Multi-group modified polysiloxane and preparation method, application and polyurethane foam thereof

By using multi-group modified polysiloxane as a foam stabilizer in polyurethane foam, the problem of cell coarse cells and thermal conductivity increases when bio-based polyols replace petroleum-based polyols is solved, and the application performance of the foam is improved, achieving the realization of the foam. Higher bio-based polyol replacement amount and excellent performance.

CN116253889BActive Publication Date: 2024-12-03JIANGSU MAYSTA CHEM +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310205834.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-06
Publication Date
2024-12-03
Estimated Expiration
2043-03-06

AI Technical Summary

Technical Problem

When bio-based polyols replace traditional polyether polyols, the polyurethane foam has problems such as darker color, thicker surface pore size, decreased thermal conductivity and increased thermal conductivity, resulting in cracking of the foam and unable to completely replace petrochemical-based polyether.

Method used

Using polygroup modified polysiloxane, by adding monoallyl polyoxyethylene ether and double-terminal carbon-containing double bonds to low-hydrogen-containing polysiloxanes as foam stabilizers, Improve the problem of cell coarse and thermal conductivity of bio-based polyols when replacing petroleum-based polyols.

Benefits of technology

Significantly improves the problem of cell coarse and thermal conductivity caused by bio-based polyol replacement of petroleum-based polyol, improves the increase of bio-based polyol, and improves the application performance of polyurethane foam, including reducing the closed cell ratio and compressive strength differences .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The invention discloses a multi-group modified polysiloxane and a preparation method, application and polyurethane foam thereof, and relates to the technical field of polyurethane rigid foam. The multi-group modified polysiloxane is modified by adding monoallyl polyoxyethylene ether and a modifier containing carbon-carbon double bonds at both ends to the conventional allyl polyether for polyether modification of low hydrogen polysiloxane, which can significantly improve the problems of coarse pores and high thermal conductivity caused by partial replacement of petroleum-based polyether polyols by bio-based polyols. Under the same application effect, the amount of bio-based polyol added can be increased. Under the same bio-based polyol content, the application performance is better, and the polysiloxane is widely used as a foam stabilizer in the preparation of polyurethane foam.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurethane rigid foams, and in particular to a multi-group modified polysiloxane and a preparation method and application thereof, and polyurethane foam. Background Art

[0002] Polyurethane rigid foam is widely used in household appliances, pipe insulation, refrigerated containers, and construction due to its low density and low thermal conductivity. In the prior art, polyurethane rigid foam is composed of white material and black material. The main component of the white material is polyether polyol, which mostly comes from petrochemical or coal chemical products. It is a non-renewable resource and its price is limited by energy price fluctuations. As a renewable resource, bio-based polyols are increasingly being studied in the preparation of polyols, and researchers have also developed a variety of bio-based polyols.

[0003] CN201510660909.4 reports a bio-based polyurethane spray foam. This invention has a high content of bio-based materials, which are used in the thermal insulation and waterproof spraying of walls or roofs, so that the foam material has similar properties to foams produced from all petroleum-based materials; CN201810136827.3 reports a bio-based polyurethane containing a carbonate structure. The invention has the characteristics of water resistance, heat resistance, etc., and the preparation method is simple and the cost is low.

[0004] However, in the process of replacing traditional polyether polyols with bio-based polyols in polyurethane foam, researchers have also found some problems with bio-based polyols, such as darker color of polyurethane foam, coarser pore size on the surface of polyurethane foam, decreased thermal conductivity, increased thermal conductivity, and even foam cracking. At present, it is not possible to completely replace petrochemical-based polyethers with bio-based polyols, and they can only be mixed or partially replaced.

[0005] In order to improve a series of problems such as coarsening of foam cells and increase in thermal conductivity that occur during the process of partial replacement of petrochemical-based polyethers by bio-based polyols, the present application is specially proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a multi-group modified polysiloxane and a preparation method, application and polyurethane foam thereof.

[0007] The present invention is achieved in that:

[0008] In a first aspect, the present invention provides a multi-group modified polysiloxane having the structural formula

[0009]

[0010] Wherein: m = 10 to 60, n = 1 to 10, r = 1 to 4, p = 1 to 3;

[0011] R 1 Selected from methyl, R 2 , R 3 and R 4 Any of the following:

[0012] R 2 The general formula is -CH 2 CH 2 CH 2 O(C 2 H 4 O) a (C 3 H 6 O) b R 6 , where a = 2 to 30, b = 2 to 15, R 6 is H or an alkyl group containing 1 to 4 carbon atoms;

[0013] R 3 The general formula is -CH 2 CH 2 CH 2 O(C 2 H 4 O) c H, where c = 3 to 20;

[0014] R 4 The general formula is -(CH 2 ) x R(CH 2 ) x -or-(CH 2 ) x R(CH 2 ) x-2 CHCH 2 , x = 2 ~ 4, where the structure of R is: -C w H 2w -, w = 1-5, or or -O(C 2 H 4 O) d (C 3 H 6 O) e -, d = 0 to 8, e = 0 to 5, d + e > 0 or t = 0 to 15;

[0015] R 5 Selected from methyl, R 2 , R 3 and R 4 Any one of .

[0016] In a second aspect, the present invention provides a method for preparing a multi-group modified polysiloxane as described in any one of the aforementioned embodiments, comprising: reacting a mixture of a compound containing a carbon-carbon double bond, a low hydrogen polysiloxane, an amine auxiliary agent and a solvent under the action of a catalyst to obtain the obtained product.

[0017] In a third aspect, the present invention provides the use of the multi-group modified polysiloxane as described in any one of the aforementioned embodiments or the multi-group modified polysiloxane prepared by the preparation method of the multi-group modified polysiloxane as described in any one of the aforementioned embodiments as a foam stabilizer in the preparation of polyurethane foam.

[0018] In a fourth aspect, the present invention provides a polyurethane foam, comprising a polyether polyol, a bio-based polyol and a foam stabilizer, wherein the mass percentage of the polyether polyol and the bio-based polyol is 50-90%:10%-50%, the amount of the foam stabilizer added is 1%-3% of the total amount of the polyether polyol and the bio-based polyol, and the foam stabilizer is the multi-group modified polysiloxane described in any one of the aforementioned embodiments or the multi-group modified polysiloxane prepared by the preparation method of the multi-group modified polysiloxane described in any one of the aforementioned embodiments.

[0019] The present invention has the following beneficial effects:

[0020] The multi-group modified polysiloxane provided by the present invention is modified by adding monoallyl polyoxyethylene ether and a modifier containing carbon-carbon double bonds at both ends to the conventional allyl polyether for polyether modification of low hydrogen polysiloxane. The multi-group modified polysiloxane of the present application brings more plasticity in structure, and the corresponding groups in the structure can be adjusted according to different types of bio-based polyols. This modified polysiloxane can significantly improve the problems of coarse pores and high thermal conductivity caused by partial replacement of petroleum-based polyols by bio-based polyols. Under the same application effect, the amount of bio-based polyols added can be increased, and its application performance is better under the same bio-based polyol content. The multi-group modified polysiloxane provided by the present invention is widely used as a foam stabilizer in the preparation of polyurethane foam. The polyurethane foam with multi-group modified polysiloxane added has the problems of coarse pores and increased thermal conductivity caused by partial replacement of petrochemical-based polyols by bio-based polyols, and the closed cell rate is reduced, and the reduction rate of parallel compression strength and vertical compression strength is improved. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0022] The present invention provides a multi-group modified polysiloxane, the structural formula of which is

[0023]

[0024] Wherein: m = 10 to 60, n = 1 to 10, r = 1 to 4, p = 1 to 3;

[0025] R 1 Selected from methyl, R 2 , R 3 and R 4 Any of the following:

[0026] R 2 The general formula is -CH 2 CH 2 CH 2 O(C 2 H 4 O) a (C 3 H 6 O) b R 6 , where a = 2 to 30, b = 2 to 15, R 6 is H or an alkyl group containing 1 to 4 carbon atoms;

[0027] R 3 The general formula is -CH 2 CH 2 CH 2 O(C 2 H 4 O) c H, where c = 3 to 20;

[0028] R 4 The general formula is -(CH 2 ) x R(CH 2 ) x -or-(CH 2 ) x R(CH 2 ) x-2 CHCH 2 , x = 2 ~ 4, where the structure of R is: -C w H 2w -, w = 1-5, or or -O(C 2 H 4 O) d (C 3 H 6 O) e -, d = 0 to 8, e = 0 to 5, d + e > 0 or t = 0 to 15;

[0029] R 5 Selected from methyl, R 2 , R 3 and R 4 Any one of .

[0030] Preferably, R 4 The structural formula is: in Use M E express.

[0031] Furthermore, the present invention also provides a method for preparing the multi-group modified polysiloxane, which comprises the following steps:

[0032] (1) Prepare low hydrogen polysiloxane.

[0033] Low hydrogen polysiloxane can be purchased from the market or prepared independently. The preparation method is as follows: hexamethyldisiloxane, octamethylcyclotetrasiloxane and high hydrogen polysiloxane are used as raw materials, reacted at 60°C for 8 hours under an acidic catalyst to obtain low hydrogen polysiloxane. The acidic catalyst is acidic clay.

[0034] In the present application, different types of low hydrogen-containing polysiloxane can be obtained by adjusting the usage ratio of the raw materials hexamethyldisiloxane, octamethylcyclotetrasiloxane and high hydrogen-containing polysiloxane, for example, MD 40 D' 5 M.MD 35 D' 7 M.MD 50 D' 8 M, wherein, adjusting the usage ratio of the raw materials hexamethyldisiloxane, octamethylcyclotetrasiloxane and high hydrogen-containing polysiloxane according to the specific type of low hydrogen-containing polysiloxane is a conventional technology and will not be elaborated in detail in this application.

[0035] (2) Prepare compounds containing carbon-carbon double bonds.

[0036] The compounds containing carbon-carbon double bonds include allyl polyethers, monoallyl polyoxyethylene ethers, and compounds containing carbon-carbon double bonds at both ends.

[0037] Among them, the allyl polyether realizes the polyether modification of polysiloxane, and the average molecular weight of the allyl polyether is 1000-1500; the allyl polyether contains 60%-80% ethyleneoxy groups in molar percentage, and the terminal is hydroxyl or methyl.

[0038] The average molecular weight of monoallyl polyoxyethylene ether is 200-400;

[0039] The modified substance containing carbon-carbon double bonds at both ends includes at least one of bisallyl polyether, polysiloxane containing carbon-carbon double bonds at both ends, terminal diene and bisphenol A bisallyl ether polyether; preferably, the polysiloxane containing carbon-carbon double bonds at both ends is vinyl-terminated polydimethylsiloxane. The vinyl-terminated polydimethylsiloxane can be purchased commercially or homemade. The preparation method is to add octamethylcyclotetrasiloxane and tetramethyldivinyldisiloxane to a reactor, react at 70°C for 5 hours under the action of acidic white clay to obtain vinyl-terminated polydimethylsiloxane. Different types of vinyl-terminated polydimethylsiloxane can be obtained by adjusting the dosage ratio of the raw materials octamethylcyclotetrasiloxane and tetramethyldivinyldisiloxane, for example, M E D 10 M E 、M E D 8 M E Among them, adjusting the dosage ratio of the raw materials according to the specific type of vinyl-terminated polydimethylsiloxane is a conventional technology and will not be elaborated in detail in this application.

[0040] Preferably, the mass ratio of the allyl polyether, the monoallyl polyoxyethylene ether and the compound containing a carbon-carbon double bond at both ends is 200-250:4-9:1-3.

[0041] (3) A mixture of a compound containing a carbon-carbon double bond, a low hydrogen-containing polysiloxane, an amine auxiliary agent and a solvent is reacted in the presence of a catalyst to obtain the product.

[0042] Specifically, a compound containing a carbon-carbon double bond, a low hydrogen polysiloxane and a solvent are added in a mass ratio of 205-262:50-90:40-50; the amount of the amine auxiliary agent accounts for 80-120 ppm of the total amount of the feed; the above-mentioned compound containing a carbon-carbon double bond, the low hydrogen polysiloxane, the amine auxiliary agent and the solvent are uniformly mixed to obtain a mixture, the mixture is stirred in a nitrogen atmosphere, the temperature is raised to 85-105° C., and the mixture is kept warm for 0.5-1h, and then a catalyst is added (the amount of the catalyst accounts for 8-12 ppm of the total amount of the feed), and after keeping warm for 5-7h, the remaining solvent in the mixture is removed.

[0043] Preferably, the amine auxiliary agent includes at least one of N,N-dimethylethanolamine, N,N-dibutylethanolamine, 3-dimethylpropylamine and 2-butylaminoethanol; more preferably, the amine auxiliary agent is NN-dimethylethanolamine; the solvent is isopropanol or toluene. The catalyst is a palladium-containing complex, a rhodium-containing complex or a platinum-containing complex; more preferably, the catalyst is chloroplatinic acid.

[0044] In the present application, on the basis of the conventional allyl polyether for polyether modification of low hydrogen polysiloxane, monoallyl polyoxyethylene ether and a double-end group containing carbon-carbon double bonds are added for multi-group modification. The multi-group modified polysiloxane of the present application brings more plasticity in structure, and the corresponding groups in the structure can be adjusted according to different types of bio-based polyols. This modified polysiloxane can significantly improve the problems of coarse pores and high thermal conductivity caused by partial replacement of petroleum-based polyols by bio-based polyols. Under the same application effect, the amount of bio-based polyol added can be increased, and its application performance is better at the same bio-based polyol content. The present invention is widely applicable to industries such as home appliances and panels.

[0045] In addition, the present application also provides the use of the above-mentioned multi-group modified polysiloxane as a foam stabilizer in the preparation of polyurethane foam. The multi-group modified polysiloxane of the present application can be used as a foam stabilizer in polyurethane foam in which bio-based polyols partially replace petrochemical-based polyethers, which can improve a series of problems such as coarsening of foam cells and increase in thermal conductivity caused by partial replacement of petrochemical-based polyethers by bio-based polyols.

[0046] For example, the present application provides a polyurethane foam, which includes a petroleum-based polyether polyol, a bio-based polyol and a foam stabilizer, the mass percentage of the polyether polyol and the bio-based polyol is 50-90%: 10%-50%, the added amount of the foam stabilizer is 1%-3% of the total amount of the petroleum-based polyether polyol and the bio-based polyol, and the foam stabilizer is the above-mentioned multi-group modified polysiloxane.

[0047] The polyurethane foam with multi-group modified polysiloxane added has improved the problems of coarsening of foam cells and increase in thermal conductivity caused by partial replacement of petrochemical-based polyether by bio-based polyols, and the reduction of closed cell rate, parallel compression strength and vertical compression strength reduction rate have all been improved. Under the same application effect, the amount of bio-based polyol added can be increased, and its application performance is better at the same bio-based polyol content.

[0048] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0049] Example 1

[0050] The present embodiment provides a multi-group modified polysiloxane, and the preparation method thereof comprises: adding 210.0 g of an allyl-started polyether with an average molecular weight of 1000 (the polyether contains 80% ethyleneoxy groups by mole percentage and a hydroxyl group at the end), 9.0 g of a monoallyl polyoxyethylene ether with an average molecular weight of 400, 1.0 g of 1,8-nonadiene, 90.0 g of a low hydrogen-containing polysiloxane (MD 40 D' 5M), 50g isopropanol, 100ppm N,N-dimethylethanolamine. The mixture is stirred in a nitrogen atmosphere, heated to 85-90°C, kept warm for 0.5h, 10ppm chloroplatinic acid is added, kept warm for 6h, and the solvent is removed to obtain a clear and transparent light brown liquid, which is a multi-group modified polysiloxane.

[0051] Example 2

[0052] The present embodiment provides a multi-group modified polysiloxane, and the preparation method thereof comprises: adding 250.0 g of an allyl-started polyether with an average molecular weight of 1500 (the polyether contains 60% ethyleneoxy groups by mole percentage and a hydroxyl group at the end), 4.0 g of a monoallyl polyoxyethylene ether with an average molecular weight of 200, 1.0 g of 1,7-octadiene, 50.0 g of a low-hydrogen polysiloxane (MD 35 D' 7 M), 50g isopropanol, 100ppm N,N-dimethylethanolamine. The mixture is stirred in a nitrogen atmosphere, heated to 85-90°C, kept warm for 0.5h, 10ppm chloroplatinic acid is added, kept warm for 6h, and the solvent is removed to obtain a clear and transparent light brown liquid, which is a multi-group modified polysiloxane.

[0053] Example 3

[0054] The present embodiment provides a multi-group modified polysiloxane, and the preparation method thereof comprises: adding 210.0 g of an allyl starting polyether with an average molecular weight of 1000 (the polyether contains 80% by mole of ethyleneoxy groups and a methyl group at the end), 4.0 g of a monoallyl polyoxyethylene ether with an average molecular weight of 200, 2.0 g of bisphenol A bisallyl ether, 90.0 g of a low hydrogen polysiloxane (MD 40 D' 5 M), 50g isopropanol, 100ppm N,N-dimethylethanolamine. The mixture is stirred in a nitrogen atmosphere, heated to 85-90°C, kept warm for 0.5h, 10ppm chloroplatinic acid is added, kept warm for 6h, and the solvent is removed to obtain a clear and transparent light brown liquid, which is a multi-group modified polysiloxane.

[0055] Example 4

[0056] The present embodiment provides a multi-group modified polysiloxane, and the preparation method thereof comprises: adding 220.0 g of an allyl starting polyether with an average molecular weight of 1000 (the polyether contains 80% by mole of ethyleneoxy groups and is terminated with a hydroxyl group), 8.0 g of a monoallyl polyoxyethylene ether with an average molecular weight of 400, 3.0 g of a bisallyl polyether with an average molecular weight of 400 (the polyether contains 80% by mole of ethyleneoxy groups), 80.0 g of the obtained low hydrogen polysiloxane (MD 50 D' 8 M), 40g toluene, 100ppm N,N-dimethylethanolamine. The mixture was stirred in a nitrogen atmosphere, heated to 85-90°C, kept warm for 0.5h, 10ppm chloroplatinic acid was added, kept warm for 6h, and the solvent was removed to obtain a clear and transparent light brown liquid, which was multi-group modified polysiloxane.

[0057] Example 5

[0058] The present embodiment provides a multi-group modified polysiloxane, and the preparation method thereof comprises: adding 200.0 g of an allyl-started polyether with an average molecular weight of 1000 (the polyether contains 80% by mole of ethyleneoxy groups and a hydroxyl group at the end), 8.0 g of a monoallyl polyoxyethylene ether with an average molecular weight of 400, 3.0 g of a vinyl-terminated polydimethylsiloxane (M E D 10 M E ), 80.0g low hydrogen polysiloxane (MD 40 D' 5 M), 40g toluene, 100ppm N,N-dimethylethanolamine. The mixture was stirred in a nitrogen atmosphere, heated to 100-110°C, kept warm for 1h, 10ppm chloroplatinic acid was added, kept warm for 6h, and the solvent was removed to obtain a clear and transparent light brown liquid, which was multi-group modified polysiloxane.

[0059] Example 6

[0060] The present embodiment provides a multi-group modified polysiloxane, and the preparation method thereof comprises: adding 240.0 g of an allyl-started polyether with an average molecular weight of 1200 (the polyether contains 80% by mole of ethyleneoxy groups and is terminated with a hydroxyl group), 8.0 g of a monoallyl polyoxyethylene ether with an average molecular weight of 200, 2.0 g of a vinyl-terminated polydimethylsiloxane (M E D 8 M E ), 50.0 g of the obtained low hydrogen polysiloxane (MD35 D' 7 M), 40g toluene, 100ppm N,N-dimethylethanolamine. The mixture was stirred in a nitrogen atmosphere, heated to 100-110°C, kept warm for 0.5h, 10ppm chloroplatinic acid was added, kept warm for 6h, and the solvent was removed to obtain a clear and transparent light brown liquid, which was multi-group modified polysiloxane.

[0061] Comparative Example 1

[0062] This comparative example provides a modified polysiloxane, and its preparation method is basically the same as that of Example 1, except that some raw materials in Example 1 are omitted: 9.0 g of monoallyl polyoxyethylene ether with an average molecular weight of 400, 1.0 g of 1,8-nonadiene and 50 g of isopropanol.

[0063] The specific preparation method is as follows: 210.0 g of an allyl-started polyether with an average molecular weight of 1000 (the polyether contains 80% ethyleneoxy groups by mole and has a hydroxyl group at the end), 90.0 g of a low-hydrogen polysiloxane (MD 40 D' 5 M), 100ppm N,N-dimethylethanolamine. The mixture was stirred in a nitrogen atmosphere, heated to 85-90°C, kept warm for 0.5h, 10ppm chloroplatinic acid was added, and kept warm for 6h to obtain a clear and transparent light brown liquid, which was the modified polysiloxane.

[0064] Comparative Example 2

[0065] This comparative example provides a modified polysiloxane, and its preparation method is basically the same as that of Example 2, except that some raw materials in Example 2 are omitted: 4.0 g of monoallyl polyoxyethylene ether with an average molecular weight of 200, 1.0 g of 1,7-octadiene and 50 g of isopropanol.

[0066] The specific preparation method is as follows: 250.0 g of an allyl-started polyether with an average molecular weight of 1500 (the polyether contains 60% ethyleneoxy groups by mole and has a hydroxyl group at the end), 50.0 g of a low hydrogen-containing polysiloxane (MD 35 D' 7 M), 100ppm N,N-dimethylethanolamine. The mixture was stirred in a nitrogen atmosphere, heated to 85-90°C, kept warm for 0.5h, 10ppm chloroplatinic acid was added, and kept warm for 6h to obtain a clear and transparent light brown liquid, which was the modified polysiloxane.

[0067] Comparative Example 3

[0068] This comparative example provides a modified polysiloxane, and its preparation method is basically the same as that of Example 3, except that some raw materials in Example 3 are omitted: 4.0 g of monoallyl polyoxyethylene ether with an average molecular weight of 200, 2.0 g of bisphenol A bisallyl ether, and 50 g of isopropanol.

[0069] The specific preparation method is as follows: 210.0 g of an allyl-started polyether with an average molecular weight of 1000 (the polyether contains 80% ethyleneoxy groups by mole percentage and a methyl group at the end), 90.0 g of a low-hydrogen polysiloxane (MD 40 D' 5 M), 100ppm N,N-dimethylethanolamine. The mixture was stirred in a nitrogen atmosphere, heated to 85-90°C, kept warm for 0.5h, 10ppm chloroplatinic acid was added, kept warm for 6h, and the solvent was removed to obtain a clear and transparent light brown liquid, which was multi-group modified polysiloxane.

[0070] Comparative Example 4

[0071] This comparative example provides a modified polysiloxane, and its preparation method is basically the same as that of Example 4, except that: 8.0 g of monoallyl polyoxyethylene ether with an average molecular weight of 400 and 3.0 g of bisallyl polyether with an average molecular weight of 400 (the polyether contains 80% by mole of ethyleneoxy groups) in Example 4 are omitted, and 40 g of toluene as a solvent are also omitted.

[0072] The specific preparation method is as follows: 220.0 g of an allyl-started polyether with an average molecular weight of 1000 (the polyether contains 80% ethyleneoxy groups by mole percentage and is terminated with a hydroxyl group) and 80.0 g of the obtained low hydrogen-containing polysiloxane (MD 50 D' 8 M), 100ppm N,N-dimethylethanolamine. The mixture was stirred in a nitrogen atmosphere, heated to 85-90°C, kept warm for 0.5h, 10ppm chloroplatinic acid was added, and kept warm for 6h to obtain a clear and transparent light brown liquid, which was the modified polysiloxane.

[0073] Comparative Example 5

[0074] This comparative example provides a modified polysiloxane, and its preparation method is basically the same as that of Example 6, except that some raw materials in Example 6 are omitted: 8.0 g of monoallyl polyoxyethylene ether with an average molecular weight of 200, 2.0 g of vinyl-terminated polydimethylsiloxane (M E D 8 M E ), 40g toluene.

[0075] The specific preparation method is as follows: 240.0 g of an allyl-started polyether with an average molecular weight of 1200 (the polyether contains 80% by mole of ethyleneoxy groups and is terminated with a hydroxyl group), 50.0 g of a low-hydrogen polysiloxane (MD 35 D' 7 M), 100 ppm N,N-dimethylethanolamine. The mixture was stirred in a nitrogen atmosphere, heated to 100-115°C, kept warm for 0.5 h, 10 ppm chloroplatinic acid was added, and kept warm for 6 h to obtain a clear and transparent light brown liquid, which was the modified polysiloxane.

[0076] The examples and comparative examples were evaluated for application, and the polyurethane white material was mixed according to the following table, and then evaluated and compared for application.

[0077] Table 1 Partial parameters of polyurethane white material components (mass ratio)

[0078] raw material Ratio 1 Ratio 2 Ratio 3 Polyether polyol A 100 70 50 Bio-based polyol B 0 30 50 Foam stabilizer 2.0 2.0 2.0

[0079] Polyether polyol A is a sucrose-initiated polyether polyol with a hydroxyl value of 380 mgKOH / g and a hydroxyl functionality of 6;

[0080] Bio-based polyol B is an epoxidized soybean oil-based vegetable oil polyol with a hydroxyl value of 310 mgKOH / g and a hydroxyl functionality of 4.5.

[0081] The rigid polyurethane foam obtained above was subjected to performance tests, wherein the thermal conductivity was determined according to GB / T10295-2008 Determination of steady-state thermal resistance and related properties of thermal insulation materials, the closed cell ratio was determined according to GB / T 10799-2008 Determination of volume percentage of open and closed cells in rigid foam plastics, and the compression strength test of rigid polyurethane foam was conducted according to GB 8813-88 Compression test method for rigid foam plastics, wherein the parallel compression strength refers to the direction parallel to the pressure and the foam growth direction, and the perpendicular compression strength refers to the direction perpendicular to the pressure and the foam growth direction.

[0082] Table 2 Test results of application performance of rigid polyurethane foam prepared by mix 1

[0083]

[0084] Table 3 Test results of application performance of rigid polyurethane foam prepared by mix 2

[0085]

[0086]

[0087] Table 4 Test results of application performance of rigid polyurethane foam prepared by mix 3

[0088]

[0089] As can be seen from Table 2, without the use of bio-based polyols, the performance of each rigid polyurethane foam is not much different. Tables 3 and 4 show the performance test results of each rigid polyurethane foam after adding bio-based polyols. It can be seen that the conventional modified polysiloxane has obvious differences in foam performance, the thermal conductivity increases; the closed cell rate decreases; the pore distribution is uneven, which is manifested as the difference between parallel compression strength and vertical compression strength increases. Comparing the data of Examples 1-6 and Comparative Examples 1-5 in Tables 3 and 4, it can be seen that the increase in thermal conductivity in Examples 1-6 is much smaller than that in Comparative Examples 1-5, and the more the thermal conductivity increases, the lower the thermal conductivity will be. At the same time, the decrease in closed cell rate in Examples 1-6 is much smaller than that in Comparative Examples 1-5, and the increase in the difference between parallel compression strength and vertical compression strength in Examples 1-6 is much smaller than that in Comparative Examples 1-5. The above data show that under the same application effect, the multi-group modified polysiloxane of the present invention can significantly increase the amount of bio-based polyol added, and its application performance is better at the same bio-based polyol content.

[0090] In summary, the multi-group modified polysiloxane provided by the present application is modified by adding monoallyl polyoxyethylene ether and a double-end group containing a carbon-carbon double bond on the basis of polyether modification of low-hydrogen polysiloxane by conventional allyl polyether, and the molecules of the obtained multi-group modified polysiloxane contain monoallyl polyoxyethylene ether and diene substances. The multi-group modified polysiloxane of the present application brings more plasticity in structure, and the corresponding groups in the structure can be adjusted according to different types of bio-based polyols. This modified polysiloxane can significantly improve the problems of coarse pores and high thermal conductivity caused by partial replacement of petroleum-based polyols by bio-based polyols. Under the same application effect, the amount of addition of bio-based polyols can be increased, and at the same bio-based polyol content, its application performance is better. The present invention is widely applicable to industries such as home appliances and panels.

[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polyurethane foam, characterized in that It includes polyether polyol, bio-based polyol and foam stabilizer, the mass percentage of the polyether polyol and the bio-based polyol is 50-90%:10%-50%, the added amount of the foam stabilizer is 1%-3% of the total amount of the polyether polyol and the bio-based polyol, and the foam stabilizer is a multi-group modified polysiloxane, and the structural formula of the multi-group modified polysiloxane is: ; Where: m = 10 ~ 60, n = 1 ~ 10, r = 1 ~ 4, p = 1 ~ 3; R1 is selected from any one of methyl, R2, R3 and R4; The general formula of R2 is -CH2CH2CH2O(C2H4O) a (C3H6O) b R6, wherein a=2-30, b=2-15, R6 is H or an alkyl group containing 1-4 carbon atoms; The general formula of R3 is -CH2CH2CH2O(C2H4O) c H, where c = 3~20; The general formula of R4 is -(CH2) x R(CH2) x-2 CH=CH2, x=2~4, the structure of R: -C w H 2w -, w = 1~5, or , or -O(C2H4O) d (C3H6O) e -, d=0~8, e=0~5, d+e>0 or , t=0~15; R5 is selected from any one of methyl, R2, R3 and R4.

2. The polyurethane foam according to claim 1, characterized in that The structural formula of R4 of the multi-group modified polysiloxane is expressed as .

3. The polyurethane foam according to claim 1, characterized in that The preparation method of the multi-group modified polysiloxane comprises: reacting a mixture of a compound containing a carbon-carbon double bond, a low-hydrogen polysiloxane, an amine auxiliary agent and a solvent under the action of a catalyst to obtain the polysiloxane.

4. The polyurethane foam according to claim 3, characterized in that In the preparation method of the multi-group modified polysiloxane, the mass ratio of the compound containing carbon-carbon double bonds, the low hydrogen-containing polysiloxane and the solvent is 205-262:50-90:40-50.

5. The polyurethane foam according to claim 3, characterized in that In the preparation method of the multi-group modified polysiloxane, the amine auxiliary agent is used in an amount of 80-120 ppm in parts per million of the total feed amount.

6. The polyurethane foam according to claim 3, characterized in that In the preparation method of the multi-group modified polysiloxane, the catalyst is used in an amount of 8-12 ppm in parts per million of the total feed amount.

7. The polyurethane foam according to claim 3, characterized in that In the preparation method of the multi-group modified polysiloxane, the reaction of the mixture with the catalyst comprises: stirring the mixture in a nitrogen atmosphere, heating to 85-105° C., keeping the temperature for 0.5-1 h, then adding the catalyst, keeping the temperature for 5-7 h, and removing the remaining solvent in the mixture.

8. The polyurethane foam according to claim 4, characterized in that In the preparation method of the multi-group modified polysiloxane, the compound containing carbon-carbon double bonds includes allyl polyether, monoallyl polyoxyethylene ether and a compound containing carbon-carbon double bonds at both ends.

9. The polyurethane foam according to claim 8, characterized in that The mass ratio of the allyl-containing polyether, the monoallyl polyoxyethylene ether and the compound containing carbon-carbon double bonds at both ends is 200-250:4-9:1-3.

10. The polyurethane foam according to claim 8, characterized in that The allyl-containing polyether has an average molecular weight of 1000-1500, contains 60%-80% ethyleneoxy groups by mole percentage, and has a hydroxyl group or a methyl group at the end.

11. The polyurethane foam according to claim 8, characterized in that The average molecular weight of the monoallyl polyoxyethylene ether is 200-400.

12. The polyurethane foam according to claim 8, characterized in that The compound containing carbon-carbon double bonds at both ends includes at least one of terminal bisallyl polyether, polysiloxane containing carbon-carbon double bonds at both ends, and bisphenol A bisallyl ether.

13. The polyurethane foam according to claim 12, characterized in that The polysiloxane containing carbon-carbon double bonds at both ends is vinyl-terminated polydimethylsiloxane.

14. The polyurethane foam according to claim 3, characterized in that In the preparation method of the multi-group modified polysiloxane, the catalyst is a palladium-containing complex, a rhodium-containing complex or a platinum-containing complex.

15. The polyurethane foam according to claim 3, characterized in that In the preparation method of the multi-group modified polysiloxane, the catalyst is chloroplatinic acid.

16. The polyurethane foam according to claim 3, characterized in that In the preparation method of the multi-group modified polysiloxane, the amine auxiliary agent includes at least one of N,N-dimethylethanolamine, N,N-dibutylethanolamine, 3-dimethylpropylamine and 2-butylaminoethanol.

17. The polyurethane foam according to claim 3, characterized in that In the preparation method of the multi-group modified polysiloxane, the amine auxiliary agent is N,N-dimethylethanolamine.

18. The polyurethane foam according to claim 3, characterized in that In the preparation method of the multi-group modified polysiloxane, the solvent is isopropanol or toluene.

Citation Information

Patent Citations

  • Bio-based carbonate-containing polyurethane, and preparation method and application thereof

    CN108395512A

  • Biology base polyurethane spray coating foam plastic and preparation method of biology base polyurethane spray coating foam plastic

    CN105294989A

  • Polyether modified siloxane and synthesis method thereof

    CN111040175A

  • Silicone copolymer, method for producing same, rigid foam stabilizer and rigid polyurethane foam

    CN113831538A

  • Organosilicon polyether copolymer as well as preparation method and application thereof

    CN114106336A