Semiconductor devices and their manufacturing methods
By using a rapid thermal annealing process in semiconductor device manufacturing to form a uniform tunnel barrier layer, the problems of uneven crystal growth and metal atom diffusion caused by high-temperature and long-term heat treatment are solved, thereby improving TMR characteristics and reducing resistance characteristics.
Patent Information
- Application Number
- CN202211557074.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-12-07
- Filing Date
- 2022-12-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-12-06
AI Technical Summary
In existing semiconductor device manufacturing technologies, high-temperature and long-term heat treatment leads to uneven crystal growth in the tunnel barrier layer, resulting in poor TMR characteristics of the MTJ structure, and the mixed diffusion of interlayer metal atoms causes a deterioration in resistance characteristics.
Rapid thermal annealing (RTA) is employed to form a uniform tunnel barrier layer by repeatedly forming thin material layers and crystallizing them in a short time. This reduces the mixing and diffusion of metal atoms between layers and improves the crystallinity of the tunnel barrier layer.
The TMR characteristics of the MTJ structure were improved, the RA value was reduced, the resistance characteristics of the variable resistor element were improved, and the characteristic degradation caused by heat treatment was reduced.
Smart Images

Figure CN116249430B_ABST
Abstract
Description
[0001] Cross-reference to related applications
[0002] This application claims priority to Korean Patent Application No. 10-2021-0174229, filed on December 7, 2021, the entirety of which is incorporated herein by reference. Technical Field
[0003] Several embodiments of the present invention relate to storage circuits or storage devices and their application in electronic devices or electronic systems. Background Technology
[0004] Recent trends in the electrical and electronics industry toward miniaturization, low power consumption, high performance, and multifunctionality have prompted semiconductor manufacturers to focus on high-performance, high-capacity semiconductor devices. Examples of such high-performance, high-capacity semiconductor devices include memory devices capable of storing data by switching between different resistance states based on applied voltage or current. Semiconductor devices can include RRAM (resistive random access memory), PRAM (phase-change random access memory), FRAM (ferroelectric random access memory), MRAM (magnetic random access memory), and electronic fuses (E-fuse). Summary of the Invention
[0005] Various embodiments of the present invention include storage circuits or storage devices and their application in semiconductor devices or semiconductor systems, as well as various implementations of semiconductor devices that can improve the performance of semiconductor devices.
[0006] According to one embodiment, the semiconductor device may include a magnetic tunnel junction (MTJ) structure having a free layer, a fixed layer, and a tunnel blocking layer, wherein the free layer has a variable magnetization direction, the fixed layer has a fixed magnetization direction, and the tunnel blocking layer is interposed between the free layer and the fixed layer, and includes multiple material layers having a thickness of two monolayers or less, wherein each material layer is individually crystallized.
[0007] According to another embodiment, a method for manufacturing a semiconductor device may include: forming a first magnetic layer on a substrate; forming a tunnel barrier layer on the first magnetic layer by repeatedly performing a cell process for forming a material layer and performing a rapid thermal annealing (RTA) process on the material layer; and forming a second magnetic layer on the tunnel barrier layer. Attached Figure Description
[0008] Figure 1A and Figure 1B This is a cross-sectional view showing a method for forming a variable resistive element according to a comparative example.
[0009] Figure 2This is a cross-sectional view illustrating an example of a variable resistance element according to an embodiment of the present invention.
[0010] Figures 3A to 3E This is a cross-sectional view illustrating an example of a method for forming a semiconductor device according to another embodiment of the present invention.
[0011] Figures 4A to 4F This is a cross-sectional view illustrating an example of a method for forming a tunnel barrier layer according to yet another embodiment of the present invention.
[0012] Figure 5 The graphs show the magnetoresistance (MR) and exchange coupling field (Hex) characteristics of a variable resistive element according to another embodiment and comparative example of the present invention.
[0013] Figure 6 This is a cross-sectional view illustrating an example of a semiconductor device according to another embodiment of the present invention and a method for forming the semiconductor device.
[0014] Figure 7 This is a cross-sectional view illustrating yet another embodiment of a semiconductor device according to the present invention, and another example of a method for forming the semiconductor device. Specific Implementation
[0015] The various embodiments described herein can be described with reference to sectional views, plan views, and block diagrams, which are ideal schematic diagrams of specific embodiments according to the invention. It is worth noting that the structure of the drawings may be modified due to manufacturing processes and / or manufacturing tolerances. The invention is not limited to the described embodiments and the specific structures shown in the drawings, but may instead include other embodiments or modifications of the described embodiments, including any structural changes caused by manufacturing process requirements. Therefore, the areas shown in the drawings are schematic, and the shapes of the areas shown in the drawings are intended to illustrate the specific structure of the areas of the elements, and are not intended to limit the scope of the invention.
[0016] Before explaining the embodiments of the present invention, comparative examples will be described.
[0017] Figure 1A and Figure 1B This is a cross-sectional view showing a method for forming a variable resistive element according to a comparative example.
[0018] refer to Figure 1A According to the comparative example, the variable resistor element 1 can be an MRAM including an MTJ structure having a free layer 12, a tunnel blocking layer 13, and a fixed layer 14. One type of MRAM is a spin torque conversion MRAM (STT-MRAM) including an MTJ structure, and the change in the magnetization direction of the free layer 12 is based on the spin conversion torque.
[0019] The free layer 12 can have a variable magnetization direction that allows the MTJ structure to have a variable resistance value. The free layer 12 can also be referred to as a storage layer.
[0020] The fixed layer 14 can have a fixed magnetization direction, which remains unchanged when the magnetization direction of the free layer 12 changes. For this reason, the fixed layer 14 can be referred to as the reference layer.
[0021] Depending on the voltage or current applied to the variable resistive element 1, the magnetization direction of the free layer 12 can be changed by spin-commutation torque. When the magnetization directions of the free layer 12 and the fixed layer 14 are parallel to each other, the variable resistive element 1 can be in a low-resistance state, which can indicate a digital data bit "0". Conversely, when the magnetization directions of the free layer 12 and the fixed layer 14 are opposite to each other, the variable resistive element 1 can be in a high-resistance state, which can indicate a digital data bit "1". That is, the variable resistive element 1 can serve as a storage unit to store digital data bits based on the orientation of the free layer 12.
[0022] The tunneling barrier layer 13 can allow electrons to tunnel through and change the magnetization direction of the free layer 12. The tunneling barrier layer 13 may include an insulating oxide.
[0023] The variable resistance element 1 may also include multiple layers for improving the characteristics of the MTJ structure. For example, the variable resistance element 1 may also include a buffer layer 11 disposed beneath the MTJ structure.
[0024] A buffer layer 11 can be disposed below the free layer 12 to improve the vertical magnetocrystalline anisotropy of the free layer 12. Alternatively, the buffer layer 11 can promote crystal growth of the layer disposed on the buffer layer 11. Alternatively, the buffer layer 11 can resolve the lattice constant mismatch between the bottom electrode and the layer disposed on the buffer layer 11.
[0025] The switching of the magnetization direction of free layer 12 can be affected by tunnel magnetoresistance (TMR). MRAM cells with high TMR can have high read signals that can increase the read speed of MRAM cells during operation.
[0026] Generally, compared to MTJs with structural defects, MTJs with a uniform crystal structure and no microstructural defects in the layers they comprise can have a higher TMR. Therefore, TMR can be increased by maximizing coherent tunneling through the tunnel barrier layer 13 and the free layer 12 and fixed layer 14 disposed on and below the tunnel barrier layer 13.
[0027] Therefore, the free layer 12, tunnel barrier layer 13, and fixed layer 14 can be crystallized by applying heat treatment to the material layers used to form the free layer 12, tunnel barrier layer 13, and fixed layer 14. The heat treatment for crystal growth of the free layer 12, tunnel barrier layer 13, and fixed layer 14 can be performed at high temperatures for an extended period. The heat treatment can be performed in a furnace. The total time for heat treatment in the furnace (including the heat treatment itself, which takes several tens of minutes at the crystallization temperature, as well as the heating process before and the cooling process after the heat treatment) can take several hours. When performing such high-temperature and long-duration heat treatment, the total heat budget applied to the MTJ is very high, and therefore the layers included in the MTJ and the layers located beneath the MTJ may be affected.
[0028] like Figure 1A As shown, the mixing and diffusion of metal atoms included in the buffer layer 11 and the free layer 12 can occur between the buffer layer 11 and the free layer 12. Therefore, particles 12' comprising metal atoms originating from the free layer 12 can exist in the buffer layer 11 adjacent to the interface between the buffer layer 11 and the free layer 12, and particles 11' comprising metal atoms originating from the buffer layer 11 can exist in the free layer 12 adjacent to the interface between the buffer layer 11 and the free layer 12. The mixing and diffusion of metal atoms between the layers included in the variable resistor element 1 can degrade the characteristics of the variable resistor element 1.
[0029] Furthermore, defects may occur in the internal structure of the tunnel barrier layer 13, which is crystallized through prolonged heat treatment at high temperatures. For example... Figure 1A As shown, the tunnel barrier layer 13 may have an inhomogeneous crystal structure with crystallization defects generated by long-term heat treatment at high temperatures.
[0030] Reference Figure 1B The problems in crystal growth of tunnel barrier layer 13 caused by high temperature and long duration heat treatment are described again.
[0031] refer to Figure 1B Since the tunnel barrier layer 13 is formed by forming a material layer 13A as a monolayer and then crystallizing the material layer 13A through high-temperature and long-term heat treatment, the crystal growth and orientation of the tunnel barrier layer 13 can become non-uniform. Therefore, the tunnel barrier layer 13 has crystallization defects and an inhomogeneous crystal structure, which deteriorates the TMR characteristics of the variable resistor element 1.
[0032] Therefore, embodiments of the present invention can provide semiconductor devices and methods for manufacturing thereof that can improve the crystallinity of the tunnel blocking layer of MTJ and reduce or minimize interlayer mixing and diffusion, thereby improving the characteristics of variable resistance elements.
[0033] Figure 2This is a cross-sectional view illustrating an example of a variable resistance element according to an embodiment of the present invention.
[0034] refer to Figure 2 The variable resistor element 100 may include an MTJ structure, which includes a free layer 104 having a variable magnetization direction, a fixed layer 106 having a fixed magnetization direction, and a tunnel blocking layer 105 inserted between the free layer 104 and the fixed layer 106.
[0035] In the MTJ structure, the free layer 104 can have one of a different magnetization direction or one of a different electron spin direction to switch the polarity of the free layer 104, thereby causing a change in the resistance value. In some embodiments, the polarity of the free layer 104 is changed or flipped according to a voltage or current signal applied to the MTJ structure (e.g., a drive current exceeding a certain threshold). Due to the change in the polarity of the free layer 104, the free layer 104 and the fixed layer 106 have different magnetization directions or different electron spin directions, which allows the variable resistive element 100 to store different data or represent different data bits. The free layer 104 can also be referred to as a storage layer. The magnetization direction of the free layer 104 can be substantially perpendicular to the surfaces of the free layer 104, the tunnel blocking layer 105, and the fixed layer 106. In other words, the magnetization direction of the free layer 104 can be substantially parallel to the stacking direction of the free layer 104, the tunnel blocking layer 105, and the fixed layer 106. Therefore, the magnetization direction of the free layer 104 can vary between the downward and upward directions. The change in the magnetization direction of the free layer 104 can be caused by the spin-commutation torque generated by the applied current or voltage.
[0036] The free layer 104 may have a single-layer or multi-layer structure comprising ferromagnetic materials. For example, the free layer 104 may comprise an alloy based on at least one of Fe, Ni, or Co (e.g., Fe-Pt alloy, Fe-Pd alloy, Co-Pd alloy, Co-Pt alloy, Fe-Ni-Pt alloy, Co-Fe-Pt alloy, Co-Ni-Pt alloy, or Co-Fe-B alloy or others) or may comprise a metal stack (such as Co / Pt or Co / Pd or others).
[0037] In both data read and write operations, the tunnel barrier layer 105 allows electrons to tunnel through. In a write operation for storing new data, a high write current can be directed through the tunnel barrier layer 105 to change the magnetization direction of the free layer 104, and thus alter the resistance state of the MTJ used to write the new data bits. In a read operation, a low read current can be directed through the tunnel barrier layer 105 without changing the magnetization direction of the free layer 104, thereby measuring the existing resistance state of the MTJ under the existing magnetization direction of the free layer 104, and thus reading the data bits stored in the MTJ. The tunnel barrier layer 105 may comprise insulating oxides such as, for example, MgO, CaO, SrO, TiO, VO, NbO, Al2O3, TiO2, Ta2O5, RuO2, B2O3, etc.
[0038] The tunnel barrier layer 105 can ensure a low resistance area product (RA) value and high TMR characteristics to improve the characteristics of the variable resistor element 100.
[0039] TMR can be expressed as the ratio of the difference between the resistance in the antiparallel state (Rap) and the resistance in the parallel state (Rp) to the resistance in the parallel state (Rp). An MTJ with a uniform crystal structure and no structural defects can have a high TMR compared to an MTJ with structural defects. A high TMR is preferred for stable read operations due to the larger signal difference between the on / off states of the higher TMR generation unit. The resistance of the magnetic storage device can vary depending on the thickness T of the tunnel barrier layer 105.
[0040] The resistance (RA) value is a resistance value normalized per unit area and can be expressed as the product of resistance and area. In magnetic storage devices, the RA value can be an important factor in determining the signal-to-noise ratio (SNR) and the RC time constant. The RA value can also be an indicator of the voltage used to reverse the magnetization direction of the free layer 104 (e.g., the threshold switching voltage). As the RA value increases, the cell can use a higher threshold switching voltage, thereby degrading cell performance and shortening cell lifetime. The RA value can be reduced by decreasing the thickness T of the tunnel barrier layer 105. However, when the thickness T of the tunnel barrier layer 105 decreases, the TMR value may also decrease. Therefore, it is impossible to achieve both a low RA value and high TMR performance simply by adjusting the thickness T of the tunnel barrier layer 105.
[0041] According to one embodiment of the present invention, structural defects in the crystal structure of the tunnel blocking layer 105 can be eliminated or minimized, thereby maintaining a low RA value and improving TMR characteristics.
[0042] In several embodiments, the tunnel blocking layer 105 may have a uniform crystal structure with no defects or minimized defects. In some embodiments, the tunnel blocking layer 105 may have a bcc(001) crystal structure. In some embodiments, the tunnel blocking layer 105 may have the same crystal structure as the free layer 104. In some embodiments, both the tunnel blocking layer 105 and the free layer 104 may have a bcc(001) crystal structure.
[0043] In several embodiments, due to the high crystallinity of the tunnel barrier layer 105, coherent tunneling between the free layer 104 and the fixed layer 106 is minimized, thereby improving TMR characteristics and reducing the RA value.
[0044] Reference Figures 3A to 3E as well as Figures 4A to 4F The formation of the uniform crystal structure of the tunnel barrier layer 105 will be described in detail.
[0045] The thickness T of the tunnel barrier layer 105 can be such that the RA value is 20Ωμm. 2 Or within a smaller range. As mentioned above, when the thickness T of the tunnel blocking layer 105 decreases, the RA value decreases, the TMR decreases, and the characteristics of the variable resistor element 100 may deteriorate. Therefore, the thickness T of the tunnel blocking layer 105 can be set such that the variable resistor element 100 exhibits optimal characteristics due to a low RA value and a high TMR value.
[0046] When the tunnel barrier layer 105 has a thickness T such that the RA value is greater than 20Ωμm 2 At this point, the resistance becomes too high, making the variable resistance element 100 difficult to operate. The lower limit of the thickness T of the tunnel blocking layer 105 can be within a range so that the characteristics of the variable resistance element 100 do not deteriorate due to the RA and TMR values.
[0047] The fixed layer 106 may have a fixed magnetization direction that remains unchanged when the magnetization direction of the free layer 104 changes. The fixed layer 106 may be referred to as a reference layer. In some embodiments, the magnetization direction of the fixed layer 106 may be fixed in a downward direction. In some embodiments, the magnetization direction of the fixed layer 106 may be fixed in an upward direction.
[0048] The fixing layer 106 may have a single-layer or multi-layer structure comprising ferromagnetic materials. For example, the fixing layer 106 may comprise an alloy based on at least one of Fe, Ni, or Co (e.g., Fe-Pt alloy, Fe-Pd alloy, Co-Pd alloy, Co-Pt alloy, Fe-Ni-Pt alloy, Co-Fe-Pt alloy, Co-Ni-Pt alloy, or Co-Fe-B alloy) or may comprise a metal stack (such as Co / Pt or Co / Pd or others).
[0049] When a voltage or current is applied to the variable resistor element 100, the magnetization direction of the free layer 104 can change due to spin-commutation torque. In some embodiments, when the magnetization directions of the free layer 104 and the fixed layer 106 are parallel to each other, the variable resistor element 100 can be in a low-resistance state, which can indicate a digital data bit "0". Conversely, when the magnetization directions of the free layer 104 and the fixed layer 106 are antiparallel to each other, the variable resistor element 100 can be in a high-resistance state, which can indicate a digital data bit "1". In some embodiments, the variable resistor element 100 can be configured to store a data bit "1" when the magnetization directions of the free layer 104 and the fixed layer 106 are parallel to each other and to store a data bit "0" when the magnetization directions of the free layer 104 and the fixed layer 106 are antiparallel to each other.
[0050] The variable resistance element 100 may also include one or more layers that perform multiple functions to improve the characteristics of the MTJ structure. For example, the variable resistance element 100 may also include at least one of a buffer layer 102, a lower layer 103, a spacer layer 107, a magnetic correction layer 108, and a cover layer 109.
[0051] Buffer layer 102 can be disposed below lower layer 103 to promote crystal growth of lower layer 103, thereby improving the perpendicular magnetocrystalline anisotropy of free layer 104. Buffer layer 102 can have a single-layer or multi-layer structure comprising, for example, metals, metal alloys, metal nitrides, or metal oxides, or combinations thereof. Moreover, buffer layer 102 can be formed of, for example, a material compatible with the bottom electrode, or include such a material to resolve the lattice constant mismatch between the bottom electrode and lower layer 103. For example, buffer layer 102 may include tantalum (Ta).
[0052] The lower layer 103 may be disposed below the free layer 104 and is used to improve the perpendicular magnetocrystalline anisotropy of the free layer 104. The lower layer 103 may have a single-layer or multi-layer structure comprising, for example, a metal, a metal alloy, a metal nitride, or a metal oxide, or a combination thereof. In some embodiments, the lower layer 103 may include a single-layer or multi-layer structure having a metal nitride. For example, the lower layer 103 may include one or more of, for example, TaN, AlN, SiN, TiN, VN, CrN, GaN, GeN, ZrN, NbN, MoN, or HfN.
[0053] In embodiments, the mixing or diffusion of atoms between the buffer layer 102 and the lower layer 103 and the free layer 104 can be prevented or minimized. Typically, crystallization of the layers included in the MTJ may require high-temperature and long-duration heat treatment, which may also affect the buffer layer 102 and the lower layer 103 disposed beneath the MTJ. As a result, metal atoms in the buffer layer 102 and the lower layer 103 can diffuse into the free layer 104, and metal atoms in the free layer 104 can diffuse into the buffer layer 102 and the lower layer 103. However, in several embodiments, the amount of heat exposure to the buffer layer 102 and the lower layer 103 during heat treatment can be minimized by utilizing specific heat treatment conditions (described below). Therefore, the mixing or diffusion of atoms between the buffer layer 102 and the lower layer 103 and the free layer 104 can be prevented or minimized. Therefore, the buffer layer 102, the lower layer 103, and the free layer 104 can have a uniform crystal structure and uniform configuration, thereby minimizing the degradation of the characteristics of the variable resistor element 100. (Refer to...) Figures 3A to 3E and Figures 4A to 4F The method of preventing the mixing or diffusion of atoms between the buffer layer 102 and the lower layer 103 and the free layer 104 through special heat treatment is described in detail.
[0054] Spacer 107 can be inserted between magnetic correction layer 108 and fixing layer 106, and spacer 107 can act as a buffer between magnetic correction layer 108 and fixing layer 106. Spacer 107 can be used to improve the characteristics of magnetic correction layer 108. Spacer 107 can include, for example, a noble metal, such as ruthenium (Ru).
[0055] The magnetic correction layer 108 can be used to counteract the effects of stray magnetic fields caused by the fixed layer 106. In this case, the effects of the stray magnetic field of the fixed layer 106 can be reduced, and therefore the bias magnetic field in the free layer 104 can be reduced. The magnetic correction layer 108 may have a magnetization direction that is antiparallel to the magnetization direction of the fixed layer 106. In an embodiment, when the fixed layer 106 has a downward magnetization direction, the magnetic correction layer 108 may have an upward magnetization direction. Conversely, when the fixed layer 106 has an upward magnetization direction, the magnetic correction layer 108 may have a downward magnetization direction. The magnetic correction layer 108 may be exchange-coupled with the fixed layer 106 through the spacer layer 107 to form a synthetic antiferromagnetic (SAF) structure. The magnetic correction layer 108 may have a single-layer or multi-layer structure comprising ferromagnetic materials.
[0056] In one embodiment, the magnetic correction layer 108 is located above the fixed layer 106; however, the magnetic correction layer 108 can be disposed at different locations. For example, when the magnetic correction layer 108 is patterned to be spaced apart from the MTJ structure, the magnetic correction layer 108 can be located above, below, or adjacent to the MTJ structure.
[0057] The capping layer 109 can be used to protect the variable resistor element 100 and / or serve as a hard mask for patterning the variable resistor element 100. In some embodiments, the capping layer 109 may include a variety of conductive materials, such as metals. In some embodiments, the capping layer 109 may include, for example, a metallic material with few or no pinholes, and the capping layer 109 has high tolerance to wet etching and / or dry etching. In some embodiments, for example, the capping layer 109 may include, for example, metals, nitrides, or oxides, or combinations thereof. For example, the capping layer 109 may include noble metals, such as ruthenium (Ru).
[0058] The capping layer 109 may have a single-layer or multi-layer structure. In some embodiments, the capping layer 109 may have a multi-layer structure comprising oxides or metals or combinations thereof. For example, the capping layer 109 may have a multi-layer structure comprising an oxide layer, a first metal layer, and a second metal layer.
[0059] A material layer used to address the lattice structure differences and lattice constant mismatch between the fixed layer 106 and the magnetic correction layer 108 can be interposed between the fixed layer 106 and the magnetic correction layer 108. For example, such a material layer can be amorphous and can include metals, metal nitrides, or metal oxides.
[0060] The variable resistance element 100 according to the embodiment described above can improve TMR characteristics and RA value through a tunnel barrier layer 105 having a uniform crystal structure and minimized crystal defects. Furthermore, according to the variable resistance element 100, each layer can have a uniform structure and uniform composition because atomic mixing or diffusion between the buffer layer 102 and the lower layer 103 and the free layer 104 can be prevented or minimized, thereby preventing deterioration of the characteristics of the variable resistance element 100.
[0061] Reference Figures 3A to 3E An example of a method for forming a semiconductor device according to an embodiment of the present invention is described. Figure 2 The illustrated embodiments describe a detailed description of the variable resistance element.
[0062] Figures 3A to 3E This is a cross-sectional view illustrating an example of a method for forming a semiconductor device according to an embodiment of the present invention.
[0063] refer to Figure 3A The buffer layer 102 and the lower layer 103 can be sequentially formed on the substrate 101 having a predetermined structure.
[0064] Substrate 101 may include a semiconductor substrate. Substrate 101 may be formed of a silicon-containing material. Substrate 101 may include, for example, silicon, monocrystalline silicon, polycrystalline silicon, amorphous silicon, silicon-germanium, monocrystalline silicon-germanium, polycrystalline silicon-germanium, carbon-doped silicon, combinations thereof, or multilayers thereof. Substrate 101 may include another semiconductor material, such as germanium. Substrate 101 may include a group III / V semiconductor substrate, such as a chemical compound semiconductor substrate, such as gallium arsenide (GaAs). Substrate 101 may include a silicon-on-insulator (SOI) substrate.
[0065] The predetermined structure formed on the substrate 101 may include switching elements, contact plugs, etc. The switching elements may be coupled with variable resistor elements (see...). Figure 2 The reference numeral 100 is connected and used to control the bias voltage applied to the variable resistor element 100. The switching element may include one or more transistors, diodes, or a combination of transistors and diodes. The switching element may be electrically connected to a contact plug in one part of the switching element and electrically connected to a wire (e.g., a source wire) in another part of the switching element.
[0066] like Figure 3A As shown, the material layer 104A used to form the free layer can be formed on the lower layer 103.
[0067] Material layer 104A can be transformed through crystallization. Figure 3B The free layer 104 is a layer. The material layer 104A can be amorphous.
[0068] refer to Figure 3B Material layer 104A can be crystallized to form free layer 104. Tunnel blocking layer 105 can be formed on free layer 104.
[0069] In several embodiments, the tunnel barrier layer 105 can be formed by performing a process of repeatedly forming a unit material layer of thin thickness, and then crystallizing the layer by performing N rapid thermal annealing (RAT).
[0070] Reference Figures 4A to 4F The formation of the tunnel barrier layer 105 will be described in detail.
[0071] refer to Figure 4A The first material layer 105A-1 can be formed on the material layer 104A.
[0072] The first material layer 105A-1 may be a unit material layer for forming the tunnel barrier layer 105 and includes insulating oxides, such as, for example, MgO, CaO, SrO, TiO, VO, NbO, Al2O3, TiO2, Ta2O5, RuO2, B2O3, etc.
[0073] The first material layer 105A-1 can be amorphous.
[0074] In some embodiments, the thickness T1 of 105A-1 can be in the range of two monolayers or less. The thickness T1 of the first material layer 105A-1 can preferably be thin enough to form a sufficiently uniform structure without crystallization defects by the RTA process. When the first material layer 105A-1 has a thickness greater than two monolayers, crystallization defects may occur during crystallization, and therefore the first material layer 105A-1 may have an inhomogeneous crystal structure.
[0075] Then, the RTA process can be performed on the first material layer 105A-1.
[0076] In several embodiments, the crystallization of the layers included in a conventional MTJ can be efficiently achieved by an RTA process that performs the heat treatment in a relatively short time, compared to the conventional high-temperature and long-duration heat treatment used for crystallization of layers included in a conventional MTJ.
[0077] In some embodiments of the present invention, the RTA process can be performed at a temperature of 600°C or lower. The temperature of the RTA process can be selected taking into account both the crystallinity of the first material layer 105A-1 and the deterioration of the characteristics of the variable resistance element 100. When the RTA process is performed at a temperature above 600°C, the first sublayer (see...) Figure 4B The crystallization of the first material layer 105A-1 (as indicated by reference numeral 105-1) can be improved, but the layer below the first material layer 105A-1 may be affected, thereby deteriorating the properties of that layer. When the RTA process is performed at too low a temperature, sufficient energy may not be applied for the crystallization of the first material layer 105A-1, resulting in poor crystallinity of the first sublayer 105-1. Therefore, the lower limit of the temperature for performing the RTA process can be the temperature at which the first material layer 105A-1 can crystallize.
[0078] In some embodiments, the RTA process can be performed for one minute or less. Since minimizing the heat treatment time for crystallization of the first material layer 105A-1 is important, the RTA process can be performed for the shortest possible time during which the first material layer 105A-1 can crystallize. When the RTA process is performed for more than one minute, the heat exposure to the layer disposed beneath the material layer 105A-1 may increase, thereby deteriorating the properties of that layer. The lower limit for performing the RTA process can be the time during which the first material layer 105A-1 can crystallize.
[0079] refer to Figure 4BA first sublayer 105-1, having a very thin thickness T1 of two monolayers or less, can be formed by forming a first material layer 105A-1 as a unit material layer and performing an RTA process. As defined below, a unit material layer crystallized by the RTA process of the present invention is referred to herein as "solidly crystallized". A separately crystallized material layer does not have material from adjacent layers that diffuses into or mixes with the separately crystallized material layer.
[0080] Since the first material layer 105A-1 can be formed as a relatively thin layer T1 with two monolayers or less and the heat treatment can be performed in a very short time by the RTA process, the first sublayer 105-1 can have a uniform crystal structure without crystallization defects.
[0081] refer to Figure 4C The second material layer 105A-2 can be formed on the first sublayer 105-1 and can be subjected to RTA process.
[0082] The second material layer 105A-2 may include the same material as the first material layer 105A-1. In some embodiments, the second material layer 105A-2 may include insulating oxides, such as, for example, MgO, CaO, SrO, TiO, VO, NbO, Al2O3, TiO2, Ta2O5, RuO2, B2O3, etc.
[0083] The second material layer 105A-2 may have a thickness T2 of two monolayers or less. The thickness T2 of the second material layer 105A-2 may be the same as or different from the thickness T1 of the first material layer 105A-1.
[0084] The conditions for the RTA process applied to the second material layer 105A-2 are within the scope used to describe the RTA process applied to the first material layer 105A-1. The conditions for the RTA process applied to the second material layer 105A-2 may be the same as or different from the conditions for the RTA process applied to the first material layer 105A-1.
[0085] refer to Figure 4D A second sublayer 105-2 with a relatively thin thickness T2 of two monolayers or less can be formed on top of the first sublayer 105-1 by forming a second material layer 105A-2 and performing an RTA process.
[0086] Since the second sublayer 105-2 can be formed as a thinner layer T2 with two monolayers or less, and the heat treatment can be performed in a relatively short time by the RTA process compared to conventional heat treatment, the second sublayer 105-2 can be effectively crystallized to have a uniform crystal structure without crystallization defects.
[0087] exist Figure 4D In the first sublayer 105-1, there is an interface between the first sublayer 105-1 and the second sublayer 105-2. However, in another embodiment, the interface between the first sublayer 105-1 and the second sublayer 105-2 may not be clearly presented, and the first sublayer 105-1 and the second sublayer 105-2 may exist in a merged form.
[0088] refer to Figure 4E The first sublayer 105-1, the second sublayer 105-2, ..., the Nth sublayer 105-N may be formed by performing a unit cycle of forming a unit material layer and performing the RTA process N times.
[0089] The first sublayer 105-1, the second sublayer 105-2, ..., the Nth sublayer 105-N can form a tunnel blocking layer 105. In some embodiments, interfaces may exist between the sublayers. In some embodiments, the interfaces between the sublayers may not be clearly presented and may exist in a merged form.
[0090] The sum of the thicknesses of the sublayers (T1+T2+…TN) can correspond to the thickness T of the tunnel barrier layer 105.
[0091] refer to Figure 4F The tunnel barrier layer 105 with a uniform crystal structure can be formed by the method described above.
[0092] The thickness T of the tunnel barrier layer 105 can be such that the RA value is 20Ωμm. 2 Or within a smaller range.
[0093] and Figures 4A to 4F Similarly, the free layer 104 can be formed by crystallizing the material layer 104A during the formation of the tunnel barrier layer 105. The crystallization of the material layer 104A can be achieved after all N RTA processes, or during a portion of the N RTA processes.
[0094] In one embodiment, since the RTA process for crystallization can be performed in the shortest possible time, the heat exposure of the buffer layer 102 and the lower layer 103 can be reduced, thereby preventing or minimizing the impact on the buffer layer 102 and the lower layer 103. Therefore, the mixing or diffusion of atoms between the buffer layer 102 and the lower layer 103 and the free layer 104 can be prevented, allowing each layer to have a uniform structure and uniform composition. As a result, the deterioration of the characteristics of the variable resistor element 100 due to mixing or diffusion can be prevented.
[0095] Refer again Figure 3B The tunnel barrier layer 105 can be formed on the free layer 104.
[0096] The tunnel barrier layer 105 can have a uniform crystal structure without crystal defects.
[0097] Because it can prevent the mixing or diffusion of atoms between the free layer 104 and the buffer layer 102 and the lower layer 103, the free layer 104 can have a uniform crystal structure.
[0098] In some embodiments, the tunnel blocking layer 105 may have the same crystal structure as the free layer 104. In some embodiments, the tunnel blocking layer 105 and the free layer 104 may have a bcc(001) crystal structure.
[0099] refer to Figure 3C The material layer 106A used to form the fixing layer can be formed on the tunnel barrier layer 105.
[0100] Material layer 106A can be transformed into fixed layer 106 through crystallization. Figure 3D The layer shown is called the 106A material layer. The 106A material layer can be amorphous.
[0101] Then, material layer 106A can be crystallized by performing an annealing process. The annealing process applied to material layer 106A can be performed under the following conditions: material layer 106A can crystallize and the layers disposed below material layer 106A can be unaffected.
[0102] refer to Figure 3D The fixing layer 106 can be formed on the tunnel blocking layer 105.
[0103] refer to Figure 3E The spacer layer 107, the magnetic correction layer 108, and the cover layer 109 can be formed sequentially on the fixed layer 106.
[0104] Subsequently, patterning processes, such as ion beam etching, can be performed to form the variable resistance element 100.
[0105] According to a method for manufacturing the variable resistance element 100 as described above, the tunnel barrier layer 105 can be formed by repeatedly forming a unit material layer with a thickness of two monolayers or less and performing an RTA process. Therefore, the TMR characteristics can be improved and the RA value reduced simultaneously. Furthermore, during heat treatment, the thermal exposure of the layers disposed beneath the tunnel barrier layer 105 can be reduced or minimized, making it possible to prevent the mixing or diffusion of atoms between the buffer layer 102 and the lower layer 103 and the free layer 104. Therefore, layer variation included in the variable resistance element 100 can be reduced or minimized.
[0106] Reference Figure 5 An effect according to an embodiment of the present invention will be described in detail.
[0107] Figure 5 The graphs show the magnetoresistance (MR) and exchange coupling field (Hex) characteristics of a variable resistive element according to an embodiment and comparative example of the present invention.
[0108] exist Figure 5 In this context, "example" means such as Figures 3A to 3E and Figures 4A to 4F The variable resistance element shown is formed using the RTA process, and the “Comparative Example” represents a variable resistance element formed by the following conventional method: forming the layers included in the variable resistance element and crystallizing the layers by performing a high-temperature and long-duration heat treatment in a furnace instead of the RTA process.
[0109] like Figure 5 As shown, in the example case, compared to the comparative example, the Hex0 characteristics exhibit the same level as the comparative example, while the MR characteristics are improved by approximately 13%. That is, according to several embodiments, it is possible to increase the crystallinity of the tunnel barrier layer and to prevent the mixing or diffusion of atoms between the free layer and the layer disposed below the free layer by forming the tunnel barrier layer, wherein the tunnel barrier layer is formed by repeatedly performing a thin unit layer formation and a short-time RTA process instead of the conventional high-temperature and long-time heat treatment. As a result, the characteristics of the variable resistance element can be improved.
[0110] The semiconductor memory device disclosed in this document may include a cell array of variable resistive elements 100. The semiconductor memory may also include multiple components, such as lines, elements, etc., to drive or control each variable resistive element 100. Reference Figures 6 to 7 To describe one of these examples.
[0111] Figure 6 This is a cross-sectional view showing a semiconductor device with a structure manufactured based on some embodiments of the technology disclosed above.
[0112] refer to Figure 6A semiconductor device according to one embodiment may include a substrate 600, lower contacts 620 formed on the substrate 600, corresponding variable resistor elements 100, each formed on a corresponding lower contact 620, and upper contacts 650, each formed on a corresponding variable resistor element 100. For each variable resistor element 100, a specific structure (such as a switch or switching circuit / element), for example, a transistor for controlling access to a particular variable resistor element 100, may be provided on the substrate 600 to control the variable resistor element 100, wherein the switch can be turned on to select the variable resistor element 100 or turned off to not select the variable resistor element 100. Each lower contact 620 may be disposed on the substrate 600 and couples the lower end of the corresponding variable resistor element 100 to a corresponding portion of the substrate 600 (e.g., the drain of a transistor) as a switching circuit for the variable resistor element 100. Each upper contact 650 may be disposed on the corresponding variable resistor element 100 and couples the upper end of the variable resistor element 100 to a line (e.g., a bit line). Figure 6 The image shows two variable resistor elements 100 as examples of elements in an array of variable resistor elements 100, while the number of variable resistor elements 100 can be different.
[0113] A method for manufacturing a device may include a substrate 600 in which transistors are formed. A first interlayer dielectric layer 610 may then be formed over the substrate 600. A lower contact 620 may be formed by selectively etching the first interlayer dielectric layer 610 to form a plurality of spaced holes H, each hole H tunneling through the dielectric layer 610 to expose a corresponding portion of the substrate 600. The holes H may be filled with a conductive material. A variable resistance element 100 may then be formed by forming a material layer for the variable resistance element 100 over the first interlayer dielectric layer 610 and the lower contact 620. The material layer may be selectively etched to form a plurality of variable resistance elements 100. Each of the variable resistance elements 100 may be located on a corresponding lower contact 620. The etching process for forming the variable resistance element 100 may include an ion beam etching (IBE) method with strong physical etching characteristics. A second interlayer dielectric layer 630 may then be formed over the first electrolyte layer 610 to cover the spacing between the variable resistance elements 100. Then, the third electrolyte layer 640 can be formed on the variable resistor element 100 and the second interlayer dielectric layer 630, and then the upper contact 650, which extends through the third electrolyte layer 640 and is coupled to the upper end of the corresponding variable resistor element 100, can be formed using process steps similar to those described above for forming the lower contact 620.
[0114] exist Figure 6In a semiconductor device, all layers forming the variable resistance element 100 can have sidewalls aligned with each other. This is because the variable resistance element 100 is formed using an etching process with a single mask.
[0115] and Figure 6 Unlike other embodiments, a portion of each of the variable resistive elements 100 can be patterned independently of each other. This process... Figure 7 As shown in the image.
[0116] Figure 7 This is a cross-sectional view illustrating a semiconductor device and a method for manufacturing the semiconductor device, based on another embodiment of this disclosure. The following description will focus on... Figure 6 On those different features.
[0117] refer to Figure 7 A semiconductor device according to one embodiment may include a portion of a variable resistance element 100 (e.g., buffer layer 102 and lower layer 103) having sidewalls that are not aligned with the sidewalls of the other layers of the variable resistance element 100. Figure 7 As shown, the buffer layer 102 and the lower layer 103 may have sidewalls aligned with the sidewalls of the lower contact 720.
[0118] Figure 7 The semiconductor devices in the process can be manufactured using the following techniques.
[0119] First, a first interlayer dielectric layer 710 can be formed on the substrate 700 and then selectively etched to form a plurality of holes H penetrating the first interlayer dielectric layer 710 to expose portions of the corresponding substrate 700. Then, a lower contact 720 can be formed by filling only the lower portion of the holes H. For example, the lower contact 720 can be formed by a series of processes including forming a conductive material to cover the resulting structure having the holes formed therein, and removing a portion of the conductive material by an etch-back process until the conductive material has a desired thickness. Then, a buffer layer 102 and a lower layer 103 can be formed to fill the remaining portion of each hole H. For example, the buffer layer 102 can be formed by forming a material layer for forming the buffer layer 102, which covers the resulting structure having the lower contact 720, and then removing a portion of the conductive material by an etch-back process until the conductive material has a desired thickness. The lower layer 103 can be formed by forming a material layer for forming the lower layer 103, which covers the resulting structure formed by the lower contact 720 and the buffer layer 102, and then performing a planarization process, such as CMP (chemical mechanical planarization), until the top surface of the first interlayer dielectric layer 710 is exposed. The remaining portion of the variable resistor element 100 can then be formed by forming a material layer for forming the remaining layers of the variable resistor element 100, excluding the lower contact 720 and the buffer layer 102 and the lower layer 103 above the first interlayer dielectric layer 710.
[0120] Subsequent processes and Figure 6 The processes shown are basically the same.
[0121] In this embodiment, the height required for a single etching to form the variable resistance element 100 can be reduced, which lowers the difficulty level of the etching process.
[0122] Despite Figure 7 In one embodiment, the buffer layer 102 and the lower layer 103 of the variable resistor element 100 are buried in the corresponding holes H, but other parts of the variable resistor element 100 may also be buried as needed.
[0123] Although specific embodiments of the invention have been described, it should be noted that these embodiments are for illustrative purposes and not for limiting the invention. Furthermore, it should be understood that the invention can be implemented in various ways by those skilled in the art through substitutions, alterations, and modifications without departing from the scope of the invention as set forth in the foregoing description.
Claims
1. A semiconductor device, comprising: Magnetic tunnel junction (MTJ) structure, which has The free layer has a variable magnetization direction. A fixed layer having a fixed magnetization direction, and A tunneling barrier layer, interposed between the free layer and the fixed layer, comprises multiple material layers having a thickness of two monolayers or less, wherein each material layer is individually crystallized, wherein the tunneling barrier layer has a resistivity-area product RA value of 20 Ωμm. 2 Or a thickness within a smaller range.
2. The semiconductor device according to claim 1, wherein, The tunnel barrier layer has a uniform crystalline structure.
3. The semiconductor device according to claim 1, wherein, The tunnel barrier layer comprises at least one insulating oxide of the following: MgO, CaO, SrO, TiO, VO, NbO, Al2O3, TiO2, Ta2O5, RuO2, and B2O3.
4. The semiconductor device according to claim 1, wherein, The free layer and the tunnel blocking layer have the same crystal structure.
5. The semiconductor device according to claim 4, wherein, The free layer and the tunnel blocking layer have a bcc (001) crystal structure.
6. The semiconductor device of claim 1 further comprises a buffer layer disposed beneath the MTJ structure and having a uniform composition by suppressing the mixing or diffusion of atoms between the buffer layer and the free layer.
7. A method for manufacturing a semiconductor device, comprising: A first magnetic layer is formed on the substrate; A tunnel barrier layer is formed above the first magnetic layer; as well as A second magnetic layer is formed on top of the tunnel barrier layer. The formation of the tunnel barrier layer includes repeatedly executing a unit process, the unit process comprising: A material layer is formed on top of the first magnetic layer; and The material layer is subjected to a rapid thermal annealing (RTA) process.
8. The method according to claim 7, wherein, The tunnel barrier layer is formed such that the resistivity-area product RA is within 20 Ωμm. 2 Or a thickness within a smaller range.
9. The method according to claim 7, wherein, The material layer is formed to have a thickness of two monolayers or less.
10. The method according to claim 7, wherein, The material layer is amorphous and is crystallized through the RTA process to transform it into a layer with a uniform crystal structure.
11. The method according to claim 7, wherein, The tunnel barrier layer is formed of at least one insulating oxide including MgO, CaO, SrO, TiO, VO, NbO, Al2O3, TiO2, Ta2O5, RuO2, and B2O3.
12. The method according to claim 7, wherein, The RTA process is performed at 600°C or lower for 1 minute or less.
13. The method according to claim 7, wherein, The first magnetic layer is amorphous and is crystallized by the RTA process during the crystallization of the material layer.
14. The method according to claim 7, wherein, The first magnetic layer and the tunnel blocking layer are formed to have the same crystal structure as each other.
15. The method of claim 7, wherein, The first magnetic layer and the tunnel blocking layer are formed to have a bcc (001) crystal structure.
16. The method according to claim 7, wherein, The thickness of each material layer formed in each unit process may be the same or different from each other.
17. The method according to claim 7, wherein, The conditions under which the RTA process is performed in each unit process may be the same or different from each other.
18. The method of claim 7, further comprising forming a buffer layer beneath the first magnetic layer, wherein, The buffer layer has a uniform composition by suppressing the mixing or diffusion of atoms between the buffer layer and the first magnetic layer.
19. The method of claim 7, further comprising crystallizing the second magnetic layer by performing an annealing process.
Citation Information
Patent Citations
Tunnel magnetoresistance device
KR1020090133101A
Memory device
KR1020150121637A
Method of forming metal oxide layer and magnetic memory device including the same
KR1020160056376A