A method for manufacturing a steel ingot for a spent fuel dry storage container and a forging

Through the smelting process of electric arc furnace and refining furnace, combined with rapid precipitation and re-precipitation deoxidation technology, the problems of poor performance and processing difficulties of spent fuel dry storage steel are solved, and the high-performance steel ingots for spent fuel dry storage containers are realized. manufacture.

CN116254451BActive Publication Date: 2024-11-29SHANGHAI ELECTRIC SHMP CASTING & FORGING CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202211589135.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-11-29
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The existing spent fuel dry storage steel has poor performance and difficult processing, and the production process of the existing technology is cumbersome and difficult to control.

Method used

A manufacturing method, including arc furnace smelting and refining furnace smelting, reduce carbon and phosphorus content through precise control of ingredients and alloy elements, and perform rapid pre-deoxygenation and re-precipitation and deoxygenation, ensuring the purity of molten steel and trace elements control, and finally High-performance forgings are obtained by vacuum casting and forging.

Benefits of technology

It realizes the manufacturing of steel ingots with extremely low carbon content and high purity, taking into account the carbon component segregation problem of large steel ingots. The forgings have good strength and excellent low-temperature toughness, and are easy to process and easy to operate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a method for manufacturing a steel ingot for a spent fuel dry storage container and a forging, which belongs to the field of metallurgy. Aiming at the problem that the existing steel for spent fuel dry storage has poor performance and is difficult to process, the present invention provides a method for manufacturing a steel ingot for a spent fuel dry storage container, comprising the following steps: batching; arc furnace smelting; refining furnace smelting; heating to different stages and adding different alloys accordingly; vacuum degassing operation; after the vacuum degassing operation is completed, sampling is performed to adjust the composition, and nitrogen blowing is started at the same time, and the temperature is adjusted to 1630°C to 1635°C before hanging out for pouring; vacuum pouring of the steel ingot; forging. The preparation method of the present invention not only ensures an extremely low carbon content, but also takes into account the carbon component segregation problem of large steel ingots, the control of various trace elements is accurate, the purity of molten steel is excellent, and the level of flaw detection and inclusion control is high, which lays a solid foundation for the subsequent product performance, and the preparation process is simple and easy to operate; at the same time, the forging of the present invention has good strength and excellent low-temperature toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metallurgy, and more specifically, relates to a method for manufacturing a steel ingot for a spent fuel dry storage container and a forging. Background Art

[0002] Nuclear energy is an efficient and clean energy source. It not only has obvious advantages in safety, stability and environmental protection, but is also an economical energy source. However, spent fuel, as nuclear fuel that has been exposed to radiation and used, cannot continue to maintain nuclear reactions. Spent fuel has extremely strong radioactivity, with a certain neutron emission rate and heat release. Therefore, the safe storage of spent fuel is one of the important contents of nuclear power plant safety management.

[0003] Corresponding improvements have also been made to address the above problems. For example, the Chinese patent application number is CN201911356754.X, and the publication date is April 21, 2020. The patent discloses a SA517GrF steel plate for spent fuel storage tanks and its production method. The chemical composition and mass percentage of the steel plate conform to ASME SA-517 / SA-517M, and trace alloying elements Nb (0.01% to 0.02%) and Ti (0.01% to 0.03%) are added on the basis of the steel plate, and the rest are Fe and unavoidable impurities; the production method includes smelting process, rolling process, water cooling process, quenching process and tempering process. The disadvantage of this patent is that the production process is cumbersome and difficult to control.

[0004] Another example is Chinese patent application number CN201610417470.7, which was published on November 9, 2016. The patent discloses a special steel-based alloy material for reactor spent fuel storage and a preparation method thereof. The special steel-based alloy material has the following composition and mass percentage: C≤0.03%, N≤0.02%, S≤0.01%, P≤0.03%, Mn≤1.0%, Cr: 10.0-32.0%, Al: 3.0-20.0%, B: 0.5-5.0%, Ti: 0.75-12.5%, and the rest is iron and unavoidable impurities, and the ratio of Ti content to B content satisfies Ti:B=1.5-2.5. After the micro-nano TiB2 particles are formed in situ during the batching and vacuum induction melting process, they are cast and molded, and then subjected to processes such as hot forging, hot rolling and annealing to finally obtain a special steel-based alloy material bar or plate for reactor spent fuel storage. The shortcoming of this patent is that although it can significantly reduce the cost of raw materials, the overall performance is relatively general. Summary of the invention

[0005] 1. Problems to be solved

[0006] In view of the problem that the existing steel for dry storage of spent fuel has poor performance and is difficult to process, the present invention provides a method for manufacturing a steel ingot for a spent fuel dry storage container and a forging. The preparation method of the present invention not only ensures an extremely low carbon content but also takes into account the carbon component segregation problem of large steel ingots. The various trace elements are precisely controlled, the purity of molten steel is excellent, and the level of flaw detection and inclusion control is high, which lays a solid foundation for subsequent product performance. The preparation process is simple and easy to operate. At the same time, the forging of the present invention has good strength and excellent low-temperature toughness.

[0007] 2. Technical solution

[0008] To solve the above problems, the present invention adopts the following technical solutions.

[0009] A method for manufacturing a steel ingot for a spent fuel dry storage container comprises the following steps:

[0010] S1: Ingredients: Use the following components in percentage by mass: 55-65% high-quality carbon scrap steel, 20-25% carbon steel scraps, 20-30% high-quality pig iron, and 2.5% electrolytic nickel;

[0011] S2: Smelting in an electric arc furnace for decarbonization and dephosphorization; when the smelting temperature of the electric arc furnace reaches above 1670℃, the smelted steel is placed in a refining bag. When the steel reaches 20-30 tons, aluminum ingots are added; when the steel is finished, lime is added;

[0012] S3: Smelting in a refining furnace, after the refining bag reaches the heating station, adding aluminum-iron alloy, slag (the slag includes lime and fluorite), aluminum powder and calcium silicon powder;

[0013] S4: Raise the temperature to 1600℃~1620℃, take samples during the process, and stop heating if the carbon content reaches 0.05%;

[0014] S5: After continuing to heat up to 1640°C to 1660°C, Ni, Mo, Mn alloy and aluminum powder are added to continue reduction;

[0015] S6: After continuing to heat up to 1660°C to 1680°C, take a slag sample, add V-Fe alloy, Nb-Fe alloy and Al-Fe alloy after the slag is white;

[0016] S7: perform vacuum degassing operation;

[0017] S8: After the vacuum degassing operation is completed, samples are taken for composition adjustment, and nitrogen blowing is started at the same time. The temperature is adjusted to 1630℃~1635℃ and then the casting is hoisted out;

[0018] S9: Vacuum casting of steel ingot;

[0019] S10: After demoulding, the forgings are hot-sent to the forging workshop for forging to obtain forgings.

[0020] Furthermore, the amount of aluminum ingot added in step S2 is: 3-5 kg / t, t is the rated molten steel volume of the electric arc furnace; the amount of lime added is 500-600 kg; at the same time, decarburization is performed to C≤0.02% and dephosphorization is performed to P≤0.003% in step S2.

[0021] Furthermore, the amount of aluminum-iron alloy added in step S3 is: 200-250kg, the slag contains 2000-2500kg of lime and 400-500kg of fluorite; the amount of aluminum powder is: 2.0-3.0kg / t, and the amount of calcium silicon powder is: 1.0-1.5kg / t; the amount of aluminum powder in step S5 is: 0.5kg / t; wherein t is the rated molten steel volume of the electric arc furnace.

[0022] Furthermore, the heating method in step S4 is to use the aluminothermic method: add 300-350 kg of aluminum ingots, insert an oxygen tube to blow oxygen for 3-4 minutes; and during the heating period, sampling is performed every 10 minutes, and if the carbon content reaches 0.05%, the power is stopped to heat up.

[0023] Furthermore, when performing oxygen blowing operation, the verticality of the oxygen pipe is maintained at more than 75°, and the oxygen jet is prevented from blowing onto the ladle wall.

[0024] Furthermore, when the vacuum degassing operation is performed in step S7, the argon blowing flow rate is adjusted to 200-250 LN / min, the vacuum degree is ≤65Pa, and the effective time is 30-35min, and the effective time starts when the vacuum degree reaches 65Pa.

[0025] Furthermore, in step S9, the ingot mold is placed in a vacuum tank, the vacuum degree is maintained at ≤65Pa, the molten steel from the refining ladle is injected into the tundish, the temperature of the molten steel in the tundish is controlled at 1585-1595°C, the tundish stopper is opened, and argon is blown through the stopper during pouring, with an argon pressure of 0.1-0.3Mpa.

[0026] Furthermore, after the pouring is completed, a heat-generating agent is added within one minute; the amount of the heat-generating agent is: 0.5kg / t1; t1 is the smelting target value; three minutes later, the heat-generating agent and carbonized rice husk are added again, the amount of the heat-generating agent is: 2.5kg / t1, wherein t1 is the smelting target value; the amount of the carbonized rice husk is: 1.5kg / t1, wherein t1 is the smelting target value.

[0027] A forging produced by the method for producing a steel ingot for a spent fuel dry storage container as described in any one of the above, comprising the following components in percentage by mass: C: 0.055-0.08%, N: 80-120 ppm, Al: 0.015-0.03%, P: ≤0.006%; S: ≤0.003%, Mo: 0.03-0.05%, V: 0.02-0.03%, Nb: 0.01-0.02%, O: ≤15 ppm, and the remainder being iron and unavoidable impurities.

[0028] 3. Beneficial effects

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The manufacturing method of the present invention reduces the carbon content and phosphorus content by placing the batch materials into an electric arc furnace for smelting first, and at the same time can reduce the amount of alloy added to the subsequent refining furnace, effectively avoiding the problem of carbon increase during the refining process; secondly, since the carbon at the end of the electric arc furnace is extremely low and the oxygen content in the steel is very high, the aluminum ingots in the steel-discharging process are quickly precipitated and pre-deoxidized to quickly reduce the oxygen content; and the aluminum-iron alloy added during the refining process is again precipitated and deoxidized, and then diffused and deoxidized by aluminum powder and silicon-calcium powder, so that the oxygen is reduced to less than 50ppm before vacuum degassing; the whole method ensures an extremely low carbon content while taking into account the carbon component segregation problem of large steel ingots, the control of various trace elements is accurate, the purity of molten steel is excellent, and the level of flaw detection and inclusion control is high, laying a solid foundation for subsequent product performance; at the same time, the forgings of the present invention have good strength and excellent low-temperature toughness, that is, on average: Rm (room temperature) ≥ 610Mpa, Rm (240℃) ≥ 560Mpa, -101℃ AKV ≥ 55J;

[0031] (2) The present invention controls the amount of aluminum ingots, aluminum powder and silicon-calcium powder during the smelting process of electric arc furnace and refining furnace, so as to avoid excessive addition of a large amount causing waste of resources and easily increasing impurities, and too small an amount added which does not achieve good deoxidation efficiency; and the amount added is selected according to the rated amount of molten steel in the furnace, further ensuring the maximum utilization of resources; at the same time, the high voltage and low current heating method is adopted to reduce electrode peeling, further reducing the carbon increase problem that may occur during the refining process; after the casting process is completed, the rapid addition of the heating agent can effectively prevent the steel liquid surface from forming a film, further ensuring the forming effect of the subsequent forgings. DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with specific embodiments.

[0033] At present, China has carried out independent research and development of spent fuel dry storage equipment for the second-generation M310 unit, but there is still a blank in the research and development of spent fuel dry storage for the third-generation passive nuclear power unit. The cylinder forgings for a spent fuel dry storage and transportation container, the steel grade for the forgings is: SA350 Gr.LF3.Cl2, the delivery tonnage is about 59 tons, and the double vacuum steel ingot tonnage needs to reach 200 tons. The wall thickness of the forging quenching and tempering is 290mm. There is no precedent in China. The forgings are required to have good strength and excellent low-temperature toughness. The material alloy content is low and the hardenability is limited. In order to meet the performance of thick-walled forgings, the material needs to be ultra-low carbon, micro-alloyed and ultra-pure. The difficulty in manufacturing this large steel ingot is that the C content is extremely low (C≤0.08%, and it is not suitable for smelting with conventional C removal equipment such as AOD and VOD), and the control range is extremely narrow. At the same time, under the condition of meeting the low carbon requirement, high requirements are imposed on harmful elements such as O and S, many alloy elements, and a very narrow control range for some trace elements, which brings great difficulty to the manufacturing. Therefore, the present application provides a method for manufacturing a 200-ton and large steel ingot for a spent fuel dry storage container, which can ensure its excellent performance while being easy to manufacture.

[0034] Example 1

[0035] A method for manufacturing a steel ingot for a spent fuel dry storage container comprises the following steps:

[0036] S1: Ingredients: Use the following components in percentage by mass: 55-65% high-quality carbon scrap steel, 20-25% carbon steel scrap, 20-30% high-quality pig iron, and 2.5% electrolytic nickel; specifically, the composition of the high-quality carbon scrap steel must satisfy Mo≤0.05%, P≤0.010%, S≤0.010%, Cr≤0.030%, and Cu≤0.030%; the composition of the high-quality pig iron must satisfy P≤0.030%, S≤0.030%, As≤0.001%, Sn≤0.001%, and Sb≤0.001%

[0037] S2: Smelting in an electric arc furnace for decarburization and dephosphorization; when the smelting temperature of the electric arc furnace reaches above 1670°C, the smelted steel, i.e., molten steel, is placed in a refining ladle, and the refractory bricks of the refining ladle use low-carbon magnesium carbon bricks (carbon content <8%) to avoid the problem of carbon increase during the refining process; when the steel is put to 20-30 tons, aluminum ingots are added; when the steel is put after completion, lime is added; specifically, the ingredients of step S1 are put into an electric arc furnace for smelting, and the decarburization is ≤0.02% and the dephosphorization is ≤0.003% during the smelting process; and further, the amount of aluminum ingots added is: 3-5kg / t, t is the rated amount of molten steel in the electric arc furnace; the amount of lime added is 500-600kg;

[0038] S3: smelting in a refining furnace, after the refining bag reaches the heating station, adding aluminum-iron alloy, slag (the slag includes lime and fluorite), aluminum powder and silicon-calcium powder; specifically, the amount of aluminum-iron alloy added is: 200-250kg, the lime in the slag is 2000-2500kg, and the fluorite is 400-500kg; the amount of aluminum powder is: 2.0-3.0kg / t, and the amount of silicon-calcium powder is: 1.0-1.5kg / t, t is the rated molten steel volume of the electric arc furnace; in step S2 and step S3, the amount of aluminum ingot, aluminum powder and silicon-calcium powder is controlled to avoid excessive amount of addition causing waste of resources and easy increase of impurities, and too small amount of addition not achieving good deoxidation efficiency; and the amount added is selected according to the rated molten steel volume in the furnace to further ensure the maximum utilization of resources;

[0039] S4: Use maximum voltage and low current to heat up to 1600℃~1620℃, and take samples every 10 minutes to avoid errors caused by short time intervals and little difference in test results; if the time interval is too long, it is difficult to stop the power-on heating in time, which will affect the follow-up; if the carbon content reaches 0.05%, stop the power-on heating; specifically, in this step, the heating method adopts the aluminothermic method to heat up: add 300~350kg of aluminum ingots, insert an oxygen pipe to blow oxygen for 3~4min; and when blowing oxygen, keep the verticality of the oxygen pipe greater than 75°, and avoid the oxygen jet blowing to the wall of the refining bag; the aluminothermic method can effectively reduce the carbon increase problem in the refining process; and the high voltage and low current method is used for temperature control, which can reduce electrode peeling, increase the service life of the electrode and ensure stable operation;

[0040] S5: After heating to 1640℃~1660℃, add Ni alloy, Mo alloy, Mn alloy and aluminum powder to continue reduction; Mn is one of the main elements that refines grains and improves the toughness of steel. Mn can reduce the cementite that appears at the grain boundary after slow cooling, especially for hot rolling and normalizing steel. Adding a small amount of Mn can stabilize the oxygen elements in the steel, providing conditions for the stable yield of subsequent easily oxidized element alloys and trace element alloys; Ni is a pure solid solution element in steel, which has the effect of significantly reducing the Due to the cold brittle transition temperature, Ni forms an infinite solid solution with iron, and Ni refines the ferrite grains through its adsorption in the grains, thereby improving the impact toughness of the steel; Mo can improve the hardenability of the steel; since Ni alloy and Mn alloy are refractory and non-oxidizable alloys, high temperature is required to help them melt quickly, so such alloys are added after the temperature is raised to 1640℃~1660℃; and the amount of aluminum powder in this step is: 0.5kg / t; where t is the rated amount of molten steel in the electric arc furnace, and diffusion deoxidation is carried out by aluminum powder;

[0041] S6: After continuing to heat up to 1660℃~1680℃, take slag sample, add V-Fe alloy, Nb-Fe alloy and Al-Fe alloy after slag whitening, wherein V-Fe alloy is added according to mass fraction of V: ​​0.02%, Nb-Fe alloy is added according to mass fraction of Nb: 0.025%, and Al-Fe alloy is added according to mass fraction of Al: 0.05~0.08% (the above alloys are added without burning loss);

[0042] S7: perform vacuum degassing operation; before performing this step, carbon powder can be appropriately added according to the carbon content, based on the smelting target value, ignoring the burn-off, to make the carbon-oxygen reaction in the steel more intense during VD and achieve the best deoxidation effect; during vacuum degassing operation, the argon blowing flow rate is adjusted to 200-250LN / min, the vacuum degree is ≤65Pa, and the effective time is 30-35min, which is the effective time starting from the vacuum degree of 65Pa;

[0043] S8: After the vacuum degassing operation is completed, sampling is performed to adjust the composition slightly, and nitrogen blowing is started at the same time, with a nitrogen blowing flow rate of 300-350LN / min and a nitrogen blowing time of 25-30min, and N: 200-250ppm; Al: 0.025-0.035%; at the same time, it is explained here that the manufacturing method can be divided into two refining packages according to the smelting target value, and the adjustment at this time also includes adjusting the carbon content of the first package to: 0.080-0.085%; adjusting the carbon content of the second package to 0.045-0.055%, and the two packages of molten steel control different carbon contents, and reverse segregation control is performed to reduce carbon segregation of the ingot; then the temperature is adjusted to 1630℃-1635℃ before hanging out for pouring;

[0044] S9: Vacuum pouring of steel ingot; place the steel ingot mold in a vacuum tank, maintain the vacuum degree ≤65Pa, use argon to replace air in the tundish, the argon blowing pressure is 2~3Mpa, the time is ≥10min, the molten steel from the refining ladle is injected into the tundish, the molten steel temperature in the tundish is controlled at 1585~1595℃, the tundish plug rod is opened, and pouring is performed at full speed. During pouring, the plug rod is blown with argon, and the argon pressure is 0.1~0.3Mpa; further, after the pouring is completed, a heating agent is added within one minute. The rapid addition of the heating agent can effectively prevent the steel liquid from forming a film, and further ensure the forming effect of the subsequent forgings; the amount of the heating agent is: 0.5kg / t1; t1 is the smelting target value; three minutes later, the heating agent and carbonized rice husk are added again, the amount of the heating agent is: 2.5kg / t1, t1 is the smelting target value; the amount of the carbonized rice husk is: 1.5kg / t1, t1 is the smelting target value

[0045] S10: After demoulding, the forgings are hot-sent to the forging workshop for forging to obtain forgings.

[0046] The manufacturing method of the present invention reduces the carbon content and phosphorus content by placing the batched materials into an electric arc furnace for smelting first, and can also reduce the amount of alloy added to the subsequent refining furnace, effectively avoiding the problem of carbon increase in the refining process; secondly, since the carbon at the end of the electric arc furnace is extremely low and the oxygen content in the steel is very high, the aluminum ingots in the steel-releasing process are quickly precipitated and pre-deoxidized to quickly reduce the oxygen content; and the aluminum-iron alloy added in the refining process is again precipitated and deoxidized, and then aluminum powder and silicon-calcium powder are diffused and deoxidized, so that the oxygen is reduced to less than 50ppm before vacuum degassing; the whole method ensures an extremely low carbon content while taking into account the carbon component segregation problem of large steel ingots, the trace elements are accurately controlled, the purity of the molten steel is excellent, and the level of flaw detection and inclusion control is high, laying a solid foundation for the subsequent product performance; at the same time, the whole method is simple to prepare, the process is convenient, and it is easy to produce in large quantities.

[0047] A forging made by the above-mentioned method for manufacturing a steel ingot for a spent fuel dry storage container comprises the following components in mass percentage: C: 0.055-0.08%, N: 80-120ppm, Al: 0.015-0.03%, P: ≤0.006%; S: ≤0.003%, Mo: 0.03-0.05%, V: 0.02-0.03%, Nb: 0.01-0.02%, O: ≤15ppm, and the rest is iron and inevitable impurities. At the same time, the low-temperature forging of the present invention not only meets the requirements of normal temperature strength, stable structure at low temperature, good welding performance and processing performance and necessary physical properties, but also has a great guarantee of low-temperature toughness, that is, on average: Rm (room temperature) ≥610Mpa, Rm (240℃) ≥560Mpa, -101℃ AKV ≥55J.

[0048] Example 2

[0049] In this embodiment, a specific example is given, taking a steel ingot for a spent fuel storage and transportation cylinder forging of a certain batch, the steel grade is SA350 Gr.LF3.Cl2, the ingot shape is 180t, two furnaces are cast together, and the rated molten steel volume of each furnace is 90t. The specific preparation method is as follows:

[0050] S1: Ingredients: 57t of high-quality carbon scrap steel, 20t of carbon steel scraps, 20t of high-quality pig iron, and 2.7t of electrolytic Ni;

[0051] S2: Electric arc furnace smelting, C removal: 0.01%, P removal: 0.002%, temperature 1675℃, put the steel into refining bag, when the steel reaches 20 tons, add 270kg Al ingot, after the steel is put, add 500kg lime;

[0052] S3: Smelting in a refining furnace, after the refining bag reaches the heating station, add 200kg of aluminum-iron alloy, slag materials: 2500kg of lime, 500kg of fluorite; add 180kg of aluminum powder and 90kg of calcium silicon powder;

[0053] S4: Use maximum power to raise the temperature to about 1600℃, take samples every 10 minutes, and after 40 minutes, C: 0.04%;

[0054] S5: After heating to 1645°C, add Ni alloy, Mo alloy, Mn alloy, add 45kg Al powder, and continue reduction;

[0055] S6: After continuing to heat up to 1670°C, take a slag sample, the slag is white; add 55kg of V-Fe alloy, 37kg of Nb-Fe alloy, and 100kg of Al-Fe alloy;

[0056] Before VD, according to the C content, the first package of molten steel C: 0.065%, add 20kg of C powder, the second package C: 0.04% add 10kg of carbon powder;

[0057] S7: The ladle is moved to the degassing station for vacuum degassing (VD). During the VD process, the argon blowing flow rate is adjusted to ~250LN / min, and the timing starts when the vacuum degree reaches 65Pa, with an effective time of 30min.

[0058] S8: After VD is completed, take samples, fine-tune the composition, and start nitrogen blowing at the same time. The nitrogen blowing flow rate is ~350LN / min, and the nitrogen blowing time is ~30min. Take samples, N: 2200ppm, adjust Al: 0.025~0.035%, the first package C: 0.085%, the second package C: 0.050%; adjust the temperature to 1635℃, and lift out for casting;

[0059] S9: Vacuum pouring of steel ingots, vacuum degree 45Pa, argon is used to replace air in the tundish, argon blowing pressure 2Mpa, time 10 minutes; molten steel from the refining ladle is poured into the tundish, the temperature of the molten steel in the tundish is measured at 1590℃, the tundish plug rod is opened, and pouring is carried out at full speed, and argon is blown on the plug rod during pouring, and the argon pressure is 0.1-0.3Mpa; after the pouring is completed, 90kg of exothermic agent is added within 1min, 450kg of exothermic agent is added after 3 minutes, and then 270kg of carbonized rice husk is added;

[0060] S10, after demoulding, hot forging workshop forging is carried out to obtain forgings. The forgings are sampled, and the composition all meets the design internal control requirements, C: 0.075%, N: 100ppm, Al: 0.020%, P: 0.005%, S: 0.001%, Mo: 0.04%, V: 0.025%, Nb: 0.015%, O: 8ppm, and no defects larger than 1mm are found in the forgings UT flaw detection.

[0061] The examples described in the present invention are merely descriptions of the preferred implementation modes of the present invention, and are not intended to limit the concept and scope of the present invention. Without departing from the design concept of the present invention, various modifications and improvements made to the technical solutions of the present invention by engineers and technicians in this field should all fall within the protection scope of the present invention.

Claims

1. A method for manufacturing a steel ingot for a spent fuel dry storage container, characterized in that: The following steps are involved: S1: Ingredients: Use the following components in mass percentage: 57.1% high-quality carbon scrap steel, 20.1% carbon steel scrap, 20.1% high-quality pig iron, and 2.7% electrolytic nickel; the composition of high-quality carbon scrap steel meets Mo≤0.05%, P≤0.010%, S≤0.010%, Cr≤0.030%, Cu≤0.030%; the composition of high-quality pig iron meets P≤0.030%, S≤0.030%, As≤0.001%, Sn≤0.001%, Sb≤0.001%; S2: Smelting in an electric arc furnace for decarbonization and dephosphorization; when the smelting temperature of the electric arc furnace reaches above 1670℃, the smelted steel is placed in a refining bag. When the steel reaches 20-30 tons, aluminum ingots are added; when the steel is finished, lime is added; S3: Smelting in a refining furnace, after the refining bag is brought to the heating station, adding aluminum-iron alloy, slag, aluminum powder and calcium silicon powder; the slag includes lime and fluorite; S4: Raise the temperature to 1600℃~1620℃, take samples during the process, and stop heating if the carbon content reaches 0.05%; S5: After continuing to heat up to 1640℃~1660℃, Ni, Mo, Mn alloy and aluminum powder are added to continue reduction; S6: After continuing to heat up to 1660℃~1680℃, take slag samples, add V-Fe alloy, Nb-Fe alloy and Al-Fe alloy after the slag is white; S7: perform vacuum degassing operation; S8: After the vacuum degassing operation is completed, samples are taken for composition adjustment, and nitrogen blowing is started at the same time. The temperature is adjusted to 1630℃~1635℃ and then the casting is hoisted out; S9: Vacuum casting of steel ingot; S10: After demoulding, the forgings are hot-sent to the forging workshop for forging to obtain forgings.

2. The method for manufacturing a steel ingot for a spent fuel dry storage container according to claim 1, characterized in that: The steel grade of the steel ingot for the spent fuel dry storage container is SA350 Gr.LF3.Cl2, the ingot shape is 180t, and two furnaces are cast together, with a rated molten steel volume of 90t per furnace. The specific preparation method is as follows: S1: Ingredients: 57t of high-quality carbon scrap steel, 20t of carbon steel scraps, 20t of high-quality pig iron, and 2.7t of electrolytic Ni; S2: Electric arc furnace smelting, C removal: 0.01%, P removal: 0.002%, temperature 1675℃, put the steel into refining bag, when the steel reaches 20 tons, add 270kg Al ingot, after the steel is put, add 500kg lime; S3: Smelting in a refining furnace, after the refining bag reaches the heating station, add 200kg of aluminum-iron alloy, slag materials: 2500kg of lime, 500kg of fluorite; add 180kg of aluminum powder and 90kg of calcium silicon powder; S4: Use maximum power to raise the temperature to about 1600℃, take samples every 10 minutes, after 40 minutes, C: 0.04%; S5: After heating to 1645°C, add Ni alloy, Mo alloy, Mn alloy, add 45kg Al powder, and continue reduction; S6: After continuing to heat up to 1670°C, take a slag sample, the slag is white; add 55kg of V-Fe alloy, 37kg of Nb-Fe alloy, and 100kg of Al-Fe alloy; Before VD, according to the C content, the first package of molten steel C: 0.065%, add 20kg of C powder, the second package C: 0.04% add 10kg of carbon powder; S7: The ladle is moved to the degassing station for vacuum degassing operation VD. During the VD process, the argon blowing flow rate is adjusted to 250LN / min, and the timing starts when the vacuum degree reaches 65Pa, and the effective time is 30min; S8: After VD is completed, take samples, fine-tune the composition, and start nitrogen blowing at the same time. The nitrogen blowing flow rate is 350 LN / min, and the nitrogen blowing time is 30 minutes. Take samples, N: 2200ppm, adjust Al: 0.025~0.035%, the first package C: 0.085%, the second package C: 0.050%; adjust the temperature to 1635℃, and lift out for casting; S9: Vacuum pouring of steel ingots, vacuum degree 45Pa, argon is used to replace air in the tundish, argon blowing pressure 2Mpa, time 10 minutes; molten steel from the refining ladle is poured into the tundish, the temperature of the molten steel in the tundish is measured at 1590℃, the tundish plug is opened, and pouring is carried out at full speed, and argon is blown on the plug during pouring, and the argon pressure is 0.1~0.3MPa; after pouring, 90kg of exothermic agent is added within 1min, 450kg of exothermic agent is added after 3 minutes, and then 270kg of carbonized rice husk is added; S10, after demoulding, hot-send to forging workshop for forging to obtain forgings.

3. The method for manufacturing a steel ingot for a spent fuel dry storage container according to claim 1, characterized in that: The heating method in step S4 is to use the aluminothermic method: add 300-350 kg of aluminum ingots, insert an oxygen tube to blow oxygen for 3-4 minutes; and during the heating period, sample once every 10 minutes, and stop the power-on heating if the carbon content reaches 0.05%.

4. The method for manufacturing a steel ingot for a spent fuel dry storage container according to claim 3, characterized in that: When performing oxygen blowing operation, keep the verticality of the oxygen pipe greater than 75° and avoid the oxygen jet blowing to the ladle wall.

5. The method for manufacturing a steel ingot for a spent fuel dry storage container according to claim 1, characterized in that: When the vacuum degassing operation is performed in step S7, the argon blowing flow rate is adjusted to 200-250 LN / min, the vacuum degree is ≤65Pa, and the effective time is 30-35min, which is the effective time starting from when the vacuum degree reaches 65Pa.

6. The method for manufacturing a steel ingot for a spent fuel dry storage container according to claim 1, characterized in that: In step S9, the ingot mold is placed in a vacuum tank, the vacuum degree is maintained at ≤65Pa, the molten steel from the refining ladle is injected into the tundish, the temperature of the molten steel in the tundish is controlled at 1585-1595°C, the tundish stopper is opened, and argon is blown through the stopper during pouring, with the argon pressure being 0.1-0.3Mpa.

7. The method for manufacturing a steel ingot for a spent fuel dry storage container according to claim 6, characterized in that: After pouring is completed, add the heat-generating agent within one minute; the amount of the heat-generating agent is: 0.5 kg / t1; t1 is the smelting target value; three minutes later, add the heat-generating agent and carbonized rice husk again, the amount of the heat-generating agent is: 2.5 kg / t1, t1 is the smelting target value; the amount of carbonized rice husk is: 1.5 kg / t1, t1 is the smelting target value.

Citation Information

Patent Citations

  • Special steel base alloy material for reactor spent fuel storage and transportation and preparation method thereof

    CN106086692A

  • SA517GrF steel plate for spent fuel storage tank and production method thereof.

    CN111041385A

  • Novel manufacturing technology of large-sized carburized bearing steel G20Cr2Ni4A for wind electricity

    CN104532102A

  • Method for producing circular sulfur-resistant pipeline steel billet for oil and gas collection and transmission

    CN105018855A

  • Smelting method for 10Cr11Co3W3NiMoVNbNB low-carbon low-silicon low-aluminum high-boron steel

    CN106381441A