A stable cerium-containing catalyst and its preparation method and application

The cerium-containing catalyst prepared by soluble salts of magnesium, aluminum and cerium and alkaline solution solves the problems of insufficient catalyst stability and selectivity in the existing technology, realizes the efficient synthesis of cyclic carbonate, and meets the requirements of industrial production. need.

CN116272948BActive Publication Date: 2024-10-25INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111559990.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-20
Publication Date
2024-10-25
Estimated Expiration
2041-12-20

AI Technical Summary

Technical Problem

The catalysts in existing cyclic carbonate synthesis methods have problems such as solvent dissolution, low stability, high safety hazards, and harsh operating conditions. In particular, heterogeneous catalysts have insufficient activity and selectivity under high temperatures and pressures, making it difficult to meet the needs of industrial production.

Method used

The soluble salts of magnesium, aluminum and cerium are mixed with an alkaline solution, and then crystallized, dried and roasted to prepare a stable cerium-containing catalyst, which can be used to catalyze the reaction of carbonates and diols under mild conditions to form high selectivity and High yields of cyclic carbonates.

Benefits of technology

The prepared cerium-containing catalyst has high stability, reusability, simple process, avoids high temperature and high pressure conditions, diol conversion rate is as high as over 92%, cyclic carbonate selectivity and yield are over 91%, and production cost is low. Suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003420403980000011
    Figure BDA0003420403980000011
  • Figure BDA0003420403980000121
    Figure BDA0003420403980000121
  • Figure BDA0003420403980000131
    Figure BDA0003420403980000131
Patent Text Reader

Abstract

The present invention provides a stable cerium-containing catalyst and a preparation method and application thereof. The preparation method comprises the following steps: (1) stirring and mixing soluble salts of magnesium, aluminum and cerium, an alkaline solution and a solvent to obtain a mixed solution; (2) stirring the mixed solution in step (1), and then sequentially performing a crystallization treatment, a drying treatment and a roasting treatment to obtain the cerium-containing catalyst. The catalyst has low production cost, strong alkalinity, high stability, can be repeatedly used and can be scaled up for production. Compared with homogeneous catalysts, it has the advantages of easy separation of the catalyst and the product and high product selectivity; after mixing and stirring carbonate, diol and the cerium-containing catalyst, heating treatment is performed to obtain a cyclic carbonate. The synthesis method is simple, the experimental conditions are mild, no solvent, high temperature and high pressure and other harsh conditions are required, and the reaction time is shorter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of heterogeneous catalysis, and specifically relates to a stable cerium-containing catalyst and a preparation method and application thereof. Background Art

[0002] Cyclic carbonates are a very important class of chemicals and organic intermediates, with high boiling point, low odor, low toxicity and biodegradability. Among cyclic carbonates, the most representative ones are glycerol carbonate, ethylene carbonate, propylene carbonate and 1,2-butylene carbonate. Ethylene carbonate is often used as a reaction medium, extractant, plasticizer, polar solvent of foaming agent and stabilizer of lubricating oil in the production of polymer compounds and various chemical processes; propylene carbonate can be used as a solvent and plasticizer for dielectric polymers of batteries and capacitors, a resin curing accelerator, a pigment dispersant and aprotic solvent, an intermediate for the production of polycarbonate and fine chemicals, etc.; 1,2-butylene carbonate has important commercial value and is mainly used in the production of plasticizers, surfactants and reactive intermediate materials of polymers. It can also be used as a degreasing solvent, paint stripper, wood adhesive resin, foundry sand adhesive, etc. It can also be used as a battery electrolyte in lithium batteries.

[0003]

[0004] The synthesis of cyclic carbonates by transesterification of diols and carbonates is a green and high-value synthetic conversion route. The diol raw materials used to synthesize cyclic carbonates mainly include ethylene glycol (EG), propylene glycol (PG), 1,2-butanediol (BG), etc. Diols have many important application values, such as making explosives, plastics, paints, etc., but their main application areas are in the polyester industry. With the rapid development of my country's polyester industry in recent years, the demand for diols has increased year by year. At present, the coal-to-ethylene glycol production process produces about 10% of by-products of fusel alcohols, accompanied by substances rich in methanol, ethanol, ethylene glycol, 1,2-butanediol, etc. If they are fully utilized as raw materials for the production of cyclic carbonates, it will be a very green way.

[0005] At present, the synthesis methods of cyclic carbonates mainly include phosgene method, carbon dioxide and epoxide cycloaddition method, direct coupling of carbon dioxide and diol, urea alcoholysis method, ester exchange method, etc. Among them, the phosgene method requires the use of toxic reagent phosgene, which not only causes environmental pollution but also generates byproduct hydrochloric acid, and is now banned; although the cycloaddition method meets the requirements of green chemistry, it needs to react under harsh conditions of high temperature and high pressure, which has safety hazards and is easy to cause danger, and the source of raw materials is easy to cause environmental pollution, which is not conducive to industrial production; although the coupling method has a high yield, it requires a high reaction pressure, the reaction is prone to explosion, the operating conditions are harsh, and the safety factor is low; in the urea alcoholysis method, the catalyst is easily dissolved in the organic solvent, resulting in reduced product purity and subsequent separation difficulties. The ester exchange method uses a heterogeneous catalyst to synthesize cyclic carbonates using diols and carbonates. The reaction conditions are simple and mild, the raw materials are easy to obtain, the products are easy to separate, and the equipment requirements are low. Therefore, it is currently the most commonly used synthesis method. At present, the catalysts commonly used in the ester exchange method mainly include acid-base homogeneous catalysts (mainly acid-base metal salts, ionic liquids, etc., including hydrochloric acid, phosphoric acid, concentrated sulfuric acid, and alkaline catalysts mainly include hydroxides, sodium methoxide, sodium ethoxide, etc.), heterogeneous acid-base catalysts (molecular sieves and solid catalysts prepared by loading, doping, and modification of alkali metal and alkaline earth metal oxides, hydrotalcite, etc.) and other catalysts such as lipase.

[0006] CN101108843B discloses a synthetic method of a water-containing system cyclic carbonate, wherein the synthetic method is with epoxy compound and carbon dioxide as raw materials, uses bidentate ionic liquid as catalyst and alkali metal salt as promotor in the reaction process, is 0.1-10.0MPa at reaction pressure, and temperature is 313.15-483.15K, and the time is to synthesize cyclic carbonate under the condition of 0-6h. The synthetic method is low in cost, environmentally friendly, and reaction conditions are mild, and the catalyst is thermally stable and highly selective, can be reused and keep the advantages such as high activity, and has very strong industrial application prospects. However, the bidentate ionic liquid catalyst used, the imidazole ring catalytic efficiency with methyl is lower, and it is also necessary to add a promotor simultaneously, and the catalytic system is more complicated.

[0007] CN105153104A discloses a method for synthesizing propylene carbonate, wherein CO2 and propylene oxide are used as raw materials, ionic liquid is loaded on bentonite as a catalyst, and propylene carbonate is synthesized in a high-pressure reactor. The catalyst provided by the method has high activity and strong selectivity, but still needs a carrier for loading, which is limited to a certain extent in practical applications and may even reduce the stability of the catalyst.

[0008] Therefore, how to find a highly active and highly selective heterogeneous transesterification catalyst that does not require solvents and carriers is of great value and significance for the production of high-quality cyclic carbonates. Summary of the invention

[0009] In order to solve the above technical problems, the present invention provides a stable cerium-containing catalyst and a preparation method and application thereof. The catalyst has the advantages of high stability, high activity and strong reusability; the catalyst can use carbonate and diol raw materials under mild conditions to prepare cyclic carbonates with high selectivity, high yield and easy product separation.

[0010] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a method for preparing a stable cerium-containing catalyst, the preparation method comprising the following steps:

[0012] (1) stirring and mixing soluble salts of magnesium, aluminum and cerium, an alkaline solution and a solvent to obtain a mixed solution;

[0013] (2) After stirring the mixed solution in step (1), crystallization treatment, drying treatment and calcination treatment are sequentially performed to obtain the cerium-containing catalyst.

[0014] In the present invention, the preparation method is simple and easy to operate, has low production cost, and can be scaled up for production. The prepared cerium-containing catalyst has the advantages of strong alkalinity, high stability, high activity, and the like.

[0015] As a preferred technical solution of the present invention, the molar ratio of the soluble salt of magnesium to the soluble salts of aluminum and cerium in step (1) is (2-4):1, for example, it can be 2:1, 2.2:1, 2.4:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1 or 4:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] In the present invention, the molar ratio of the soluble salts of aluminum and cerium is (1-9):1, for example, it can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1 or 9:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, the soluble salt of magnesium in step (1) comprises any one or a combination of at least two of magnesium nitrate, magnesium chloride, magnesium carbonate or magnesium sulfate. Typical but non-limiting examples of the combination include: a combination of magnesium nitrate and magnesium chloride, a combination of magnesium chloride and magnesium carbonate, or a combination of magnesium carbonate and magnesium sulfate.

[0018] Preferably, the soluble salt of aluminum in step (1) comprises any one of aluminum nitrate, aluminum chloride, aluminum carbonate or aluminum sulfate, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of aluminum nitrate and aluminum chloride, a combination of aluminum chloride and aluminum carbonate, or a combination of aluminum carbonate and aluminum sulfate, etc.

[0019] Preferably, the soluble salt of cerium in step (1) comprises any one of cerium nitrate, cerium chloride, cerium sulfate or cerium acetate, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of cerium nitrate and cerium chloride, a combination of cerium chloride and cerium sulfate, or a combination of cerium sulfate and cerium acetate, etc.

[0020] As a preferred technical solution of the present invention, the alkali in the alkaline solution in step (1) includes any one of NaOH, KOH, NaHCO3, Na2CO3 or ammonia water, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of NaOH and KOH, a combination of KOH and NaHCO3, or a combination of NaHCO3 and ammonia water, etc.

[0021] Preferably, the hydroxide ion concentration of the alkaline solution in step (1) is 2-10 mol / L, for example, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L or 10 mol / L, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0022] Preferably, the solvent in step (1) comprises deionized water.

[0023] Preferably, the pH value of the mixed solution in step (1) is 9-11, for example, it can be 9, 9.2, 9.4, 9.6, 9.8, 10, 10.2, 10.4, 10.6, 10.8 or 11, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0024] Preferably, the method of stirring and mixing the soluble salts of magnesium, aluminum and cerium, the alkaline solution and the solvent in step (1) comprises: mixing the soluble salts of magnesium, aluminum and cerium and the solvent, dispersing them under ultrasonic stirring for 0.5-2h, and then adding the alkaline solution to the soluble salts and the solvent at a rate of 20-150 drops / min.

[0025] As a preferred technical solution of the present invention, the stirring time in step (2) is 0.5-2h, for example, it can be 0.5h, 1h, 1.5h or 2h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] Preferably, the temperature of the crystallization treatment in step (2) is 60-180°C, for example, it can be 60°C, 80°C, 100°C, 120°C, 140°C, 160°C or 180°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the crystallization treatment time in step (2) is 8-24 hours, for example, it can be 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] As a preferred technical solution of the present invention, after the crystallization treatment in step (2), the obtained mixed solution is subjected to solid-liquid separation treatment, and the obtained solid is washed to neutrality.

[0029] As a preferred technical solution of the present invention, the temperature of the drying treatment in step (2) is 70-120°C, for example, it can be 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the drying time in step (2) is 12-24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] Preferably, the temperature of the calcination treatment in step (2) is 400-800°C, for example, it can be 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the calcination time in step (2) is 2-8 h, for example, 2 h, 3 h, 4 h, 5 h, 6 h, 7 h or 8 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] In a second aspect, the present invention provides a stable cerium-containing catalyst, which is prepared by the preparation method described in the first aspect.

[0034] In a third aspect, the present invention provides a use of the cerium-containing catalyst as described in the second aspect, wherein the cerium-containing catalyst is used to synthesize cyclic carbonates.

[0035] As a preferred technical solution of the present invention, the application includes the following steps: mixing and stirring carbonate, diol and cerium-containing catalyst and then heating to obtain cyclic carbonate.

[0036] In the present invention, the synthesis conditions of the cyclic carbonate are mild and the process is simple, and harsh conditions such as organic solvents, high temperature and high pressure are not required.

[0037] As a preferred technical solution of the present invention, the molar ratio of carbonate to diol is (2-10):1, for example, it can be 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the mass ratio of the cerium-containing catalyst to the diol is (0.001-0.2):1, for example, it can be 0.001:1, 0.005:1, 0.01:1, 0.02:1, 0.04:1, 0.06:1, 0.08:1, 0.1:1, 0.12:1, 0.14:1, 0.16:1, 0.18:1 or 0.2:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the temperature of the heating treatment is 80-200°C, for example, it can be 80°C, 100°C, 120°C, 140°C, 160°C, 180°C or 200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the holding time of the heating treatment is 20-300 min, for example, it can be 80°C, 100°C, 120°C, 140°C, 160°C, 180°C or 200°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] Compared with the prior art, the present invention has the following beneficial effects:

[0042] (1) The present invention provides a heterogeneous catalyst for synthesizing cyclic carbonates. The catalyst has low production cost, strong alkalinity, high stability, can be reused multiple times, and can be scaled up for production. Compared with homogeneous catalysts, it has the advantages of easy separation of the catalyst and the product and high product selectivity.

[0043] (2) When the catalyst prepared by the present invention is used to synthesize cyclic carbonates, the process is simple and the experimental conditions are mild. Compared with other synthesis routes, it does not require harsh conditions such as solvents, high temperature and high pressure, and the reaction time is shorter; the diol conversion rate is as high as over 92%, and the selectivity and yield of cyclic carbonates are both as high as over 91%. DETAILED DESCRIPTION

[0044] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0045] Example 1

[0046] This embodiment provides a preparation method and application of a cerium-containing catalyst, the preparation method and application comprising the following steps:

[0047] (1) 7.68 g of Mg(NO3)2·6H2O, 3.455 g of Al(NO3)3·9H2O, 0.65 g of Ce(NO3)3·6H2O and 100 ml of deionized water were mixed to prepare solution A, and the mixture was dispersed under ultrasonic stirring for 1 h. NaOH and Na2CO3 were dissolved in deionized water to prepare solution B with a hydroxide ion concentration of 4 mol / L. Solution B was then added dropwise to solution A at a rate of 90 drops / min through a basic burette until the pH of the mixed solution reached 10, thereby obtaining a mixed solution.

[0048] (2) After stirring the mixed solution in step (1) for 1 hour, the mixture was crystallized at 120° C. for 12 hours, and the obtained slurry was filtered. The filtered solid was washed with deionized water until neutral, and then dried at 100° C. for 18 hours. After drying, the solid was ground and calcined at 600° C. for 5 hours to obtain Mg3Al 0.9 Ce 0.1 O composite catalyst;

[0049] (3) 18.0 g of dimethyl carbonate, 3.1 g of ethylene glycol and 0.17 g of the Mg3Al obtained in step (2) were added. 0.9 Ce 0.1 O was added into the reactor, the reaction temperature was 150°C, and the reaction was carried out at 750 rpm for 100 min to obtain a cyclic carbonate.

[0050] Example 2

[0051] This embodiment provides a preparation method and application of a cerium-containing catalyst, the preparation method and application comprising the following steps:

[0052] (1) 5.12 g of Mg(NO3)2·6H2O, 0.375 g of Al(NO3)3·9H2O, 3.91 g of Ce(NO3)3·6H2O and 100 ml of deionized water were mixed to prepare solution A, and the mixture was dispersed under ultrasonic stirring for 2 h. NaOH and NaHCO3 were dissolved in deionized water to prepare solution B with a hydroxide ion concentration of 2 mol / L. Solution B was then added dropwise to solution A at a rate of 150 drops / min through a basic burette until the pH of the mixed solution reached 9, thereby obtaining a mixed solution.

[0053] (2) After stirring the mixed solution in step (1) for 2 hours, the mixed solution was crystallized at 180°C for 8 hours to obtain a slurry, which was filtered. The filtered solid was washed with deionized water several times until it was neutral, and then dried at 120°C for 12 hours. After drying, the solid was ground and calcined at 800°C for 2 hours to obtain Mg2Al0.9 Ce 0.1 O catalyst;

[0054] (3) 9.0 g of dimethyl carbonate, 3.1 g of ethylene glycol and 0.07 g of Mg2Al obtained in step (2) were added. 0.9 Ce 0.1 O was added into the reactor, the reaction temperature was 200°C, and the reaction was carried out at 750 rpm for 20 min to obtain a cyclic carbonate.

[0055] Example 3

[0056] This embodiment provides a preparation method and application of a cerium-containing catalyst, the preparation method and application comprising the following steps:

[0057] (1) 10.24 g of Mg(NO3)2·6H2O, 3.455 g of Al(NO3)3·9H2O, 0.65 g of Ce(NO3)3·6H2O and 100 ml of deionized water were mixed to prepare solution A, and the mixture was dispersed under ultrasonic stirring for 1 h. NaOH was dissolved in deionized water to prepare solution B with a hydroxide ion concentration of 10 mol / L. Solution B was then added dropwise to solution A at a rate of 20 drops / min through a basic burette until the pH of the mixed solution reached 11, thereby obtaining a mixed solution.

[0058] (2) After stirring the mixed solution in step (1) for 0.5 h, the mixed solution was crystallized at 60° C. for 24 h to obtain a slurry, which was filtered. The filtered solid was washed with deionized water several times until it was neutral, and then dried at 70° C. for 24 h. After drying, the solid was ground and calcined at 400° C. for 8 h to obtain Mg4Al 0.9 Ce 0.1 O catalyst;

[0059] (3) 45.0 g of dimethyl carbonate, 3.1 g of ethylene glycol and 0.62 g of the Mg4Al4O3 obtained in step (2) were added to the mixture. 0.9 Ce 0.1 O was added into the reactor, the reaction temperature was 80°C, and the reaction was carried out at 750 rpm for 300 min to obtain a cyclic carbonate.

[0060] Example 4

[0061] This embodiment provides a preparation method and application of a cerium-containing catalyst, the preparation method and application comprising the following steps:

[0062] (1) 7.68 g of Mg(NO3)2·6H2O, 3.376 g of Al(NO3)3·9H2O, 0.432 g of Ce(NO3)3·6H2O and 100 ml of deionized water were mixed to prepare solution A, and the mixture was dispersed under ultrasonic stirring for 0.5 h. NaOH and Na2CO3 were dissolved in deionized water to prepare solution B with a hydroxide ion concentration of 4 mol / L. Solution B was then added dropwise to solution A at a rate of 90 drops / min through a basic burette until the pH of the mixed solution reached 10.5, thereby obtaining a mixed solution.

[0063] (2) After stirring the mixed solution in step (1) for 0.5 h, the mixed solution was crystallized at 60° C. for 12 h to obtain a slurry, which was filtered. The filtered solid was washed with deionized water several times until it was neutral, and then dried at 80° C. for 12 h. After drying, the solid was ground and calcined at 500° C. for 5 h to obtain Mg3Al 0.9 Ce 0.1 O catalyst;

[0064] (3) 18.0 g of dimethyl carbonate, 3.1 g of ethylene glycol and 0.17 g of Mg3Al2O3 prepared in step (2) were added to the mixture. 0.9 Ce 0.1 O was added into the reactor, the reaction temperature was 150°C, and the reaction was carried out at 750 rpm for 40 min to obtain a cyclic carbonate.

[0065] Example 5

[0066] The only difference between this embodiment and embodiment 4 is that the reaction time in step (3) is 30 min, and the other conditions are the same as those in embodiment 4.

[0067] Example 6

[0068] The only difference between this embodiment and embodiment 4 is that the reaction temperature in step (3) is 120° C., and the other conditions are the same as those in embodiment 4.

[0069] Example 7

[0070] The only difference between this embodiment and embodiment 6 is that the catalyst after the synthesis of cyclic carbonate in step (3) of embodiment 6 is separated, washed and dried, and then the catalyst is reused in step (3) to catalyze the synthesis of cyclic carbonate. The catalyst is reused 5 times. Other conditions are the same as those in embodiment 6.

[0071] Example 8

[0072] The only difference between this embodiment and embodiment 5 is that step (1) "3.376g Al(NO3)3·9H2O, 0.432g Ce(NO3)3·6H2O" is replaced by "1.875g Al(NO3)3·9H2O, 2.171g Ce(NO3)3·6H2O", and the other conditions are the same as those in embodiment 4.

[0073] Example 9

[0074] The only difference between this embodiment and embodiment 8 is that in step (3), "3.1 g ethylene glycol" is replaced by "3.1 g 1.2-propylene glycol", and the other conditions are the same as those in embodiment 8.

[0075] Example 10

[0076] The only difference between this embodiment and embodiment 8 is that "3.1 g ethylene glycol" in step (3) is replaced by "3.1 g 1,2-butanediol" and the reaction temperature in step (3) is 160°C. Other conditions are the same as those in embodiment 8.

[0077] Embodiment 11

[0078] The only difference between this embodiment and embodiment 4 is that the temperature of the calcination treatment in step (2) is 300° C., and the other conditions are the same as those in embodiment 4.

[0079] Example 12

[0080] The only difference between this embodiment and embodiment 4 is that the temperature of the calcination treatment in step (2) is 900° C., and the other conditions are the same as those in embodiment 4.

[0081] Comparative Example 1

[0082] This comparative example provides a preparation method and application of a cerium-containing catalyst, and the preparation method and application include the following steps:

[0083] (1) 2.171 g of Ce(NO3)3·6H2O and 100 ml of deionized water were mixed and dispersed under ultrasonic stirring for 0.5 h, NaOH was dissolved in deionized water to prepare a solution B with a hydroxide ion concentration of 4 mol / L, and then solution B was added to solution A at a rate of 90 drops / min through a basic burette until the pH of the mixed solution reached 10.5, thereby obtaining a mixed solution;

[0084] (2) After stirring the mixed solution in step (1) for 0.5 h, the mixed solution was crystallized at 60° C. for 12 h to obtain a slurry, which was filtered. The filtered solid was washed with deionized water several times until it was neutral, and then dried at 80° C. for 12 h. After drying, the solid was ground and calcined at 500° C. for 5 h to obtain a CeO2 catalyst;

[0085] (3) 18.0 g of dimethyl carbonate, 3.1 g of ethylene glycol and 0.17 g of the CeO2 catalyst prepared in step (2) were added to a reactor at a reaction temperature of 120° C. and reacted at 750 rpm for 40 min to obtain a cyclic carbonate.

[0086] Comparative Example 2

[0087] The difference between this comparative example and comparative example 1 is that the "2.171 g Ce(NO3)3·6H2O" in step (1) is replaced by "1.875 g Al(NO3)3·9H2O", and the other conditions are the same as those in comparative example 1.

[0088] Comparative Example 3

[0089] The only difference between this comparative example and comparative example 1 is that the "2.171 g Ce(NO3)3·6H2O" in step (1) is replaced by "7.68 g Mg(NO3)2·6H2O", and the other conditions are the same as those in comparative example 1.

[0090] Comparative Example 4

[0091] The only difference between this comparative example and comparative example 1 is that the "2.171 g Ce(NO3)3·6H2O" in step (1) is replaced by "7.68 g Mg(NO3)2·6H2O and 1.875 g Al(NO3)3·9H2O", and the other conditions are the same as those in comparative example 1.

[0092] Comparative Example 5

[0093] The only difference between this comparative example and comparative example 1 is that the "2.171 g Ce(NO3)3·6H2O" in step (1) is replaced by "7.68 g Mg(NO3)2·6H2O and 2.171 g Ce(NO3)3·6H2O", and the other conditions are the same as those in comparative example 1.

[0094] The cyclic carbonate solution obtained in step (3) of Example 1-12 and Comparative Example 1-5 was centrifuged at 3000 rpm for 3 min, and an appropriate amount of the supernatant was added with an internal standard substance (biphenyl) and quantitatively analyzed by gas chromatography internal standard method. The test results are shown in Table 1.

[0095] Table 1

[0096]

[0097]

[0098] It can be seen from Table 1 that the cerium-containing catalyst prepared by the present invention is applied to the synthesis of cyclic carbonates, and the glycol conversion rate is ≥92%, the product cyclic carbonate selectivity is ≥91%, and the cyclic carbonate yield is as high as more than 91%; the cerium-containing catalyst prepared in Example 7 still has a good catalytic effect when reused 5 times, and the cyclic carbonate yield is still ≥90%; It can be seen from Examples 8, 9, and 10 that the prepared cerium-containing catalyst can achieve a relatively high selectivity and yield for the corresponding cyclic carbonate products, whether it is for the preparation of ethylene carbonate from ethylene glycol, the preparation of propylene carbonate from 1,2-propylene glycol, or the preparation of butylene carbonate from 1,2-butanediol; Example 11 The calcination treatment temperature is too low, resulting in incomplete reaction, and the soluble salts of magnesium, aluminum and cerium cannot be completely decomposed into the form of metal oxides, resulting in poor catalytic effect; Example 12 The calcination treatment temperature is too high, resulting in sintering of the catalyst, resulting in a decrease in surface area, a decrease in pore volume, a decrease in the dispersion of active sites, and a decrease in the contact area with the reactants, resulting in a poor catalytic effect.

[0099] The catalysts prepared in Comparative Examples 1-3 contain only a single metal oxide, the catalyst prepared in Comparative Example 4 is Mg-Al oxide, and the catalyst prepared in Comparative Example 5 is Mg-Ce oxide. When applied to the synthesis of cyclic carbonates, the selectivity and yield of cyclic carbonates are low, indicating that only when the catalyst contains three metals of magnesium, aluminum and cerium at the same time, the selectivity and yield of the catalytic synthesis of cyclic carbonates are good.

[0100] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. Use of a stable cerium-containing catalyst, characterized in that: The cerium-containing catalyst is used for synthesizing cyclic carbonates. The method comprises the following steps: mixing and stirring carbonate, diol and a cerium-containing catalyst and then heating to obtain a cyclic carbonate; the molar ratio of the carbonate to the diol is (2-10):1; The diol includes 1,2-propylene glycol, and the prepared cyclic carbonate includes cyclic propylene carbonate; The cerium-containing catalyst is prepared by the following preparation method, which comprises the following steps: (1) mixing soluble salts of magnesium, aluminum and cerium with a solvent, dispersing them under ultrasonic stirring for 0.5-2 hours, and then adding an alkaline solution to the soluble salts and the solvent at a rate of 20-150 drops / min to obtain a mixed solution; (2) After stirring the mixed solution in step (1), crystallization treatment, drying treatment and calcination treatment are sequentially performed to obtain the cerium-containing catalyst.

2. The use according to claim 1, characterized in that: The molar ratio of the soluble salt of magnesium to the soluble salts of aluminum and cerium in step (1) is (2-4):

1.

3. The use according to claim 1, characterized in that: The soluble salt of magnesium in step (1) includes any one of magnesium nitrate, magnesium chloride, magnesium carbonate or magnesium sulfate, or a combination of at least two thereof.

4. The use according to claim 1, characterized in that: The soluble salt of aluminum in step (1) includes any one of aluminum nitrate, aluminum chloride, aluminum carbonate or aluminum sulfate, or a combination of at least two thereof.

5. The use according to claim 1, characterized in that: The soluble salt of cerium in step (1) includes any one of cerium nitrate, cerium chloride, cerium sulfate or cerium acetate, or a combination of at least two thereof.

6. The use according to claim 1, characterized in that: The alkali in the alkaline solution of step (1) includes any one of NaOH, KOH, NaHCO3, Na2CO3 or ammonia water, or a combination of at least two of them.

7. The use according to claim 6, characterized in that: The hydroxide ion concentration of the alkaline solution in step (1) is 2-10 mol / L.

8. The use according to claim 1, characterized in that: The solvent in step (1) includes deionized water.

9. The use according to claim 1, characterized in that: The pH value of the mixed solution in step (1) is 9-11.

10. The use according to claim 1, characterized in that: The stirring time in step (2) is 0.5-2h.

11. The use according to claim 1, characterized in that: The temperature of the crystallization treatment in step (2) is 60-180°C.

12. The use according to claim 1, characterized in that: The crystallization treatment time in step (2) is 8-24 hours.

13. The use according to claim 1, characterized in that: After the crystallization treatment in step (2), the obtained mixed solution is subjected to solid-liquid separation treatment, and the obtained solid is washed to neutrality.

14. The use according to claim 1, characterized in that: The temperature of the drying treatment in step (2) is 70-120°C.

15. The use according to claim 1, characterized in that: The drying time in step (2) is 12-24 hours.

16. The use according to claim 1, characterized in that: The temperature of the calcination treatment in step (2) is 400-800°C.

17. The use according to claim 1, characterized in that: The calcination time in step (2) is 2-8 hours.

18. The use according to claim 1, characterized in that: The mass ratio of the cerium-containing catalyst to the diol is (0.001-0.2):

1.

19. The use according to claim 1, characterized in that: During the synthesis of the cyclic carbonate, the temperature of the heating treatment is 80-200°C.

20. The use according to claim 1, characterized in that: During the synthesis of the cyclic carbonate, the heat preservation time of the heating treatment is 20-300 minutes.