A nitrogen-doped hydrothermal carbon-magnesium silicate composite material and its preparation method and application

The one-step hydrothermal method of nitrogen-doped hydrothermal carbon-magnesium silicate composite material solves the problems of high cost of existing carbon-based adsorbents and single functional group of magnesium silicate adsorbent, and achieves efficient removal of tetracycline and arsenic in water. species, providing low-cost, high-performance adsorbents.

CN116272842BInactive Publication Date: 2024-10-08ZHENGZHOU MINERALS COMPOSITIVE UTILIZATION RES INST CHINESE GEOLOGICAL ACAD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211092083.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-08
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing carbon-based adsorbents have high cost, complex processes and secondary pollution problems when removing tetracycline and arsenic species in water. Moreover, the surface functional groups of the magnesium silicate adsorbent have a single type and the removal effect is not ideal.

Method used

Nitrogen-doped hydrothermal carbon-magnesium silicate composite materials are used to synthesize adsorbents with three-dimensional structures and multi-category functional groups through a one-step hydrothermal method. Diatomaceous earth and glucose are used as silicon sources and carbon sources, and ammonia water is used as nitrogen sources to provide C and N element functional groups improve adsorption performance.

Benefits of technology

It achieves high specific surface area and high adsorption capacity, significantly improves the removal effect of tetracycline and arsenic species, has low cost and simple process, and provides a low-cost, high-performance adsorbent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116272842B_ABST
    Figure CN116272842B_ABST
Patent Text Reader

Abstract

The present invention proposes a nitrogen-doped hydrothermal carbon-magnesium silicate composite material and its preparation method and application, the composite material includes a disc-shaped frame, the disc-shaped frame is a three-dimensional structure of self-assembly of magnesium silicate nanosheets, the upper and lower surfaces of the disc-shaped frame are attached with nano flower balls, the disc-shaped frame is a nano column array, the nano flower balls and nano columns are self-assembled by magnesium silicate nanosheets, and the hydrothermal carbon containing C and N functional groups is in situ grown on the surface of magnesium silicate nanosheets. The present invention adopts a one-step hydrothermal method to synthesize the composite material, the synthesis method is simple, the cost is low, and diatomaceous earth is used to obtain a nitrogen-doped hydrothermal carbon-magnesium silicate composite material of a three-dimensional structure, which not only solves the problem of a single type of nano magnesium silicate adsorption site, but also solves the problem of low specific surface area of ​​hydrothermal carbon materials; the Mg-containing adsorption sites and C and N element functional groups on the surface of the composite material can be well removed by adsorption, complexation and other methods. As (V) and tetracycline in the water body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adsorption materials, and in particular to a nitrogen-doped hydrothermal carbon-magnesium silicate composite material and a preparation method and application thereof. Background Art

[0002] Tetracycline (TC) and arsenic species are two of the main pollutants in wastewater generated by aquaculture and livestock breeding. Tetracycline is a highly effective antibiotic that is widely used to prevent and treat diseases of fish and livestock. Long-term use of tetracycline by animals or humans will cause tetracycline to accumulate in the body. However, tetracycline is difficult to metabolize in organisms, and long-term exposure to tetracycline will lead to increased bacterial resistance, posing a huge threat to human health and the ecological environment. Similarly, arsenic compounds are often used as animal growth promoters and pesticides. Arsenic is a heavy metal anion, and the enrichment of arsenic can cause great harm to the human body and the ecosystem.

[0003] The adsorption method is widely used in actual environmental remediation projects due to its advantages such as low cost and high efficiency. The surface of carbon-based adsorbents is rich in C-containing functional groups, but carbon-based adsorbents are difficult to separate from water bodies due to their small particle size, which will cause secondary pollution. Secondly, carbon-based adsorbents such as biochar often require additional activation treatment to obtain a larger specific surface area. Carbon-based adsorbents with better performance usually require two or more steps to synthesize, and the synthesis process is relatively complicated, resulting in higher synthesis costs. After doping with specific elements such as N and S, the active adsorption sites on the surface of the carbon-based adsorbent increase, and the adsorption performance will be improved to a certain extent. However, the nitrogen doping process is relatively complicated, and generally requires the carbon material to be calcined at high temperature in a nitrogen-containing atmosphere (such as ammonia and nitrogen). As a result, the synthesis cost of high-performance carbon-based adsorbents is relatively high. Therefore, it is still a difficult problem to synthesize carbon-based adsorbents with high specific surface area and high adsorption performance by a simple process.

[0004] The magnesium silicate adsorbent synthesized with cheap diatomite as silicon source has a three-dimensional porous structure and sufficient surface and interface, which makes it have a large specific surface area, low synthesis cost and simple synthesis process. However, the surface functional groups of magnesium silicate are single, and the removal effect of certain specific pollutants in water, such as As(V) and tetracycline, is not ideal. Summary of the invention

[0005] The present invention provides a nitrogen-doped hydrothermal carbon-magnesium silicate composite material, a preparation method and an application thereof. The present invention utilizes the three-dimensional structure of diatomite to obtain a nitrogen-doped hydrothermal carbon-magnesium silicate composite material with a three-dimensional structure, which not only solves the problem of a single type of adsorption sites of nano-magnesium silicate, but also solves the problem of a low specific surface area of ​​the hydrothermal carbon material; the Mg-containing adsorption sites and C and N-containing functional groups on the surface of the composite material can well remove As(V) and tetracycline in water by adsorption, complexation and the like.

[0006] The technical solution of the present invention is achieved as follows: a nitrogen-doped hydrothermal carbon-magnesium silicate composite material, the composite material includes a disc-shaped frame, the disc-shaped frame is a three-dimensional structure of self-assembled magnesium silicate nanosheets, nano flower balls are attached to the upper and lower surfaces of the disc-shaped frame, and the disc-shaped frame is a nano column array, the nano flower balls and the nano columns are both self-assembled from magnesium silicate nanosheets, and hydrothermal carbon containing C and N functional groups is in-situ grown on the surface of the magnesium silicate nanosheets.

[0007] Furthermore, the C element functional group includes one or more of an unsaturated carbon-carbon double bond, a carboxylic acid group and an ester group.

[0008] Further, the N element functional group includes one or more of pyridinic nitrogen, pyrrolic nitrogen and graphitic nitrogen.

[0009] A nitrogen-doped hydrothermal carbon-magnesium silicate composite material is prepared from the following raw materials: diatomaceous earth, glucose, ammonia water, ethanol and MgCl2·6H2O, wherein the mass ratio of diatomaceous earth to glucose is 1:0.1-2; the volume mass ratio of ammonia water to diatomaceous earth is 20-50:1 mL / g, the volume mass ratio of ethanol to diatomaceous earth is 1-10:1 mL / g, and the mass ratio of MgCl2·6H2O to diatomaceous earth is 2.5-7:1.

[0010] When the amount of ammonia added is small, it is not enough to convert all the diatomaceous earth into silicate, resulting in the presence of some magnesium hydroxide in the synthetic product; when the amount of ammonia added is high, the diatomaceous earth will dissolve quickly and cannot play the role of a self-sacrificial template, and the synthesized composite material does not have a three-dimensional structure.

[0011] Furthermore, the mass ratio of diatomite to glucose is 1:0.4-0.6; the volume mass ratio of ammonia water to diatomite is 35-45:1 mL / g, the volume mass ratio of ethanol to diatomite is 4-6:1 mL / g, and the mass ratio of MgCl2·6H2O to diatomite is 5:1. In the hydrothermal system, the formation of the magnesium silicate phase is directly related to the mass ratio of diatomite to magnesium chloride. When the mass ratio of MgCl2·6H2O to diatomite is 5:1, the synthesized magnesium silicate is a chlorite phase, and the magnesium silicate at this time is a three-dimensional structure of self-assembled sheet structures.

[0012] Furthermore, the mass concentration of the ammonia water is 22-28%.

[0013] A method for preparing a nitrogen-doped hydrothermal carbon-magnesium silicate composite material comprises the following steps:

[0014] 1) adding diatomaceous earth and glucose into deionized water, and stirring to allow the glucose to fully impregnate the diatomaceous earth to form a diatomaceous earth suspension;

[0015] 2) adding ammonia water and ethanol to the diatomaceous earth suspension in step 1), stirring evenly to obtain a suspension;

[0016] 3) dissolving magnesium chloride in deionized water to obtain a magnesium chloride solution, and slowly adding the magnesium chloride solution dropwise to the suspension in step 2) to obtain a mixed solution;

[0017] 4) The mixed solution of step 3) is aged for 8 to 10 hours under hydrothermal conditions at 180 to 200° C., cooled, washed, filtered, and dried to obtain a nitrogen-doped hydrothermal carbon-magnesium silicate composite material.

[0018] The preparation method of the present invention provides a nitrogen source for nitrogen-doped hydrothermal carbon by adding ammonia water, and compared with other nitrogen doping methods, the synthesis process is simple. At the same time, ammonia water dissociates hydroxide to react with diatomaceous earth to provide silicate for synthesizing magnesium silicate, and the synthesis of magnesium silicate phase provides a matrix for the nucleation, attachment and growth of hydrothermal carbon. Nitrogen-doped hydrothermal carbon grows in situ on the surface of magnesium silicate, and the combination between the two is more firm. In the nitrogen-doped hydrothermal carbon-magnesium silicate composite material, the magnesium silicate phase provides a framework structure for the composite material, so that the composite material has a large specific surface area, thereby exposing more functional groups containing C and N elements, which is beneficial to the adsorption and removal of water pollutants. Through a one-step hydrothermal method, three-dimensional structure construction, nitrogen doping, high specific surface area and composite of multiple categories of functional groups are achieved, which is of great significance for the low-cost synthesis of high-performance adsorbents.

[0019] In step 3), the magnesium chloride solution is added at a rate of 40 drops / min. During the addition, the suspension is magnetically stirred at a rate of 70 to 80 r / min.

[0020] The nitrogen-doped hydrothermal carbon-magnesium silicate composite material can be used to adsorb As(V) or tetracycline.

[0021] Beneficial effects of the present invention:

[0022] The present invention uses cheap and readily available diatomaceous earth and glucose as silicon and carbon sources, and ammonia water as a nitrogen source, and completes the nitrogen-doped hydrothermal carbon-magnesium silicate composite material through a one-step hydrothermal method, thereby realizing the composite of hydrothermal carbon containing C and N functional groups and magnesium silicate with a large specific surface area and a three-dimensional structure, which belongs to a composite mesoporous adsorbent with multiple functional groups, a large specific surface area and a three-dimensional structure. The specific surface area of ​​the nitrogen-doped hydrothermal carbon-magnesium silicate composite material of the present invention can reach up to 201m 2 / g, the maximum adsorption capacity for As(V) is 498mg / g, and the maximum adsorption capacity for tetracycline is 1652mg / g.

[0023] The diatomite of the present invention is used as a self-sacrificial template to provide silicate for synthesizing magnesium silicate with a three-dimensional structure. At the same time, the magnesium silicate with a three-dimensional structure can provide a matrix for the nucleation and growth of hydrothermal carbon materials due to its fast synthesis speed. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 The X-ray diffraction curve of the nitrogen-doped hydrothermal carbon-magnesium silicate composite material prepared in Example 1;

[0026] Figure 2 The 13C solid-state nuclear magnetic spectrum of the nitrogen-doped hydrothermal carbon-magnesium silicate composite material prepared in Example 1;

[0027] Figure 3 The N1s orbital XPS spectrum of the nitrogen-doped hydrothermal carbon-magnesium silicate composite material prepared in Example 1;

[0028] Figure 4 This is a scanning electron microscope photograph of the nitrogen-doped hydrothermal carbon-magnesium silicate composite material prepared in Example 1;

[0029] Figure 5 The nitrogen adsorption-desorption curve and pore size distribution curve of the nitrogen-doped hydrothermal carbon-magnesium silicate composite material prepared in Example 1;

[0030] Figure 6 The nitrogen adsorption-desorption curve and pore size distribution curve of the nitrogen-doped hydrothermal carbon-magnesium silicate composite material prepared in Example 2;

[0031] Figure 7 This is a scanning electron microscope photograph of the nitrogen-doped hydrothermal carbon-magnesium silicate composite material prepared in Example 3. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] This embodiment relates to a method for preparing a nitrogen-doped hydrothermal carbon-magnesium silicate composite material, comprising the following steps:

[0035] 1) Add 1 g of diatomaceous earth and 0.5 g of glucose into 10 mL of deionized water and stir to form a suspension;

[0036] 2) Add 40 mL of ammonia water and 5 mL of ethanol to the above suspension and stir evenly;

[0037] 3) Dissolve 5 g of MgCl2·6H2O in 20 mL of deionized water, and slowly add it dropwise to the above stirred suspension to obtain a mixed suspension;

[0038] 4) The mixed solution is aged for 8 to 10 hours in a hydrothermal condition at 180 to 200° C., cooled, washed, filtered, and dried to obtain a nitrogen-doped hydrothermal carbon-magnesium silicate composite material.

[0039] Depend on Figure 1 The X-ray diffraction pattern in shows that the synthesized product is chlorite phase magnesium silicate. The diffraction peaks at 2θ of 6.4°, 12.3°, 18.5°, 19.4°, 34.2°, 35.9° and 60.0° correspond to the (002), (004), (006), (1-11), (132), (1-34) and (060) crystal planes of chlorite phase (Mg-chlorite, JCPDS#73-2376), respectively.

[0040] Figure 2 Nitrogen doped hydrothermal carbon-magnesium silicate composites synthesized 13 C solid NMR spectrum. As can be seen from the figure, there is a broad peak at the chemical shift of 14-60ppm, and the peak intensity is relatively large, which indicates that there are a large number of aliphatic and ether carbons in the composite material. There is also a peak at the chemical shift of 100-160ppm, and its peak intensity and peak width are similar to those at 14-60ppm. The peak here is attributed to sp 2 -Hybridized carbon, indicating that there are more unsaturated carbon-carbon double bonds (C=C) in the hydrothermal carbon material. There is a slightly weaker peak at a chemical shift of about 175 ppm, which is attributed to carboxylic acid (COOH) or ester group (COOR), that is, the surface of the composite material has abundant C and O functional groups, which is conducive to the adsorption and removal of pollutants in water.

[0041] Figure 3 This is the N1s orbital XPS spectrum of the nitrogen-doped hydrothermal carbon-magnesium silicate composite material. It can be seen from the figure that the N1s XPS spectrum can be divided into three peaks, namely pyridinic nitrogen, pyrrolic nitrogen and graphitic nitrogen, and their binding energy positions are 399eV, 400.3eV and 401.4eV respectively. This shows that the N element exists in the lattice of the hydrothermal carbon component in the composite material in the form of doping.

[0042] Figure 4This is a scanning electron microscope photo of a nitrogen-doped hydrothermal carbon-magnesium silicate composite material. As can be seen from the figure, the composite material is a three-dimensional disk-shaped structure as a whole, with flower ball-shaped structures on the upper and lower surfaces of the disk, and nano-pillar arrays inside the three-dimensional structure. Both the nano-flower balls and nano-pillars are self-assembled from nano-sheet structures.

[0043] Figure 5 The nitrogen adsorption-desorption curve and pore size distribution curve of nitrogen-doped hydrothermal carbon-magnesium silicate composite material. As shown in Figure (A), the nitrogen adsorption-desorption curves are all type IV, indicating that the composite material has a mesoporous structure. The specific surface area calculated by the BET method is 201m 2 / g. There is an H3 type hysteresis loop at a relative pressure of about 0.4-1.0, which is attributed to the slit holes and wedge-shaped holes formed by the non-rigid aggregation of the thin-sheet structure, which is consistent with the SEM observation. The pore size distribution curve shows that the pore size of the composite material is concentrated in 0-20nm.

[0044] Example 2

[0045] Compared with Example 1, the difference is that the amount of glucose added in step 2) is 1 g, and the other conditions are the same as those in Example 1.

[0046] Figure 6 The nitrogen adsorption-desorption curve of the synthesized sample is shown in Figure 1. It can be seen from the figure that the nitrogen adsorption-desorption curve of the synthesized sample is type IV, indicating that the composite material has a mesoporous structure. The specific surface area calculated by the BET method is 33.7 m 2 / g. The pore size distribution curve shows that the pore size of the composite material is concentrated in 0-20nm.

[0047] Example 3

[0048] Compared with Example 2, the difference is that the amount of ethanol added in step 1) is 1 mL, and the other conditions are the same as those in Example 2.

[0049] Figure 7 This is a scanning electron microscope photo of the sample prepared in Example 3. It can be seen from the figure that a large number of nano-microsphere particles are distributed on the surface of the sample, and the particle diameter is between 150-300nm. The granular morphology is distributed on the surface of the sample, and the surface of the sample is composed of a large number of fine nano-sheets with extremely small sizes. These nano-sheets are disordered and randomly distributed, and there is no fixed distribution trend or self-assembly tendency.

[0050] Example 4

[0051] Compared with Example 3, the difference is that the amount of ammonia water added in step 1) is 20 mL, and the other conditions are the same as those in Example 3.

[0052] Comparative Example 1

[0053] Compared with Example 1, the difference is that glucose is not added in step 1), ethanol is not added in step 2), and other conditions are the same as those in Example 1. The specific surface area of ​​the sample prepared in Comparative Example 1 is 337 m 2 / g.

[0054] Glucose is used as a C source in the synthesis of nitrogen-doped hydrothermal carbon-magnesium silicate composites, and ammonia water is used as a nitrogen source to provide functional groups containing C and N elements for the composites. When the amount of glucose added is low, the specific surface area of ​​the composite is large, but the content of functional groups containing C and N elements is low; when the amount of glucose added is high, the specific surface area of ​​the composite decreases.

[0055] The nitrogen-doped hydrothermal carbon-magnesium silicate composite material prepared in Examples 1 to 4 and Comparative Example 1 was used to adsorb the solution containing As(V) and tetracycline:

[0056] The specific operation is as follows: 70 mL of a 600 mg / L pentavalent arsenic solution and an 800 mg / L tetracycline solution are placed in different beakers, and then 0.02 g of a nitrogen-doped hydrothermal carbon-magnesium silicate sample is added. After mixing, the mixture is magnetically stirred for 3 hours and filtered to complete the adsorption of As(V) and tetracycline in the solution.

[0057] The results are shown in the following table:

[0058]

[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A nitrogen-doped hydrothermal carbon-magnesium silicate composite material, characterized in that: The composite material comprises a disc-shaped frame, which is a three-dimensional structure of self-assembled magnesium silicate nanosheets. Nano flower balls are attached to the upper and lower surfaces of the disc-shaped frame. A nano column array is arranged inside the disc-shaped frame. The nano flower balls and the nano columns are both self-assembled from magnesium silicate nanosheets. Hydrothermal carbon containing C and N functional groups is in-situ grown on the surface of the magnesium silicate nanosheets.

2. The nitrogen-doped hydrothermal carbon-magnesium silicate composite material according to claim 1, characterized in that: The C element functional group includes one or more of an unsaturated carbon-carbon double bond, a carboxylic acid group, and an ester group.

3. A nitrogen-doped hydrothermal carbon-magnesium silicate composite material according to claim 1 or 2, characterized in that: The N element functional group includes one or more of pyridinic nitrogen, pyrrolic nitrogen and graphitic nitrogen.

4. A method for preparing the nitrogen-doped hydrothermal carbon-magnesium silicate composite material according to any one of claims 1 to 3, characterized in that: The following steps are involved: 1) Add diatomaceous earth and glucose into deionized water, and stir to allow the glucose to fully impregnate the diatomaceous earth to form a diatomaceous earth suspension; 2) adding ammonia water and ethanol to the diatomaceous earth suspension in step 1), stirring evenly to obtain a suspension; 3) dissolving magnesium chloride in deionized water to obtain a magnesium chloride solution, and slowly dropping the magnesium chloride solution into the suspension of step 2) to obtain a mixed solution; 4) aging the mixed solution of step 3) under hydrothermal conditions at 180-200° C. for 8-10 hours, cooling, washing, filtering, and drying to obtain a nitrogen-doped hydrothermal carbon-magnesium silicate composite material; The mass ratio of diatomaceous earth to glucose is 1:0.1~2; the volume mass ratio of ammonia water to diatomaceous earth is 20~50:1 mL / g, the volume mass ratio of ethanol to diatomaceous earth is 1~10:1 mL / g, the mass ratio of MgCl2·6H2O to diatomaceous earth is 2.5~7:1; the mass concentration of ammonia water is 22~28%.

5. The method for preparing a nitrogen-doped hydrothermal carbon-magnesium silicate composite material according to claim 4, characterized in that: The method is prepared from the following raw materials: the mass ratio of diatomaceous earth to glucose is 1:0.4-0.6; the volume mass ratio of ammonia water to diatomaceous earth is 35-45:1 mL / g; the volume mass ratio of ethanol to diatomaceous earth is 4-6:1 mL / g; and the mass ratio of MgCl2·6H2O to diatomaceous earth is 5:

1.

6. The method for preparing a nitrogen-doped hydrothermal carbon-magnesium silicate composite material according to claim 4, characterized in that: In step 3), the magnesium chloride solution is added at a rate of 40 drops / min. During the addition, the suspension is magnetically stirred at a rate of 70-80 r / min.

7. The nitrogen-doped hydrothermal carbon-magnesium silicate composite material according to any one of claims 1 to 3 is used for adsorbing As(V) or tetracycline.