A preparation method of silicon-carbon negative electrode material and silicon-carbon negative electrode and application thereof
By preparing a core-shell structure of silica-coated carbon spheres and performing magnesium thermal reduction, porous NC@Si nanospheres are formed, which solves the problems of volume change and conductivity of silicon-based anodes and improves the cycle stability and electrochemical performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202310180120.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-02-28
AI Technical Summary
Existing silicon-based anodes in lithium-ion batteries suffer from structural instability, poor cycle stability, and poor electrochemical performance due to their large volume changes and low conductivity.
By employing a size-constrained and conductive carbon composite strategy, a core-shell structure of silica-coated carbon spheres was prepared via the sol-gel method. Combined with a magnesothermic reduction reaction, NC@Si nanospheres were formed. Polydopamine nanospheres were then used to enhance the hydrolysis efficiency and steric hindrance effect of SiO2, resulting in porous NC@Si nanospheres.
It effectively improves the volume expansion problem of silicon-based anodes, enhances conductivity and cycle stability, and strengthens the structural integrity and electrochemical performance of the electrode.
Smart Images

Figure CN116262615B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicon-carbon negative electrode material preparation, and in particular to a method for preparing a silicon-carbon negative electrode material, a silicon-carbon negative electrode and applications. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, long cycle life, and environmental friendliness. They are widely used in portable electronic products, power tools, electric vehicles, and even in the aerospace field. The performance of negative electrode materials is crucial to improving the energy density of lithium-ion batteries. At present, high-performance lithium-ion battery systems require anode materials with high specific capacity and excellent rate performance. But commercial graphite-based negative electrode materials (372mAh g-1) are far from enough. Researchers have studied new negative electrode materials for lithium-ion batteries and found that among non-carbon negative electrode materials, silicon has the highest specific capacity (Li22Si5 about 4200mAh g-1), low operating voltage (<0.5V vs.Li / Li+), abundant sources (second only to oxygen in the earth's crust) and easy access, so it has received extensive research attention and is considered to be an ideal choice for the next generation of lithium-ion batteries. However, huge volume changes (>300%) are an inevitable problem for silicon-based anodes during repeated lithiation / delithiation processes, resulting in severe pulverization of active materials, followed by the continuous formation of unstable SEI films and consumption of electrolytes. This dreadful process will eventually lead to rapid capacity decay and poor cycling stability. In addition, the inherent low conductivity also seriously hinders its practical application. In order to effectively alleviate these problems, it is of great significance to develop a facile strategy for silicon-based anodes with stable structure and improved electrochemical performance.
[0003] So far, several different strategies have been proposed to address the relevant challenges. Currently, the most effective approach is to design well-designed silicon-based materials with unique structures such as nano-, porous and composite. Some studies have demonstrated that minimizing the particle size of silicon to the nanoscale is a successful approach to relieve the mechanical strain caused by volume change and maintain the structural integrity of silicon-based anodes, thereby improving the cycling stability of Si. The enhancement of cycling stability is attributed to the large specific surface area, reduced lithium ion diffusion length, and pores or voids introduced in the nanostructure. However, the fabrication of nanoscale silicon particles always requires a complex process, which is opposed by large-scale and low-cost applications. Nanostructured Si materials are usually synthesized by chemical vapor deposition (CVD) or liquid chemical methods, which usually involve the use of toxic silane or SiCl4 and have low yields, limiting their practical applications. Magnesium thermal reduction has received particular attention since it was reported by Bao et al. SiO2 can be reduced to Si by Mg through the reaction: SiO2(s)+2Mg(g)→Si(s)+2MgO(s). This discovery provides a facile and environmentally friendly method for synthesizing nano-silicon materials. In addition, since SiO2 is abundant in nature, nano-silicon can be mass-produced using this method. Recent studies have found that nanostructured Si materials prepared by magnesium thermal reduction exhibit excellent cycle stability and rate performance. However, it is not feasible to rely solely on silicon nano-materialization. To this end, researchers have explored a variety of improvement schemes, the most successful of which is to use carbon media as a stress buffer substrate for silicon to adapt to the volume change of silicon and enhance conductivity. Carbon materials have excellent structural stability and electrochemical activity, and have good compatibility with silicon. The two can be in close contact after being composited. The presence of silicon increases the specific capacity, and the presence of carbon media suppresses the volume effect of silicon, forming a conductive network and avoiding the agglomeration of nano-silicon. It is thus expected to enhance the cycle performance and high rate capability of Si anodes.
[0004] In view of the above analysis of the current situation of silicon anode, here, this case hopes to solve the two inherent defects of silicon, namely large volume expansion and low intrinsic conductivity, through a simple and effective synergistic strategy of size confinement and conductive carbon composite. Summary of the invention
[0005] In view of this, the purpose of the present invention is to propose a method for preparing a silicon-carbon negative electrode material, a silicon-carbon negative electrode and its application, and to utilize the synergistic effect of size restriction and conductive carbon composite to effectively improve silicon defects.
[0006] According to one aspect of the present invention, a method for preparing a silicon-carbon negative electrode material is provided, comprising: using a nitrogen-containing alkaline carbon source matrix as a carbon source to prepare a core-shell structure composite material of silicon dioxide-coated carbon balls; using the core-shell structure composite material of silicon dioxide-coated carbon balls as a precursor, performing a magnesium thermal reduction reaction to obtain NC@Si nanospheres.
[0007] In the above technical scheme, ultrafine and high-purity SiO2 quantum dots are anchored on polydopamine (PDA) nanospheres by a sol-gel method and NC@Si composite materials are prepared by magnesium thermal reduction. The increase in alkalinity in the process will simultaneously promote the increase in the size of the hydrolysis and polycondensation products of TEOS and the increase in the SiO2 content therein, which will lead to an increase in the size of Si particles in the subsequent magnesium thermal reduction products, accompanied by an increase in Si content. Although the increase in Si content is conducive to obtaining a higher initial discharge capacity, the corresponding volume expansion effect caused by the large size leads to a dramatic capacity decay. In order to improve The performance of Si negative electrode prepared by sol-gel method-magnesium thermal reduction method is improved by introducing nitrogen-containing alkaline carbon source matrix based on the hydrolysis mechanism of Si-based metal alkoxide and polymer steric hindrance effect. Sol-gel method.
[0008] In some embodiments, the nitrogen-containing basic carbon source matrix includes: polydopamine nanospheres.
[0009] In some embodiments, the method of using a nitrogen-containing alkaline carbon source matrix as a carbon source to prepare a core-shell structure composite material of silicon dioxide-coated carbon spheres also includes:
[0010] Trimethylaminomethane and dopamine hydrochloride were dissolved in deionized water and stirred at room temperature for several hours; polydopamine nanospheres were obtained by centrifugation and filtration and washed with deionized water several times.
[0011] In the above technical solution, the present invention introduces PDA (polydopamine nanospheres, the same below) as an alkaline carbon source matrix, based on the hydrolysis mechanism of Si-based metal alkoxides and the polymer steric hindrance effect, to improve The sol-gel method introduces PDA, an alkaline carbon source matrix, and utilizes the local high alkaline environment of PDA to improve the efficiency of TEOS hydrolysis to silicate monomers on the PDA surface, and utilizes the steric hindrance effect of PDA polymer to induce a large number of ultrafine high-purity SiO2 quantum dots to form on the PDA matrix. The PDA nanosphere composite precursor anchored with ultrafine and high-purity SiO2 quantum dots was explored. NC@Si nanospheres rich in high-purity nano-Si and having a porous structure were obtained by magnesium thermal reduction of the PDA@SiO2 precursor. For the entire NC@Si nanosphere, the nano-Si quantum dots tightly bound by the carbon matrix have only non-destructive volume expansion, which is conducive to the formation of a stable SEI layer. In addition, polydopamine after magnesium thermal reduction tends to form nitrogen-doped carbon, which is a good electronic conductor, and multi-point strong electrical contact also provides a basis for rapid Li + Diffusion and charge transfer provide ample conductive pathways, facilitating high charge capacity at high current density.
[0012] In some embodiments, the method of using a nitrogen-containing alkaline carbon source matrix as a carbon source to prepare a core-shell structure composite material of silicon dioxide-coated carbon spheres specifically includes:
[0013] The alkaline carbon source matrix is dispersed in a mixed solution of deionized water and ammonia water under ultrasonic action to obtain a carbon source suspension A, and the pH value of the carbon ball suspension is adjusted to 8-10 with ammonia water;
[0014] Adding ethyl orthosilicate to anhydrous ethanol under stirring to form solution B;
[0015] The solution B is quickly added to the suspension solution A and slowly stirred for several hours; the suspension is separated by centrifugation, repeatedly washed with anhydrous ethanol, and vacuum dried at 80° C. for several hours to obtain a core-shell structure composite material of silicon dioxide-coated carbon spheres.
[0016] In some embodiments, in the mixed solution of deionized water and ammonia water, the volume ratio of deionized water to ammonia water is 11-12:1;
[0017] The volume ratio of the tetraethyl orthosilicate to anhydrous ethanol is 1:14-15.
[0018] In the above technical solution, the traditional The sol-gel method obtains monodisperse SiO2 nanospheres in a simple way without using any additives or surfactants. In a system with low ammonia content, tetraethyl orthosilicate (TEOS) first undergoes hydrolysis reaction. During the hydrolysis process, the alkoxy group -OR cannot be completely replaced by the hydroxyl group -OH, resulting in partial hydrolysis products being biased towards Si(OR). 4-n (OH) n Such polymers cannot form SiO2 nanospheres with high purity in the subsequent dehydration reaction, as shown in equations (1) and (2).
[0019] Hydrolysis reaction: Si(OR)4+4H2O→Si(OR)n(OH) 4-n +nC2H5OH Formula (1)
[0020] Dehydration reaction: Si(OR)n(OH) 4-n →SiO(OH)2+H2O→SiO2+2H2O (cannot occur) Formula (2)
[0021] As the ammonia content increases, the OHˉ ion concentration in the system increases, the hydrolysis reaction rate accelerates, and the hydrolysis product is basically completely Si(OH)4. In the subsequent dehydration reaction, not only can higher purity SiO2 nanospheres be formed, but the polymerization rate of silicate monomers is also increased, which promotes the nucleation rate and particle growth rate, thereby generating SiO2 nanospheres with larger particle size.
[0022] Hydrolysis reaction: Si(OR)4+4H2O→Si(OH)4+4C2H5OH Formula (3)
[0023] Dehydration reaction: Si(OH)4→SiO(OH)2+H2O→SiO2+2H2O Formula (4)
[0024] Since the introduction of PDA exhibits a steric hindrance effect on the growth of SiO2, the individually grown SiO2 nanospheres can also maintain a small particle size of about 125nm in diameter.
[0025] In some embodiments, the core-shell structure composite material of silicon dioxide-coated carbon spheres is used as a precursor to perform magnesium thermal reduction reaction to obtain NC@Si nanospheres, specifically including:
[0026] The silicon dioxide-coated polydopamine core-shell nanocomposite material was mixed with sodium chloride and fine magnesium powder and ground, placed on a corundum ark, sealed with a cover and placed in a tube furnace at a temperature of 5°C min -1 Heat to 700℃ and keep warm for 3h;
[0027] Add hydrochloric acid dropwise to the product powder, wherein the concentration of the hydrochloric acid is 1-2 mol / L and the amount of the hydrochloric acid added is 200-250 mL per gram of powder, stir for 30-60 minutes and then filter and collect the filter cake;
[0028] The filter cake was added into HF solution to remove byproducts and residual SiO2, stirred for several minutes, washed with deionized water for 4 times, and vacuum dried at 80°C for 12 hours to obtain NC@Si nanospheres.
[0029] In the above technical scheme, NC@Si nanospheres were obtained by reducing PDA@SiO2 by fine Mg powder in Ar atmosphere at 700°C. During the conversion from PDA@SiO2 to NC@Si, the spherical shape and size were retained without obvious deformation or collapse and showed a rough surface.
[0030] In some embodiments, the weight ratio of the silica-coated polydopamine core-shell nanocomposite to sodium chloride and magnesium powder is 1:1:1;
[0031] The particle size of the fine magnesium powder is 100 to 200 meshes.
[0032] In the above technical solution, the purpose of selecting fine magnesium powder is: the use of fine magnesium powder can make the magnesium powder and silicon dioxide powder contact more fully during the mixing process, the magnesium thermal reduction efficiency is higher, and the purity and yield of nano-silicon are improved, thereby increasing the specific capacity. In order to improve the magnesium thermal reduction Si electrode at 0.1A g without changing other conditions and only changing the coarseness of the magnesium powder, -1Cycling performance at different current densities.
[0033] According to another aspect of the present invention, a silicon-carbon negative electrode material is provided, which is prepared by the above-mentioned method for preparing a silicon-carbon negative electrode material.
[0034] According to another aspect of the present invention, an application of a silicon-carbon negative electrode material in a composite electrode is provided, and the material of the composite electrode includes the above-mentioned silicon-carbon negative electrode material.
[0035] According to another aspect of the present invention, an application of a silicon-carbon negative electrode material in a lithium battery is provided, and the lithium battery electrode material comprises the above-mentioned silicon-carbon negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0037] Figure 1 It is a schematic flow chart of an embodiment of a method for preparing a silicon-carbon negative electrode material of the present invention;
[0038] Figure 2 The morphology of SiO2 nanospheres at different ammonia concentrations according to the embodiment of the present invention is shown in Figure 1. a) SEM of SiO2 nanospheres at low ammonia concentration. b) SEM of SiO2 nanospheres at medium ammonia concentration. c) SEM of SiO2 nanospheres at high ammonia concentration. ;
[0039] Figure 3 Schematic diagram of the cycle performance of Si electrode at different ammonia concentrations at a current density of 0.1A-1 in an embodiment of the present invention;
[0040] Figure 4 a) Coarse magnesium powder magnesium thermal reduction Si electrode in 0.1Ag -1 Schematic diagram of cycling performance under current density. b) Fine magnesium powder magnesium thermal reduction Si electrode at 0.1A g -1 Schematic diagram of cycling performance under current density;
[0041] Figure 5 Schematic diagrams of the morphology and structure characterization of nanospheres according to the embodiments of the present invention. a) SEM of PDA solid nanospheres. b) SEM of PDA@SiO2 nanospheres. c) SEM of NC@Si nanospheres. d) HRTEM image of PDA@SiO2 nanospheres. e) HADDF and EDX spectra of PDA@SiO2 nanospheres;
[0042] Figure 6 a) HRTEM and SAED images of NC@Si solid nanospheres of the embodiment of the present invention. e) HADDF and EDX spectra of NC@Si nanospheres;
[0043] Figure 7 a) PDA, pure Si, NC@Si electrode in 0.1Ag -1 Schematic diagram of cycling performance under current density. b) Schematic diagram of rate performance of PDA, pure Si, and NC@Si electrodes at different current densities;
[0044] Figure 8 These are the electrode SEM images of a) pure Si electrode and b) NC@Si electrode after 100 cycles. DETAILED DESCRIPTION
[0045] The present invention will be further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention. Similarly, the following examples are only partial embodiments of the present invention rather than all embodiments, and all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.
[0046] The present invention provides a method for preparing a silicon-carbon negative electrode material, which utilizes the synergistic effect of size restriction and conductive carbon composite to effectively improve silicon defects. Figure 1 , the process is as follows:
[0047] S1. Using a nitrogen-containing alkaline carbon source matrix as a carbon source, a core-shell structure composite material of silicon dioxide-coated carbon spheres is prepared;
[0048] S2. Using the core-shell structure composite material of silicon dioxide-coated carbon spheres as a precursor, a magnesium thermal reduction reaction is carried out to obtain NC@Si nanospheres.
[0049] For better explanation, this case is exemplified by specific implementation examples, and the steps include the technical features mentioned in the claims, and no further separate examples are listed. The details are as follows:
[0050] Preparation of polydopamine nanospheres: Trimethylaminomethane (0.6 g) and dopamine hydrochloride (0.5 g) were dissolved in 500 ml of deionized water and stirred at room temperature for 13 hours. Afterwards, the desired precipitate was obtained by centrifugation and washed with deionized water 4 times;
[0051] Preparation of PDA@SiO2 nanospheres: 0.1g of polydopamine (PDA) was dispersed into a mixed solution of deionized water (8.7ml) and ammonia water (0.75ml, 25wt%) under ultrasound (the volume ratio of deionized water to ammonia water was 11.6:1) to obtain PDA suspension A, and the pH value of the carbon sphere suspension was adjusted to 8-10 with ammonia water; then, tetraethyl orthosilicate (TEOS, 1.5ml) was added to anhydrous ethanol (21.7ml, analytical grade) under stirring to form solution B (the volume ratio of tetraethyl orthosilicate to anhydrous ethanol was 1:14.5). Solution B was quickly added to suspension solution A, and then slowly stirred for 12 hours. The suspension was separated by centrifugation, repeatedly washed with anhydrous ethanol, and vacuum dried at 80°C for 12 hours to obtain a core-shell structure composite material of silica-coated carbon spheres;
[0052] Preparation of NC@Si nanospheres: The silicon dioxide-coated polydopamine core-shell nanocomposite material was mixed with sodium chloride and fine magnesium powder (100-200 mesh) and ground, placed on a corundum ark, sealed and placed in a tube furnace at a temperature of 5 °C min -1 The temperature was raised to 700 °C at a rate of 5 °C min -1 The temperature was raised to 700°C and kept for 3 hours. The weight ratio of the PDA@SiO2 nanospheres to sodium chloride and magnesium powder was 1:1:1. Hydrochloric acid was added dropwise to the product powder. The concentration of the hydrochloric acid was 1-2 mol / L. The amount of the addition was 200 mL-250 mL per gram of powder. After stirring for 30-60 minutes, the filter cake was collected by suction filtration. The filter cake was added to HF solution (20 ml, 5%) to remove byproducts and residual SiO2. The filter cake was stirred for 5-10 minutes, then washed with deionized water 4 times, and vacuum dried at 80°C for 12 hours. After that, NC@Si nanospheres were obtained.
[0053] In this embodiment, considering The increase of alkalinity in the process will simultaneously promote the increase of the size of the hydrolysis and polycondensation products of TEOS and the increase of the SiO2 content therein, which will lead to the increase of the Si particle size in the subsequent magnesium thermal reduction product and the increase of the Si content ( Figure 2 Although the increase in Si content is conducive to obtaining a higher initial discharge capacity, the volume expansion effect caused by the corresponding large size leads to a dramatic capacity decay ( Figure 3 ). To improve The performance of Si negative electrode prepared by sol-gel method-magnesium thermal reduction method was improved by introducing PDA, an alkaline carbon source matrix, based on the hydrolysis mechanism of Si-based metal alkoxide and the polymer steric hindrance effect. The sol-gel method introduces PDA, an alkaline carbon source matrix, and utilizes the local high alkaline environment of PDA to improve the efficiency of TEOS hydrolysis to silicate monomers on the PDA surface, and utilizes the steric hindrance effect of PDA polymer to induce a large number of ultrafine high-purity SiO2 quantum dots to form on the PDA matrix. The PDA nanosphere composite precursor anchored with ultrafine and high-purity SiO2 quantum dots was explored. NC@Si nanospheres rich in high-purity nano-Si and having a porous structure were obtained by magnesium thermal reduction of the PDA@SiO2 precursor. For the entire NC@Si nanosphere, the nano-Si quantum dots tightly bound by the carbon matrix have only non-destructive volume expansion, which is conducive to the formation of a stable SEI layer. In addition, polydopamine after magnesium thermal reduction tends to form nitrogen-doped carbon, which is a good electronic conductor, and multi-point strong electrical contact also provides a basis for rapid Li + Diffusion and charge transfer provide ample conductive pathways, facilitating high charge capacity at high current density.
[0054] In this embodiment, by The sol-gel method obtains monodisperse SiO2 nanospheres in a simple way without using any additives or surfactants. In a system with low ammonia content, tetraethyl orthosilicate (TEOS) first undergoes hydrolysis reaction. During the hydrolysis process, the alkoxy group -OR cannot be completely replaced by the hydroxyl group -OH, resulting in partial hydrolysis products being biased towards Si(OR). 4-n (OH) n Such polymers cannot form SiO2 nanospheres with high purity in the subsequent dehydration reaction, as shown in equations (1) and (2).
[0055] Hydrolysis reaction: Si(OR)4+4H2O→Si(OR)n(OH) 4-n +nC2H5OH Formula (1)
[0056] Dehydration reaction: Si(OR)n(OH) 4-n →SiO(OH)2+H2O→SiO2+2H2O (cannot occur) Formula (2)
[0057] As the ammonia content increases, the OHˉ ion concentration in the system increases, the hydrolysis reaction rate accelerates, and the hydrolysis product is basically completely Si(OH)4. In the subsequent dehydration reaction, not only can higher purity SiO2 nanospheres be formed, but the polymerization rate of silicate monomers is also increased, which promotes the nucleation rate and particle growth rate, thereby generating SiO2 nanospheres with larger particle size.
[0058] Hydrolysis reaction: Si(OR)4+4H2O→Si(OH)4+4C2H5OH Formula (3)
[0059] Dehydration reaction: Si(OH)4→SiO(OH)2+H2O→SiO2+2H2O Formula (4)
[0060] like Figure 3 The SEM images shown show that the particle sizes of SiO2 nanospheres prepared at different ammonia contents are approximately 70, 200 and 340 nm, respectively.
[0061] In this embodiment, the introduction of PDA has a steric effect on the growth of SiO2, resulting in the growth of SiO2 nanospheres that can maintain a small particle size, with a diameter of about 125nm ( Figure 4 b). Then, NC@Si nanospheres were obtained by reducing PDA@SiO2 by fine Mg powder under Ar atmosphere at 700 °C. Obviously, during the conversion from PDA@SiO2 to NC@Si, the spherical shape and size were preserved without obvious deformation or collapse and showed a rough surface.
[0062] The purpose of selecting fine magnesium powder: using fine magnesium powder can make the magnesium powder and silicon dioxide powder contact more fully during the mixing process, the magnesium thermal reduction efficiency is higher, and the purity and yield of nano-silicon are improved, thereby increasing the specific capacity. Figure 4 ) is the magnesium powder thermal reduction Si electrode at 0.1A g without changing other conditions and only changing the magnesium powder coarseness. -1 Cycling performance at different current densities.
[0063] In this embodiment, the characterization and analysis results are as follows:
[0064] First, under alkaline conditions, dopamine hydrochloride and trimethylaminomethane were polymerized to form PDA solid nanospheres with a diameter of about 500 nm and a smooth surface ( Figure 5 a). Figure 5 b It can be observed that SiO2 quantum dots are uniformly anchored on the surface of PDA nanospheres, and PDA@SiO2 particles have a uniform spherical morphology, a rough surface, and a diameter of about 600nm. TEM image of PDA@SiO2 ( Figure 5 d) It also proves that PDA nanospheres are uniformly coated with SiO2, and the thickness of the SiO2 shell is about 50nm. Figure 5 e is the STEM image of PDA@SiO2 nanospheres, and the elemental mapping images of Si, C, N and O of PDA@SiO2, EDX, also illustrate the highly uniform distribution characteristics of silicon, carbon, nitrogen and oxygen elements in the composite material. Then, NC@Si nanospheres were obtained by reducing PDA@SiO2 with Mg powder in an Ar atmosphere at 700 °C ( Figure 5c). Obviously, during the conversion process from PDA@SiO2 to NC@Si, the spherical shape and size are preserved without obvious deformation or collapse and showing a rough surface.
[0065] In addition, in TEM ( Figure 6 The shell of the NC@Si particles observed in a) is composed of primary silicon microcrystals with obvious mesoporous characteristics. The lattice fringe spacing points to the (111) plane of polysilicon ( Figure 6 b,c). Selected area electron diffraction (SAED) patterns of NC@Si composites ( Figure 6 d) shows three clear and bright diffraction rings, which reveal the diffraction rings of (111), (220) and (311) polysilicon. Scanning TEM (STEM) images and energy dispersive x-ray elemental mapping of Si, C, N and O are shown in Figure 4. Figure 6 As shown in Figure 5e, this clearly shows that the nitrogen-doped carbon nanospheres are located in the center of the composite material and are uniformly wrapped by Si quantum dots, which also marks the successful preparation of NC@Si nanospheres.
[0066] The PDA, pure Si, and NC@Si electrodes were compared at 0.1 A g -1 The cycle performance after 100 charge and discharge cycles at the current density. Figure 7 As shown in a, pure Si only provides about 129.8 mAh g after 100 cycles. -1 The specific capacity of PDA was only 240.4 mAh g after 100 cycles. -1 The specific capacity of NC@Si electrode was only 26% after 100 cycles. -1 The specific capacity of the battery is 31%, and the capacity retention rate is 31% at 0.5Ag. -1 After 100 cycles, it provides about 292 mAh g -1 The NC@Si structure greatly improves the volume change of Si during cycling, promotes the transfer of electrons and Li+, and improves the integrity and stability of the electrode. In addition, the NC@Si electrode maintains a high CE of nearly 99% throughout the cycle, indicating the formation of a stable SEI. Figure 7 b shows the rate capability of the three materials at different current densities. NC@Si electrode at 0.1, 0.2, 0.5, 1, and 2 A g -1 The current densities of 601, 407, 268, 195 and 118 mAh g -1The high stable reversible capacity of NC@Si electrode is obviously better than that of pure Si electrode. The excellent rate performance of NC@Si shows that the synergistic effect of nano-Si quantum dots and nitrogen-doped carbon can effectively maintain electrode stability even at high current density. When the current density returns to 0.1Ag-1, the reversible capacity of NC@Si electrode can be quickly restored to 495mAhg -1 Once again, the excellent kinetic properties of the NC@Si composite material can be demonstrated. In contrast, the capacity recovery performance of pure Si is very poor.
[0067] In order to more intuitively demonstrate the excellent reversibility and structural stability of NC@Si electrodes, SEM ( Figure 8 ) to evaluate the structural stability of the electrode after repeated lithium-silicon alloying cycles. It is clear that the pure Si electrode ( Figure 8 a) After 100 cycles, serious particle expansion, crushing and cracking occurred. There is a clear difference between the NC@Si electrode and the pure Si electrode. Figure 8 b) Almost no cracks exist. The NC@Si electrode exhibits excellent integrity and better structural stability. These significant differences can be attributed to the good synergy between the nitrogen-doped carbon buffer layer and the ultrafine nano-Si quantum dots, which prevents the fracture of the overall structure and the loss of electrical contact, maintaining the structural stability of the electrode for long-term cycling, thus leading to excellent electrochemical performance.
[0068] Based on the method for preparing NC@Si nanospheres in the above embodiment, this case further proposes a silicon-carbon negative electrode material, an application of a silicon-carbon negative electrode material in a composite electrode, and an application of a silicon-carbon negative electrode material in a lithium battery. The advantages brought by the silicon-carbon negative electrode material have been specifically reflected in the above text and will not be repeated here. Furthermore, the combination method of applying the silicon-carbon negative electrode material to the composite electrode and lithium battery is a conventional technical means, which is not limited in this embodiment.
[0069] The above descriptions are only some embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Any equivalent device or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a silicon-carbon negative electrode material, characterized in that: include: The method uses polydopamine nanospheres as a carbon source to prepare a core-shell structure composite material of silicon dioxide-coated carbon spheres. The method specifically comprises: dispersing the polydopamine nanospheres into a mixed solution of deionized water and ammonia water under ultrasonic action to obtain a carbon source suspension A, and adjusting the pH value of the carbon sphere suspension to 8-10 with ammonia water; adding ethyl orthosilicate to anhydrous ethanol under stirring to form a solution B; and quickly adding the solution B to the suspension solution A and slowly stirring for several hours. The suspension is separated by centrifugation, repeatedly washed with anhydrous ethanol, and vacuum dried at 80° C. for several hours to obtain a composite material of a core-shell structure of carbon spheres coated with silicon dioxide; in the mixed solution of deionized water and ammonia water, the volume ratio of deionized water to ammonia water is 11-12:1; the volume ratio of tetraethyl orthosilicate to anhydrous ethanol is 1:14-15; NC@Si nanospheres were obtained by magnesium thermal reduction reaction using a core-shell structure composite material of silicon dioxide-coated carbon spheres as a precursor.
2. The method for preparing a silicon-carbon negative electrode material according to claim 1, characterized in that: The method uses polydopamine nanospheres as a carbon source to prepare a core-shell structure composite material of silicon dioxide-coated carbon spheres; the method also includes: Trimethylaminomethane and dopamine hydrochloride were dissolved in deionized water and stirred at room temperature for several hours; polydopamine nanospheres were obtained by centrifugation and filtration and washed with deionized water several times.
3. The method for preparing a silicon-carbon negative electrode material according to claim 1, characterized in that: The core-shell structure composite material of silicon dioxide-coated carbon spheres is used as a precursor, and a magnesium thermal reduction reaction is performed to obtain NC@Si nanospheres, specifically including: The silica-coated polydopamine core-shell nanocomposite material was mixed with sodium chloride and fine magnesium powder, ground, placed on a corundum ark, sealed, and placed in a tube furnace at a temperature of 5 °C min -1 Raise the temperature to 700℃ and keep it for 3 hours; Add hydrochloric acid dropwise to the product powder, wherein the concentration of the hydrochloric acid is 1-2 mol / L and the amount of the hydrochloric acid added is 200-250 mL per gram of powder, stir for 30-60 minutes and then filter and collect the filter cake; The filter cake was added into HF solution to remove byproducts and residual SiO2, stirred for several minutes, washed with deionized water for 4 times, and vacuum dried at 80 °C for 12 h to obtain NC@Si nanospheres.
4. The method for preparing a silicon-carbon negative electrode material according to claim 3, characterized in that: The weight ratio of the silicon dioxide-coated polydopamine core-shell nanocomposite material to sodium chloride and magnesium powder is 1:1:1; The particle size of the fine magnesium powder is 100-200 meshes.
5. A silicon-carbon negative electrode material, characterized in that: It is prepared by the method for preparing a silicon-carbon negative electrode material according to any one of claims 1 to 4.
6. Application of a silicon-carbon negative electrode material in a composite electrode, characterized in that: The material of the composite electrode comprises the silicon-carbon negative electrode material as described in claim 5.
7. Application of a silicon-carbon negative electrode material in a lithium battery, characterized in that: The lithium battery electrode material comprises the silicon-carbon negative electrode material as described in claim 5.
Citation Information
Cited By
Low-expansion silicon-carbon negative electrode material and preparation method and application thereof
CN120784340A
A low-expansion silicon-carbon negative electrode material, a preparation method therefor, and an application thereof
CN120784340B