3 times with 100mL of distilled water, dried with magnesium sulfate, and the solvent was distilled off under reduced pressure. The obtained polymer was dried under reduced pressure at 80°C overnight to obtain 0.83g of propylene-ethylene copolymer (copolymer (b-1)). The amount of unsaturated bonds after hydrogenation is less than 0.1 / 1000C, and the chlorine content is less than 0.1ppm. The obtained copolymer had a propylene content of 70.0 mol%, a Mw of 4,235, a Mw / Mn of 1.7, a B value of 1.2, and a kinematic viscosity at 100°C of 100 mm 2 / s, by 1 The methyl index determined by H-NMR was 83%.
[0257] [Method for producing copolymer (b-2)]
[0258] 250 mL of decane was charged into a glass polymerization vessel having an internal volume of 1 L and fully purged with nitrogen. After the temperature in the system was raised to 130° C., ethylene at a flow rate of 25 L / hr, propylene at a flow rate of 75 L / hr, and hydrogen at a flow rate of 100 L / hr were continuously supplied into the polymerization vessel, and the mixture was stirred at a stirring speed of 600 rpm. Next, 0.2 mmol of triisobutylaluminum was charged into the polymerization vessel, and then 1.213 mmol of MMAO and [methylphenylmethylene (η 5 -cyclopentadienyl)(η 5-2,7-di-tert-butylfluorenyl)] 0.00402mmol of zirconium dichloride was pre-mixed for more than 15 minutes and loaded into a polymerizer to start polymerization. Then, ethylene, propylene and hydrogen were continuously supplied and polymerization was carried out at 130°C for 15 minutes. After the polymerization was stopped by adding a small amount of isobutyl alcohol into the system, the unreacted monomers were purged. The obtained polymer solution was washed 3 times with 100mL of 0.2mol / l hydrochloric acid, then washed 3 times with 100mL of distilled water, dried with magnesium sulfate, and the solvent was distilled off under reduced pressure. The obtained polymer was dried under reduced pressure at 80°C overnight to obtain 0.77g of propylene-ethylene copolymer (copolymer (b-2)). The amount of unsaturated bonds after hydrogenation is less than 0.1 / 1000C, and the chlorine content is less than 0.1ppm. The obtained copolymer had a propylene content of 51.2 mol%, Mw of 4,172, Mw / Mn of 1.7, B value of 1.2, and a kinematic viscosity of 100°C of 102 mm 2 / s, by 1 The methyl index determined by H-NMR was 54%.
[0259] [Method for producing copolymer (b-3)]
[0260] 250 mL of decane was charged into a glass polymerization vessel having an internal volume of 1 L and fully purged with nitrogen. After the temperature in the system was raised to 130° C., ethylene at a flow rate of 7 L / hr, propylene at a flow rate of 93 L / hr, and hydrogen at a flow rate of 100 L / hr were continuously supplied into the polymerization vessel, and the mixture was stirred at a stirring speed of 600 rpm. Next, 0.2 mmol of triisobutylaluminum was charged into the polymerization vessel, and then 4.332 mmol of MMAO and [methylphenylmethylene (η 5 -cyclopentadienyl)(η 5-2,7-di-tert-butylfluorenyl)] 0.0144mmol of zirconium dichloride was pre-mixed for more than 15 minutes and loaded into a polymerizer to start polymerization. Then, ethylene, propylene and hydrogen were continuously supplied and polymerization was carried out at 130°C for 15 minutes. After the polymerization was stopped by adding a small amount of isobutyl alcohol to the system, the unreacted monomers were purged. The obtained polymer solution was washed 3 times with 100mL of 0.2mol / l hydrochloric acid, then washed 3 times with 100mL of distilled water, dried with magnesium sulfate, and the solvent was distilled off under reduced pressure. The obtained polymer was dried under reduced pressure at 80°C overnight to obtain 0.87g of propylene-ethylene copolymer (copolymer (b-3)). The amount of unsaturated bonds after hydrogenation is less than 0.1 / 1000C, and the chlorine content is less than 0.1ppm. The obtained copolymer had a propylene content of 86.0 mol%, a Mw of 4,208, a Mw / Mn of 1.7, a B value of 1.2, and a kinematic viscosity at 100°C of 104 mm 2 / s, by 1 The methyl index determined by H-NMR was 118%.
[0261] The obtained polymer was a semi-solid state that was turbid and grease-like and had no fluidity, and was a polymer with significantly poor handling properties. Therefore, it was considered that it could be confirmed that the copolymer (b-3) did not have sufficient performance as a plasticizer for the thermoplastic resin required for the present invention, and therefore, in the comparative examples described below, no study using the copolymer (b-3) was conducted.
[0262] The physical property values of the obtained copolymers (b-1), (b-2) and (b-3) are shown in Table 1. In Table 1, the content of the structural unit derived from propylene is expressed as "propylene content".
[0263] [Table 1]
[0264] Copolymer (b-1) Copolymer (b-2) Copolymer (b-3) <![CDATA[Kinematic viscosity (mm 2 / s)]]> 100 102 104 Propylene content (mol%) 70.0 51.2 86.0 Weight average molecular weight (Mw) 4,235 4,172 4,208 Molecular weight distribution (Mw / Mn) 1.7 1.7 1.7 B value 1.2 1.2 1.2 Methyl index (%) 83 54 118
[0265] Polyethylene wax
[0266] As the polyethylene wax, a polyethylene wax produced by the following production method was used.
[0267] [Manufacturing method of polyethylene wax]
[0268] 1. Preparation of Catalyst
[0269] In a glass autoclave with an internal volume of 1.5 liters, 25 g of commercially available anhydrous magnesium chloride was suspended in 500 ml of hexane. While maintaining it at 30°C and stirring, 92 ml of ethanol was added dropwise over 1 hour and the reaction was further reacted for 1 hour. After the reaction was completed, 93 ml of diethylaluminum monochloride was added dropwise over 1 hour and the reaction was further reacted for 1 hour. After the reaction was completed, 90 ml of titanium tetrachloride was added dropwise, the reaction vessel was heated to 80°C, and the reaction was continued for 1 hour. After the reaction was completed, the solid portion was washed with hexane until free titanium could not be detected by decantation. The washed solid was made into a hexane suspension, and the titanium concentration was quantified by titration for the following experiment.
[0270] 2. Manufacture of polyethylene wax
[0271] 930 ml of hexane and 70 ml of propylene were placed in a 2-liter stainless steel autoclave that was fully purged with nitrogen, and hydrogen was introduced until the pressure reached 0.1 MPa (gauge pressure). Then, after the temperature in the system was raised to 170° C., 0.1 mmol of triethylaluminum, 0.4 mmol of sesquiethylaluminum chloride, and a hexane suspension of the solid obtained above were pressed into ethylene in such a manner that the amount of the titanium component was 0.008 mmol in terms of atomic conversion, thereby starting polymerization. Then, the total pressure was maintained at 2.9 MPa (gauge pressure) by continuously supplying only ethylene, and polymerization was carried out at 170° C. for 40 minutes.
[0272] After the polymerization was stopped by adding a small amount of ethanol into the system, the unreacted ethylene and propylene were purged. The obtained polymer solution was dried under reduced pressure at 100°C overnight to obtain polyethylene wax. The obtained polyethylene wax had a density of 926 kg / m 3 , weight average molecular weight (Mw): 10,270, molecular weight distribution (Mw / Mn): 2.8, melting point: 109°C.
[0273] [Example 1 and Example 2]
[0274] [T-mold molding]
[0275] A T-die with a die width of 150 mm was installed on a 20 mmφ single screw extruder (manufactured by Toyo Seiki Seisaku-sho, Ltd., D2020), the rotation speed was set to 25 rpm, and the barrel temperature and die temperature were set to 205° C. Thermoplastic resin (a) was added from the feed hopper. Separately, copolymer (b-1) was continuously fed from a plunger-type metering pump having an extended nozzle at the outlet of the feed hopper in a manner to obtain a 50 μm thick film by extrusion film molding.
[0276] [Comparative Example 1]
[0277] A 50 μm-thick film was obtained in the same manner as in Example 1 except that the copolymer (B) was not blended.
[0278] [Comparative Example 2]
[0279] A 50 μm-thick film was obtained in the same manner as in Example 1 except that the copolymer (b-1) in Example 1 was changed to the copolymer (b-2).
[0280] [Comparative Example 3]
[0281] Before film molding, the thermoplastic resin (a) and the polyethylene wax were dry-blended in accordance with the formulation shown in Table 2, and a 50 μm thick film was obtained in the same manner as in Example 1 without blending the copolymer (B).
[0282] The resin compositions or films obtained in the above Examples and Comparative Examples were subjected to measurement of extrusion torque, discharge volume, tensile breaking strength, tensile breaking elongation, tensile tensile product, and evaluation of film appearance by the following methods.
[0283] [Extrusion torque]
[0284] The resin is put into the feed hopper, and 10 minutes after the extruder is set to the aforementioned molding conditions, the torque value displayed by the extruder is measured for 1 minute, and the value is obtained from the average value. If the value is small, even when the extrusion torque is biased to the increased side during molding, it is difficult to reach the upper limit of the device capacity, so it is easy to reduce the unevenness of the ejection amount during molding. In addition, if the value is small, when the screw speed of the extruder is increased, it is difficult to reach the upper limit of the device capacity, so the adjustment of the ejection amount becomes easy.
[0285] [Discharge volume]
[0286] The resin was fed from the hopper, and the extruder was set to the above-mentioned molding conditions. The mass of the film molded in 1 minute was measured 10 minutes later, and the discharge amount per hour was calculated from the value.
[0287] [Tensile breaking strength, tensile breaking elongation, tensile tensile product]
[0288] According to JIS K7127, the strength and elongation of the film at which the film breaks are measured in the mechanical direction, and are respectively referred to as the tensile breaking strength and the tensile breaking elongation. In addition, the product of the tensile breaking strength and the tensile breaking elongation is referred to as the tensile tensile product. The larger the value, the harder the obtained film is to break. In particular, if the value is 30,000 MPa·% or more, it indicates that the film is strong in terms of fracture resistance.
[0289] [Film appearance]
[0290] The appearance of the obtained film was evaluated by visual observation of the surface and touch. The film was evaluated as "with exudation" when an oily substance that was sticky when touched was confirmed to float on the film surface, and the film was evaluated as "without exudation" when no oily substance that was sticky when touched was confirmed to float on the film surface.
[0291] 1 Table 2]
[0292]
Claims
1. A resin composition comprising 25 to 99.99% by mass of a thermoplastic resin (A) having a weight average molecular weight (Mw) of 50,000 or more in terms of polystyrene as measured by gel permeation chromatography (GPC), and 0.01 to 15% by mass of a copolymer (B) containing a structural unit derived from an α-olefin having 3 or more carbon atoms, wherein the copolymer (B) satisfies the following requirements (b-1) to (b-3): (b-1) Kinematic viscosity at 100°C is 10 to 5,000 mm 2 / s, the kinematic viscosity at 100°C is measured based on ASTM D 445; (b-2) the content of structural units derived from α-olefins having 3 or more carbon atoms is in the range of 60 to 85 mol%; (b-3) a weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography (GPC) of 1,000 to 30,000, and a molecular weight distribution (Mw / Mn) of 2.5 or less, in, The thermoplastic resin (A) is polypropylene, and the copolymer (B) is a propylene-ethylene copolymer.
2. The resin composition according to claim 1, in, The content of the thermoplastic resin (A) is 90 to 99.99% by mass, and the content of the copolymer (B) is 0.01 to 10% by mass.
3. The resin composition according to claim 1, in, The thermoplastic resin (A) has an MFR of 0.1 to 60 g / 10 minutes, where the MFR is measured at 230° C. and a test load of 2.16 kgf in accordance with JIS K 7210.
4. The resin composition according to claim 1, in, The thermoplastic resin (A) has an MFR of 0.3 to 10 g / 10 minutes, where the MFR is measured at 230° C. and a test load of 2.16 kgf in accordance with JIS K 7210.
5. The resin composition according to claim 1, in, The kinematic viscosity of the copolymer (B) at 100°C is 10 to 3,500 mm 2 / s, and the kinematic viscosity at 100°C is measured based on ASTM D 445.
6. The resin composition according to claim 1, in, The kinematic viscosity of the copolymer (B) at 100°C is 50 to 700 mm 2 / s, and the kinematic viscosity at 100°C is measured based on ASTM D 445.
7. The resin composition according to claim 1, in, The copolymer (B) has a polystyrene-equivalent weight average molecular weight (Mw) of 1,700 to 20,000 as measured by gel permeation chromatography (GPC).
8. The resin composition according to claim 1, in, The molecular weight distribution of the copolymer (B) measured by gel permeation chromatography (GPC), that is, Mw / Mn, is 2.1 or less.
9. The method for producing the resin composition according to claim 1, comprising the following steps: Step (1), implementing the following method (α) to obtain, as the copolymer (B), a copolymer (B) that further satisfies the following requirements (b-4) and (b-5), and Step (2), melt-kneading the thermoplastic resin (A), the copolymer (B) and optional additives to obtain a resin composition; (b-4) 1 The methyl index measured by H-NMR is in the range of 60 to 130%. (b-5) when differential scanning calorimetry (DSC) is performed in the temperature range of -100°C to 150°C, no melting peak is observed, Method (α): A method comprising the step of solution polymerizing ethylene and an α-olefin having 3 or more carbon atoms in the presence of the following catalyst system, The catalyst system comprises: a bridged metallocene compound (a) represented by the following formula 1, and at least one compound (b) selected from the group consisting of an organoaluminum oxy-compound (b1) and a compound (b2) that reacts with the bridged metallocene compound (a) to form an ion pair, [Chemical formula 1] In formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 Each is independently a hydrogen atom, a hydrocarbon group or a silicon-containing hydrocarbon group, and multiple adjacent groups may be connected to each other to form a ring structure. R 6 and R 11 are the same groups as each other, being hydrogen atoms, hydrocarbon groups or silicon-containing hydrocarbon groups, R 7 and R 10 are the same groups as each other, being hydrogen atoms, hydrocarbon groups or silicon-containing hydrocarbon groups, R 6 and R 7 It can be bonded with hydrocarbons having 2 to 3 carbon atoms to form a ring structure. R 10 and R 11 It can be bonded with hydrocarbons having 2 to 3 carbon atoms to form a ring structure. R 6 , R 7 , R 10 and R 11 Not all hydrogen atoms at the same time; Y is a carbon atom or a silicon atom; R 13 and R 14 are each independently aryl; M is Ti, Zr or Hf; Q is independently a halogen atom, a hydrocarbon group, an anionic ligand or a neutral ligand capable of coordinating a lone pair of electrons; j is an integer from 1 to 4.
Citation Information
Patent Citations
Production of liquid alpha-olefin copolymer
JP1986221207A
Catalysts, these catalysts and production of these catalyst polymerization process
JP1989501950A
Production of low-molecular weight copolymer
JP1990001163B2
Synthetic lubricating oil
JP1990007998B2
Metallocene catalyst
JP1991179005A