Maleic anhydride-isobutylene copolymer microspheres and preparation method and application thereof

By using a specific ratio of maleic anhydride and isobutylene for polymerization in a protective atmosphere, maleic anhydride-isobutylene copolymer microspheres with clean surfaces and uniform particle sizes are prepared, which solves the problems of complex traditional processes and environmental pollution, and achieves Efficient, environmentally friendly preparation process and wide application.

CN116262803BActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111522526.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-13
Publication Date
2024-10-15
Estimated Expiration
2041-12-13

AI Technical Summary

Technical Problem

The preparation process of traditional maleic anhydride isobutylene copolymer is complicated, the use of reaction solvents leads to environmental pollution and odor problems, and the dispersion stability is poor, which limits the application scope of the material.

Method used

In a protective atmosphere, a specific ratio of maleic anhydride and isobutylene is used to polymerize in a specific reaction medium to prepare maleic anhydride-isobutylene copolymer microspheres with clean surfaces and uniform particle sizes, avoiding the need for emulsifiers and ester solvents. Use simplifies the process and reduces environmental pollution and energy consumption.

Benefits of technology

It achieves the stable uniformity and wide application of polymer microspheres, avoids the odor problem and poor dispersion stability in traditional methods, improves the non-migration and non-precipitation characteristics of the dispersant, and expands the scope of application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116262803B_ABST
    Figure CN116262803B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of polymers, and discloses a maleic anhydride-isobutylene copolymer microsphere and a preparation method and application thereof. The method comprises dissolving a polymerization monomer and an initiator in a medium in a protective atmosphere to obtain a mixed solution and subjecting the mixed solution to polymerization reaction, obtaining a copolymer emulsion suspension, and separating the maleic anhydride-isobutylene copolymer microsphere; the polymerization monomers are maleic anhydride and isobutylene; based on the total weight of the polymerization monomers, the amount of maleic anhydride is 50-90wt%, and the amount of isobutylene is 10-50wt%; the reaction medium is a mixture of a compound shown in formula (1) and an alkane; wherein R1 and R2 are each independently an alkyl group having 1 to 6 carbon atoms. The copolymer microspheres prepared by combining a specific reaction medium with a specific amount of monomers have uniform particle size, are clean and have no odor. The polymer microspheres have the effect of not migrating and not precipitating in polyethylene as a dispersant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of high molecular polymers, and in particular to maleic anhydride-isobutylene copolymer microspheres and a preparation method and application thereof. Background Art

[0002] The copolymer of isobutylene and maleic anhydride is an amphiphilic polymer with good thermal stability and both hydrophilic and lipophilic properties, and is often used as a dispersant. Traditional maleic anhydride isobutylene polymers are generally prepared in aliphatic hydrocarbons, dimethylformamide or ester solvents.

[0003] In the prior art, conventional maleic anhydride copolymers all use some reaction solvents and post-treatment solvents, the preparation process is relatively complicated and many solvents are environmentally unfriendly, and it is generally difficult to obtain microspherical materials. The preparation of such maleic anhydride microsphere materials can also use ester solvents such as isoamyl acetate, but due to the special interaction between the polymer and the ester solvent, and the special smell of the ester solvent, the material will have an odor even if it contains a small amount of residual ester solvent. The presence of the odor limits the application of such materials, and the traditional organic small molecule dispersant is easy to migrate out, resulting in poor dispersion stability.

[0004] Therefore, developing a reasonable and simple preparation process for maleic anhydride copolymers is beneficial to the promotion and application of such polymers. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems of the prior art that the process flow is long, the microsphere polymer is difficult to remove the reaction solvent, there is a special odor, which leads to a limited application range and poor dispersion stability. A maleic anhydride-isobutylene copolymer microsphere and a preparation method and application thereof are provided. The maleic anhydride-copolymer microsphere has a clean surface and a uniform particle size. No polluting auxiliary agents such as emulsifiers are used in the preparation process, which significantly reduces the environmental pollution caused by the preparation process. There is no special odor of ester solvents, and the polymer does not need to be washed and purified. The preparation process is environmentally friendly, economical and low in energy consumption.

[0006] In order to achieve the above-mentioned object, the first aspect of the present invention provides a method for preparing maleic anhydride-isobutylene copolymer microspheres, characterized in that the method comprises: in a protective atmosphere, dissolving a polymerization monomer and an initiator in a reaction medium to obtain a mixed solution and subjecting the mixed solution to a polymerization reaction, and separating the obtained copolymer emulsion suspension to obtain the maleic anhydride-isobutylene copolymer microspheres;

[0007] Wherein, the polymerizable monomers are maleic anhydride and isobutylene; based on the total weight of the polymerizable monomers, the amount of maleic anhydride is 50-90wt%, and the amount of isobutylene is 10-50wt%;

[0008] The reaction medium is a mixture of the compound represented by formula (1) and an alkane;

[0009]

[0010] Wherein, R1 and R2 are each independently an alkyl group having 1 to 6 carbon atoms.

[0011] The second aspect of the present invention provides a maleic anhydride-isobutylene copolymer microsphere, characterized in that the maleic anhydride-isobutylene copolymer microsphere is prepared by the above method.

[0012] The third aspect of the present invention provides a method for preparing the maleic anhydride-isobutylene copolymer microspheres and / or the use of the maleic anhydride-isobutylene copolymer microspheres as a dispersant in polyethylene.

[0013] Through the above technical scheme, the maleic anhydride-isobutylene copolymer microspheres provided by the present invention and the preparation method and application thereof obtain the following beneficial effects:

[0014] The maleic anhydride-isobutylene copolymer microspheres provided by the present invention can form stable and uniform polymer microspheres after polymerization reaction by selecting a specific reaction medium and matching it with a specific amount of monomers. Moreover, due to the improvement of the solvent, the traditional ester solvent is not used, and the obtained copolymer microspheres have no special odor and a wide range of applications. In addition, compared with the traditional organic small molecule dispersant, the maleic anhydride isobutylene polymer dispersant has the excellent characteristics of no migration and no precipitation. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 3 is a scanning electron microscope image of the maleic anhydride-isobutylene copolymer microspheres of Example 1. DETAILED DESCRIPTION

[0016] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0017] The first aspect of the present invention provides a method for preparing maleic anhydride-isobutylene copolymer microspheres, characterized in that the method comprises: in a protective atmosphere, dissolving a polymerization monomer and an initiator in a reaction medium to obtain a mixed solution and subjecting the mixed solution to a polymerization reaction, and separating the obtained copolymer emulsion suspension to obtain the maleic anhydride-isobutylene copolymer microspheres;

[0018] Wherein, the polymerizable monomers are maleic anhydride and isobutylene; based on the total weight of the polymerizable monomers, the amount of maleic anhydride is 50-90wt%, and the amount of isobutylene is 10-50wt%;

[0019] The reaction medium is a mixture of the compound represented by formula (1) and an alkane;

[0020]

[0021] Wherein, R1 and R2 are each independently an alkyl group having 1 to 6 carbon atoms.

[0022] In the present invention, maleic anhydride monomer and comonomer isobutylene are copolymerized in a specific ratio by copolymerization, so that the prepared maleic anhydride-isobutylene copolymer is in a uniform microsphere shape, and the copolymer microsphere particles are uniformly dispersed, and have more stable dispersion performance than small molecule dispersants.

[0023] According to the present invention, based on the total weight of the polymerized monomers, the amount of maleic anhydride is 50-60wt%, and the amount of isobutylene is 40-50wt%.

[0024] In the present invention, when the amounts of maleic anhydride and isobutylene meet the above ranges, the obtained maleic anhydride-isobutylene copolymer microspheres have clean surfaces and uniform particle sizes, and have more stable dispersibility when used as a dispersant, without migration or precipitation.

[0025] According to the present invention, based on the total weight of the mixed solution, the total mass concentration of the polymerizable monomers is 5-25wt%, and the mass concentration of the initiator is 0.01-1wt%.

[0026] Furthermore, based on the total weight of the mixed solution, the total mass concentration of the polymerizable monomers is 5-20wt%, and the mass concentration of the initiator is 0.1-0.5wt%.

[0027] According to the present invention, the initiator is an organic peroxide and / or an azo compound.

[0028] Furthermore, the organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate.

[0029] Furthermore, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.

[0030] According to the present invention, in formula (1), R1 and R2 are each independently an alkyl group having 1 to 4 carbon atoms, preferably a methyl group.

[0031] According to the present invention, the alkane is an alkane having 6 to 12 carbon atoms.

[0032] In the present invention, a mixture of the compound represented by formula (1) and an alkane is selected as the reaction medium, which can be used in combination with the specific amount of maleic anhydride and the comonomer described in the present invention. The surface of the obtained polymer microspheres is clean and odorless. Compared with ester solvents, the prepared copolymer microspheres have a wider range of applications when used as a dispersant.

[0033] Furthermore, the alkane is selected from at least one of hexane, heptane and octane.

[0034] Furthermore, the alkane is hexane.

[0035] According to the present invention, based on the total volume of the reaction medium, the amount of the alkane is 35-70 vol%, preferably 40-55 vol%.

[0036] According to the present invention, the polymerization reaction is carried out in an inert atmosphere. The inert atmosphere is not particularly limited and can be provided by conventional inert gases in the prior art, such as nitrogen.

[0037] According to the present invention, the conditions of the polymerization reaction include: the polymerization temperature is 61-100° C., preferably 70-90° C.; the polymerization time is 1-24 h, preferably 2-12 h.

[0038] In the present invention, a water bath and / or an oil bath is used to provide the heat required for the polymerization of the present invention.

[0039] In the present invention, the separation may be a conventional solid-liquid separation method in the art, such as centrifugal separation.

[0040] In the present invention, when centrifugal separation is adopted, the centrifugal speed is 1500-5000 rad / min, and the centrifugal time is 5-60 min.

[0041] The second aspect of the present invention provides a maleic anhydride-isobutylene copolymer microsphere, characterized in that the maleic anhydride-isobutylene copolymer microsphere is prepared by the above method.

[0042] According to the present invention, the copolymer in the maleic anhydride-isobutylene copolymer microspheres comprises a structural unit A derived from maleic anhydride and a structural unit B derived from isobutylene.

[0043] According to the present invention, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 47-54 mol%, and the molar content of the structural unit B is 46-53 mol%.

[0044] In the present invention, when the maleic anhydride-isobutylene copolymer microspheres contain the structural units in the specific molar content, the maleic anhydride-isobutylene copolymer can have microspheres with good uniformity, better dispersibility and higher comprehensive performance.

[0045] Furthermore, the molar content of the structural unit A is 49-54 mol%, and the molar content of the structural unit B is 46-51 mol%.

[0046] In the present invention, the molar content of each structural unit in the copolymer is 1 H NMR was performed, specifically, by 1 The ratio of the peak area corresponding to the characteristic hydrogen in the corresponding structural unit in HNMR was calculated.

[0047] According to the present invention, the average particle size of the maleic anhydride-isobutylene copolymer microspheres is 500-1300 nm, preferably 600-1200 nm.

[0048] In the present invention, the average particle size of the copolymer microspheres is measured using a scanning electron microscope.

[0049] According to the present invention, the number average molecular weight of the copolymer in the maleic anhydride-isobutylene copolymer microspheres is 10,000-35,000, preferably 10,000-25,000.

[0050] The third aspect of the present invention provides a method for preparing the maleic anhydride-isobutylene copolymer microspheres and / or the use of the maleic anhydride-isobutylene copolymer microspheres as a dispersant in polyethylene.

[0051] In the present invention, the maleic anhydride-isobutylene copolymer microspheres prepared by the above method have uniform particle size. By using a specific solvent and ratio, the prepared copolymer microspheres are cleaner and odorless compared to ester solvents. When used as a dispersant, the application range is wider, and it does not migrate or precipitate, and has strong stability.

[0052] The present invention will be described in detail below by way of examples. In the following examples, the polymerization yield (C p ) to calculate

[0053] C p =Mp×100% / Mm

[0054] Wherein, Mp is the mass of the obtained polymer; Mm is the total mass of the added monomers;

[0055] The tensile strength of polyethylene compounds is tested according to GB / T 1040-2006;

[0056] The amount of material migrated out of the sample was measured by liquid chromatography after washing with solvent;

[0057] The morphology of copolymer microspheres was observed and measured using scanning electron microscopy (SEM);

[0058] The average particle size of copolymer microspheres was measured by scanning electron microscopy (SEM);

[0059] The content of each structural unit in the copolymer is 1 Measured by H NMR;

[0060] The molecular weight of the copolymers was measured by gel permeation chromatography (GPC);

[0061] The raw materials used in the examples and comparative examples are all commercially available.

[0062] Example 1

[0063] 100g maleic anhydride, 2g azobisisobutylene nitrile, 75g isobutylene, 350ml acetone and 650ml hexane were added to a 3L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 159g of maleic anhydride-isobutylene copolymer microspheres 1A, and the yield of the corresponding copolymer was 90.9%. The size of the maleic anhydride-isobutylene copolymer microspheres 1A was 1300nm. Among them, the amount of maleic anhydride was 57.1wt%; the amount of isobutylene was 42.9wt%; and the amount of hexane in the reaction medium was 65vol%.

[0064] Maleic anhydride-isobutylene copolymer microspheres 1A were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 49 mol%, and the molar content of the structural unit B derived from isobutylene was 51 mol%. The molecular weight of the polymer was 35,000 g / mol.

[0065] Figure 1 is the SEM image of maleic anhydride-isobutylene copolymer microsphere 1A. Figure 1 It can be seen that the maleic anhydride-isobutylene copolymer particles prepared in Example 1 are spherical polymer particles.

[0066] Example 2

[0067] 50g maleic anhydride, 2g azobisisobutylene nitrile, 39g isobutylene, 350ml acetone and 650ml hexane were added to a 3L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 67.3g of maleic anhydride-isobutylene copolymer microspheres 2A, and the corresponding copolymer yield was 75.6%. The size of maleic anhydride-isobutylene copolymer microspheres 2A was 900nm. Among them, the amount of maleic anhydride was 56.2wt%; the amount of isobutylene was 43.8wt%; and the amount of hexane in the reaction medium was 65vol%.

[0068] Maleic anhydride-isobutylene copolymer microspheres 2A were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 50 mol%, and the molar content of the structural unit B derived from isobutylene was 50 mol%. The molecular weight of the polymer was 15,000 g / mol.

[0069] Example 3

[0070] 25g of maleic anhydride, 2g of azobisisobutylene nitrile, 19g of isobutylene, 350ml of acetone and 650ml of heptane were added to a 3L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 33g of maleic anhydride-isobutylene copolymer microspheres 3A, and the corresponding copolymer yield was 75%. The size of maleic anhydride-isobutylene copolymer microspheres 3A was 500nm. Among them, the amount of maleic anhydride was 56.8wt%; the amount of isobutylene was 43.2wt%; and the amount of hexane in the reaction medium was 65vol%.

[0071] Maleic anhydride-isobutylene copolymer microspheres 3A were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 52 mol%, and the molar content of the structural unit B derived from isobutylene was 48 mol%. The molecular weight of the polymer was 10,000 g / mol.

[0072] Example 4

[0073] 50g of maleic anhydride, 2g of azobisisobutylene nitrile, 35g of isobutylene, 500ml of acetone and 500ml of hexane were added to a 3L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5 hours. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 70.2g of maleic anhydride-isobutylene copolymer microspheres 4A, corresponding to a polymer yield of 82.6%. The size of maleic anhydride-isobutylene copolymer microspheres 4A was 1000nm. Among them, the amount of maleic anhydride was 58.8wt%; the amount of isobutylene was 41.2wt%; and the amount of hexane in the reaction medium was 50vol%.

[0074] Maleic anhydride-isobutylene copolymer microspheres 4A were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 54 mol%, and the molar content of the structural unit B derived from isobutylene was 46 mol%. The molecular weight of the polymer was 20,000 g / mol.

[0075] Example 5

[0076] 50g of maleic anhydride, 2g of azobisisobutylenenitrile, 35g of isobutylene, 700ml of acetone and 300ml of heptane were added to a 3L reactor. After the materials were mixed evenly, the temperature was raised to 50°C and the reaction was carried out for 5h. After the reaction was completed, the obtained polymer emulsion suspension was centrifuged at a speed of 2000rad / min for 20 minutes to obtain 68.8g of maleic anhydride-isobutylene copolymer microspheres 5A, and the corresponding copolymer yield was 80.9%. The size of maleic anhydride-isobutylene copolymer microspheres 5A was 960nm. Among them, the amount of maleic anhydride was 58.8wt%; the amount of isobutylene was 41.2wt%; and the amount of hexane in the reaction medium was 30vol%.

[0077] Maleic anhydride-isobutylene copolymer microspheres 5A were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 53 mol%, and the molar content of the structural unit B derived from isobutylene was 47 mol%. The molecular weight of the polymer was 25,000 g / mol.

[0078] Example 6

[0079] The method of Example 1 was followed, except that acetone was replaced by pentanone. 70.5 g of maleic anhydride-isobutylene copolymer microspheres 6A were obtained, with a corresponding copolymer yield of 82.4%. The size of the maleic anhydride-isobutylene copolymer microspheres 6A was 1050 nm.

[0080] The obtained maleic anhydride-isobutylene copolymer microspheres 6A were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 48 mol%, and the molar content of the structural unit B derived from isobutylene was 52 mol%. The molecular weight of the polymer was 22,000 g / mol.

[0081] Example 7

[0082] According to the method of Example 1, except that the amount of maleic anhydride used was 70 g, the amount of isobutylene used was 30 g, and 66 g of maleic anhydride-isobutylene copolymer microspheres 7A were obtained, corresponding to a copolymer yield of 77.4%. The size of the maleic anhydride-isobutylene copolymer microspheres 7A was 900 nm.

[0083] The obtained maleic anhydride-isobutylene copolymer microspheres 7A were 1 H NMR measurement showed that the molar content of the structural unit A derived from maleic anhydride was 49 mol%, and the molar content of the structural unit B derived from isobutylene was 51 mol%, based on the total molar amount of the copolymer structural units. The molecular weight of the polymer was 20,000 g / mol.

[0084] Example 8

[0085] The method of Example 1 was followed, except that the amount of acetone was 750 mL and the amount of heptane was 250 mL. 64 g of maleic anhydride-isobutylene copolymer microspheres 8A were obtained, corresponding to a copolymer yield of 75.3%. The size of the maleic anhydride-isobutylene copolymer microspheres 8A was 880 nm. The polymer molecular weight was 18,000 g / mol.

[0086] The obtained maleic anhydride-isobutylene copolymer microspheres 8A were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 46 mol%, and the molar content of the structural unit B derived from isobutylene was 54 mol%.

[0087] Comparative Example 1

[0088] The method of Example 1 was followed, except that the reaction medium did not contain hexane and the amount of acetone was 1000 mL. After the reaction was completed, a transparent solution was obtained, but no microspherical copolymer material was obtained.

[0089] Comparative Example 2

[0090] The method of Example 1 was followed, except that the reaction medium did not contain acetone and the amount of hexane was 1000 mL. After the reaction was completed, a block substance 2D was obtained instead of a suspension, and no microspherical copolymer material was obtained. Among them, the amount of maleic anhydride was 57.1 wt%; the amount of isobutylene was 42.9 wt%; and the amount of hexane in the reaction medium was 100 vol%.

[0091] The obtained maleic anhydride-isobutylene copolymer microspheres 2D were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 51 mol %, and the molar content of the structural unit B derived from isobutylene was 49 mol %.

[0092] Comparative Example 3

[0093] The method of Example 1 is followed, except that 200 g of maleic anhydride, 2 g of azobisisobutylene, 300 g of isobutylene, 500 ml of acetone and 500 ml of heptane are added to a 3L reactor for reaction. After the reaction is completed, a solidified solid material 3D is obtained. The amount of maleic anhydride is 40 wt %; the amount of isobutylene is 60 wt %; and the amount of hexane in the reaction medium is 50 vol %.

[0094] The obtained maleic anhydride-isobutylene copolymer microspheres 3D were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 49 mol%, and the molar content of the structural unit B derived from isobutylene was 51 mol%.

[0095] Comparative Example 4

[0096] The method of Example 1 was followed, except that acetone was replaced by decanone, to obtain a solidified maleic anhydride-isobutylene copolymer 4D, wherein the amount of maleic anhydride was 58.8 wt %; the amount of isobutylene was 41.2 wt %; and the amount of hexane in the reaction medium was 30 vol %.

[0097] The obtained maleic anhydride-isobutylene copolymer microspheres 4D were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 50 mol %, and the molar content of the structural unit B derived from isobutylene was 50 mol %.

[0098] Comparative Example 5

[0099] The method of Example 1 was followed, except that the amount of maleic anhydride was 84 g and the amount of isobutylene was 91 g. 130 g of maleic anhydride-isobutylene copolymer 5D was obtained, and the polymer yield was 74.3%. The amount of maleic anhydride was 48 wt%; the amount of isobutylene was 52 wt%; and the amount of hexane in the reaction medium was 30 vol%.

[0100] The obtained maleic anhydride-isobutylene copolymer microspheres 5D were 1 H NMR measurement showed that, based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A derived from maleic anhydride was 49 mol%, and the molar content of the structural unit B derived from isobutylene was 51 mol%.

[0101] Table 1

[0102]

[0103]

[0104] Table 2

[0105] Comparative Example 1 2 3 4 5 Maleic anhydride dosage / wt% 57.1 57.1 40 58.8 47.9 Isobutylene dosage / wt% 42.9 42.9 60 41.2 52.1 Initiator / wt% 0.18 0.18 0.13 0.18 0.13 Hexane dosage / vol% / 0 100 50 30 30 Ketone Types acetone acetone acetone Decanoate acetone Molar content of A / mol% 48 51 49 50 49 Molar content of B / mol% 52 49 51 50 51 Copolymer yield / % 50 40 60 45 74.3 Particle size / nm - - - - 800 Number average molecular weight 60000 10000 20000 21000 12000

[0106] Test Case

[0107] The copolymer microspheres, ethylene bis stearic acid amide and zinc stearate of the embodiment and the comparative example are used as dispersants in a composition of talc-filled polyethylene, wherein the polyethylene addition amount is 2000g and the filling amount of talc is 5wt% of the polyethylene weight. The components are blended and granulated by a twin-screw extruder, and the blending and granulation process parameters are as follows: the temperature of each section is 180°C, 190°C, 200°C, 210°C, 220°C, 210°C, 200°C, 190°C. The polymer blend obtained after granulation is injection molded into sheets and subjected to performance tests. The test results are shown in Table 3.

[0108] Table 3

[0109]

[0110]

[0111] Note: t0 is the initial tensile strength, t1 is the tensile strength, and m is the dispersant that migrated out of the polyethylene surface after storage for half a year.

[0112] It can be seen from the above examples and comparative examples that the preparation method provided by the present invention can realize a self-stabilizing precipitation polymerization reaction to obtain a stable polymer microsphere suspension, so that the prepared microspheres have a uniform particle size and a clean surface without pollution. It can be seen from Table 3 that the copolymer microspheres prepared in the examples have stable performance. After storage for half a year, the decrease rate of tensile strength does not exceed 3.55%, and the detected amount of polymer migrated does not exceed 0.12 mg / g.

[0113] However, the methods of Comparative Examples 1-4 cannot obtain a stable suspension, and thus cannot produce polymer microspheres. The blocky solid material is not suitable for use as a dispersant. Even if it is added to a polyethylene compound, the initial tensile strength is low, not exceeding 9 MPa. Comparative Example 5 can produce copolymer microspheres, but as can be seen from Table 3, when used as a dispersant, the tensile strength decrease rate after storage for half a year is 3.89%, and the amount of polymer detected to migrate out is as high as 0.15 mg / g.

[0114] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for preparing maleic anhydride-isobutylene copolymer microspheres, characterized in that: The method comprises: in a protective atmosphere, dissolving a polymerization monomer and an initiator in a reaction medium to obtain a mixed solution and subjecting the mixed solution to a polymerization reaction, and separating the obtained copolymer emulsion suspension to obtain the maleic anhydride-isobutylene copolymer microspheres; Wherein, the polymerizable monomers are maleic anhydride and isobutylene; based on the total weight of the polymerizable monomers, the amount of maleic anhydride is 50-90wt%, and the amount of isobutylene is 10-50wt%; The reaction medium is a mixture of the compound represented by formula (1) and an alkane; Wherein, R1 and R2 are each independently an alkyl group having 1 to 4 carbon atoms; Wherein, based on the total volume of the reaction medium, the amount of the alkane used is 30-70 vol%.

2. The preparation method according to claim 1, wherein Based on the total weight of the polymerized monomers, the amount of maleic anhydride used is 50-60wt%, and the amount of isobutylene used is 40-50wt%.

3. The preparation method according to claim 1 or 2, wherein Based on the total weight of the mixed solution, the total mass concentration of the polymerizable monomers is 5-25wt%, and the mass concentration of the initiator is 0.01-1wt%.

4. The preparation method according to claim 3, wherein Based on the total weight of the mixed solution, the total mass concentration of the polymerizable monomers is 5-20wt%, and the mass concentration of the initiator is 0.1-0.5wt%.

5. The preparation method according to any one of claims 1 to 2 and 4, wherein: The initiator is selected from organic peroxides and / or azo compounds.

6. The preparation method according to claim 5, wherein: The organic peroxide is at least one selected from dibenzoyl peroxide, diisopropyl peroxide, di-tert-butyl peroxide, dodecyl peroxide, tert-butyl perbenzoate, diisopropyl peroxydicarbonate and dicyclohexyl peroxydicarbonate; And / or, the azo compound is selected from azobisisobutyronitrile and / or azobisisoheptanenitrile.

7. The preparation method according to any one of claims 1 to 2, 4 and 6, wherein: In formula (1), R1 and R2 are methyl groups.

8. The preparation method according to any one of claims 1-2, 4 and 6, wherein: The alkane is an alkane having 6 to 12 carbon atoms.

9. The preparation method according to claim 8, wherein: The alkane is at least one selected from hexane, heptane and octane.

10. The preparation method according to claim 9, wherein: The alkane is hexane.

11. The preparation method according to any one of claims 1-2, 4, 6, 9-10, wherein: Based on the total volume of the reaction medium, the amount of the alkane used is 40-55 vol%.

12. The preparation method according to any one of claims 1-2, 4, 6, 9-10, wherein: The polymerization reaction conditions include: polymerization temperature of 61-100° C., and polymerization time of 1-24 h.

13. The preparation method according to claim 12, wherein: The polymerization reaction conditions include: polymerization temperature of 70-90° C., and polymerization time of 2-12 h.

14. A maleic anhydride-isobutylene copolymer microsphere, characterized in that: The maleic anhydride-isobutylene copolymer microspheres are prepared by the method described in any one of claims 1-13.

15. The maleic anhydride-isobutylene copolymer microspheres according to claim 14, wherein: The copolymer in the maleic anhydride-isobutylene copolymer microspheres comprises a structural unit A derived from maleic anhydride and a structural unit B derived from isobutylene; Based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 47-54 mol%, and the molar content of the structural unit B is 46-53 mol%.

16. The maleic anhydride-isobutylene copolymer microspheres according to claim 15, wherein: Based on the total molar amount of each structural unit in the copolymer, the molar content of the structural unit A is 49-54 mol%, and the molar content of the structural unit B is 46-51 mol%.

17. The maleic anhydride-isobutylene copolymer microspheres according to claim 14 or 15, wherein: The average particle size of the maleic anhydride-isobutylene copolymer microspheres is 500-1300 nm; The number average molecular weight of the copolymer in the maleic anhydride-isobutylene copolymer microspheres is 10,000-35,000.

18. The maleic anhydride-isobutylene copolymer microspheres according to claim 17, wherein: The average particle size of the maleic anhydride-isobutylene copolymer microspheres is 600-1200 nm; The number average molecular weight of the copolymer in the maleic anhydride-isobutylene copolymer microspheres is 10,000-25,000.

19. A method for preparing the maleic anhydride-isobutylene copolymer microspheres according to any one of claims 1 to 13, or use of the maleic anhydride-isobutylene copolymer microspheres according to any one of claims 14 to 18 as a dispersant in polyethylene.