A preparation method of transition metal catalyst and its application
Through the chemical combination of collagen fibers and transition metal salts and two-stage carbonization treatment, the preparation complexity and cost of transition metal biochar material preparation are solved, the stability and activation performance of the catalyst are improved, and the efficient organic Pollutant degradation effect.
Patent Information
- Application Number
- CN202310185215.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-20
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-02-20
AI Technical Summary
The existing preparation methods for transition metal biochar materials have complex preparation processes, high preparation costs and metal leaching problems, which affect activation performance.
Collagen fibers are used as reaction raw materials, and reaction intermediates are generated through soaking and heating reactions, and two-stage carbonization is carried out, combined with alkaline solution activation treatment, to improve the carbonization rate and specific surface area of the material, promote the chemical combination of metals and collagen fibers, and reduce the Metal leaching.
The preparation process is simplified, the cost is reduced, the stability and activation performance of transition metal catalysts are improved, and efficient degradation of organic pollutants is achieved.
Smart Images

Figure CN116272990B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of catalytic material manufacturing, and specifically, to a method for preparing a transition metal catalyst and its application. Background Art
[0002] In the prior art, activated persulfate is usually used to treat organic pollutants. Among them, a commonly used activator is transition metal biochar. However, the current preparation method of this type of activator has problems such as complex preparation process, high preparation cost and metal leaching. Summary of the invention
[0003] The purpose of the present application is to provide a method for preparing a transition metal catalyst and its application, which can improve the problems of complex preparation process, high preparation cost and metal leaching in the preparation method of transition metal biochar materials to a certain extent.
[0004] The embodiment of the present application is implemented as follows:
[0005] In a first aspect, the present invention provides a method for preparing a transition metal catalyst, comprising the following steps:
[0006] Soaking collagen fibers in a first solvent to obtain a first reaction precursor, wherein the pH of the first solvent is ≤7; mixing the first reaction precursor with a second reaction precursor containing a transition metal salt and heating the mixture to obtain a reaction intermediate; performing solid-liquid separation on the reaction intermediate to obtain a solid-phase reaction intermediate; heating and carbonizing the solid-phase reaction intermediate to obtain a transition metal catalyst;
[0007] Optionally, the second reaction precursor is prepared by dissolving a transition metal salt in a second solvent, wherein the pH of the second solvent is ≤7.
[0008] In the above technical scheme, collagen fibers are directly used as reaction raw materials, and the reaction solvent does not need to be adjusted to acidity in advance. Compared with the conventional preparation method (which requires an acid adjustment step in advance), the preparation process can be simplified and the preparation cost can be reduced; at the same time, in the preparation process provided in the embodiment of the present application, collagen fibers and transition metal salts are added in steps and then mixed and reacted. Compared with the conventional preparation method (the two are added to the solvent at the same time and mixed, which is basically a physical combination, causing the metal ions to be particularly easy to fall off and leach), collagen fibers and transition metals are mostly chemically combined (ionic coordination), and the stability of the two is higher, which can solve the problem of metal leaching to a certain extent.
[0009] Furthermore, the form of preparing the transition metal salt into a solution in advance and then mixing it with the collagen fibers in the first reaction precursor can improve the mixing uniformity of the two compared to directly adding the transition metal salt powder, and at the same time, it also facilitates the coordination reaction between the two.
[0010] In some optional embodiments, in the step of soaking the collagen fibers in the first solvent, the mass ratio of the collagen fibers to the first solvent is (1-2):(25-35), and / or the soaking time is 8-12 hours.
[0011] In the above technical solution, during the soaking process, the mass ratio of the collagen fibers to the first solvent and the soaking time are respectively limited within specific ranges, so that the collagen fibers have a suitable structural looseness after soaking, thereby better cooperating and combining with the transition metal.
[0012] In some optional embodiments, the mass ratio of collagen fibers to transition metal salt is (10-20):(5-10).
[0013] In the above technical solution, the mass ratio of collagen fibers and transition metal salts is limited to a specific range, so that the two have a suitable usage ratio, so that the transition metal can be better coordinated and combined with the collagen fibers.
[0014] In some optional embodiments, in the step of heating the reaction, the treatment temperature is 35-45° C., and the treatment time is 5-7 h.
[0015] In the above technical solution, the processing temperature and time in the heating reaction step are limited to specific ranges, respectively, so that the heating reaction can be carried out at a suitable temperature and duration, thereby allowing the collagen fibers and the transition metal salt to be better combined together.
[0016] In some optional embodiments, the metal ions in the transition metal salt include Fe 3+ 、Co 2+ and Cu 2+ At least one of .
[0017] The several transition metals provided in the embodiments of the present application are the most commonly used metals in persulfate activators and can be applied to most organic pollutant systems in this field, thereby facilitating the promotion and application of the technical solutions provided in the embodiments of the present application.
[0018] In some optional embodiments, the step of heating and carbonizing includes firstly performing a first stage of carbonization and then raising the temperature to perform a second stage of carbonization.
[0019] In the above technical solution, the two-stage carbonization method is adopted, which can increase the carbonization rate of the material and thus improve the activation performance of the material compared to the one-stage carbonization method.
[0020] In some optional embodiments, during the first stage carbonization, the treatment temperature is 300-500°C and the treatment time is 2-4 hours; and / or, during the second stage carbonization, the treatment temperature is 700-900°C and the treatment time is 2-4 hours.
[0021] In the above technical solution, the temperature and time in the two carbonization processes are limited to specific ranges respectively, so that the two carbonization processes can be carried out under more suitable conditions. Compared with not being within the specific range, the carbonization effect of the material can be improved.
[0022] In some optional embodiments, between the first stage carbonization and the second stage carbonization, an activation treatment is further included using an alkaline solution to the solid phase reaction intermediate after the first stage carbonization treatment;
[0023] Optionally, the mass ratio of the alkaline solution to the solid phase reaction intermediate is (3-5):1;
[0024] Optionally, the activation treatment time is 2 to 4 hours.
[0025] In the above technical solution, adding an activation treatment between the first stage carbonization and the second stage carbonization can promote the formation of pores inside the material and increase the specific surface area of the material, thereby providing more catalytic sites.
[0026] Furthermore, by limiting the mass ratio of the alkaline solution to the solid phase reaction intermediate and the activation time within a specific range, the two can have a suitable dosage ratio, thereby being able to better activate the solid phase reaction intermediate.
[0027] In a second aspect, an embodiment of the present application provides an application of a transition metal catalyst in the degradation of organic pollutants, wherein the transition metal catalyst is prepared using the preparation method of the transition metal catalyst provided in the embodiment of the first aspect.
[0028] In some optional embodiments, the following steps are included:
[0029] First, persulfate is activated with a transition metal catalyst, and then the activated persulfate is used to degrade organic pollutants;
[0030] Optionally, in the activation solution system for activating persulfate with a transition metal catalyst, the concentration ratio of the transition metal catalyst to the persulfate is (0.02-0.08) g / L: (1-3) mM;
[0031] Optionally, during the process of degrading organic pollutants, the treatment time is 30 to 60 minutes.
[0032] In the above technical solution, persulfate activated by a transition metal catalyst is used to degrade organic pollutants, which has the advantages of being green and efficient.
[0033] Furthermore, in the activation solution system for activating persulfate with a transition metal catalyst, limiting the concentration ratio of the transition metal catalyst to the persulfate within a specific range can make the two have an appropriate dosage ratio, thereby enabling better activation of the persulfate.
[0034] Furthermore, in the process of degrading organic pollutants, the treatment time is limited to a specific range. On the one hand, it can effectively avoid the failure to effectively remove organic pollutants due to a short treatment time, and on the other hand, it can effectively avoid the waste of time due to too long treatment time (after reaching the degradation saturation, continuing to extend the time will not significantly improve the degradation effect, but will only cause a waste of time). BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 A process flow chart of a method for preparing a transition metal catalyst provided in an embodiment of the present application;
[0037] Figure 2 The activation performance test results of a series of transition metal catalysts provided in Examples 1 to 3 of the present application;
[0038] Figure 3 The activation performance test results of a series of transition metal catalysts provided in Examples 4 to 6 of the present application;
[0039] Figure 4 The activation performance test results of a series of transition metal catalysts provided in Examples 7 to 9 of the present application;
[0040] Figure 5 to Figure 7 The activation performance test results of a series of transition metal catalysts provided in Examples 1 to 3 of the present application under the action of different quenchers;
[0041] Figure 8 This is a statistical diagram of the activation paths of a series of transition metal catalysts provided in Examples 1 to 3 of the present application. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0043] It should be noted that “and / or” in this application, such as “Feature 1 and / or Feature 2”, refers to the three situations of “Feature 1” alone, “Feature 2” alone, or “Feature 1” plus “Feature 2”.
[0044] In addition, in the description of the present application, unless otherwise specified, the meaning of "multiple" in "one or more" refers to two or more; the range of "value a ~ value b" includes the two end values "a" and "b", and the "unit" in "value a ~ value b + unit of measurement" represents the "unit of measurement" of both "value a" and "value b".
[0045] In the prior art, activated persulfate is usually used to treat organic pollutants. The activation pathways of persulfate are divided into free radical pathways and non-free radical pathways, which differ significantly in terms of generation pathways, action mechanisms, and degradation performance of organic pollutants. In the free radical activation pathway, persulfate is activated to first break OO to generate sulfate radicals (SO4 ·- ), and then a continuous free radical chain reaction occurs in the solution to produce hydroxyl radicals (·OH), SO4 ·- The strong oxidizing ability of ·OH can quickly oxidize and decompose organic pollutants. However, the degradation ability of free radicals generated in this activation method is easily affected by coexisting substances in the natural water environment, and even produces more toxic byproducts, which poses a risk of secondary pollution. In the non-radical activation pathway, persulfate includes four forms: singlet oxygen, electron transfer, surfactants, and high-valent metals. Unlike free radicals generated in solution, non-free radicals are mainly generated on the catalyst surface. Therefore, the surface physicochemical properties of the catalyst, such as the degree of defects, the type of functional groups, and the ability to transfer electrons, are closely related to the non-radical activation pathway.
[0046] On this basis, technicians in this field have discovered that transition metal biochar materials can activate persulfate through both free radical pathways and non-free radical pathways, and also have the advantages of being highly efficient, green and pollution-free.
[0047] However, the current preparation methods of transition metal biochar materials usually require a preliminary acid adjustment step and corresponding post-treatment steps (such as subsequent cleaning and acid removal processes), which makes the preparation process more complicated. At the same time, the transition metal salts in the current preparation process are usually directly mixed with the carbon source for reaction, so that most of the transition metals are physically combined with the carbon material, which makes it easy to cause metal leaching problems later, and then leads to poor activation performance of the prepared activator.
[0048] Through creative research, the researchers of this application found that by optimizing the types of reaction raw materials and the method of adding materials, the problems of complex preparation process, high preparation cost and metal leaching in the preparation method of transition metal biochar materials can be improved to a certain extent.
[0049] The following is a detailed description of a method for preparing a transition metal catalyst according to an embodiment of the present application and its application.
[0050] In a first aspect, the present invention provides a method for preparing a transition metal catalyst, comprising the following steps:
[0051] The collagen fibers are immersed in a first solvent to obtain a first reaction precursor, wherein the pH of the first solvent is ≤7; the first reaction precursor is mixed with a second reaction precursor containing a transition metal salt and then heated to react to obtain a reaction intermediate; the reaction intermediate is subjected to solid-liquid separation to obtain a solid-phase reaction intermediate; the solid-phase reaction intermediate is heated and carbonized to obtain a transition metal catalyst.
[0052] In the present application, collagen fibers are directly used as the reaction raw material, and there is no need to adjust the reaction solvent to acidity in advance. Compared with the conventional preparation method (which requires an acidity adjustment step in advance), the preparation process can be simplified and the preparation cost can be reduced; at the same time, in the preparation process provided in the embodiment of the present application, collagen fibers and transition metal salts are added in steps and then mixed and reacted. Compared with the conventional preparation method (the two are added to the solvent at the same time and mixed, which is basically a physical combination, causing the metal ions to be particularly easy to fall off and leached), collagen fibers and transition metals are mostly chemically combined (ionic coordination), and the stability of the two is higher, which can solve the problem of metal leaching to a certain extent.
[0053] It is understandable that the form of the second reaction precursor may be adjusted in consideration of the mixing uniformity of the collagen fibers and the transition metal.
[0054] As an example, the second reaction precursor is prepared by dissolving a transition metal salt in a second solvent, wherein the pH of the second solvent is ≤7.
[0055] It should be noted that the compositions of the first solvent and the second solvent may be the same or different, as long as the pH requirement is met.
[0056] Illustratively, the first solvent and the second solvent in the embodiments of the present application are both deionized water.
[0057] In this embodiment, the transition metal salt is prepared into a solution in advance and then mixed with the collagen fibers in the first reaction precursor. Compared with directly adding the transition metal salt powder, this can improve the mixing uniformity of the two and also facilitate the coordination reaction between the two.
[0058] It should be noted that, considering the binding effect between the collagen fibers and the transition metal, the relevant parameters in the immersion process (such as immersion time, the mass ratio of the collagen fibers to the first solvent, etc.) can be adjusted.
[0059] As an example, in the step of soaking the collagen fibers in the first solvent, the mass ratio of the collagen fibers to the first solvent is (1-2): (25-35), for example but not limited to a mass ratio of 1:25, 1:30, 1:35, 2:25, 2:30 and 2:35, or a range between any two of the mass ratios; and / or the soaking time is 8-12 hours, for example but not limited to a soaking time of 8 hours, 9 hours, 10 hours, 11 hours and 12 hours, or a range between any two of the mass ratios.
[0060] In this embodiment, during the soaking process, the mass ratio of the collagen fibers to the first solvent and the soaking time are respectively limited within specific ranges, so that the collagen fibers have a suitable structural looseness after soaking, thereby better cooperating and combining with the transition metal.
[0061] It should be noted that, considering the binding effect of collagen fibers and transition metals, the dosage ratio of the two can be adjusted.
[0062] As an example, the mass ratio of collagen fibers and transition metal salts is (10-20):(5-10), for example but not limited to, the mass ratio is any one of 10:5, 10:8, 10:10, 15:5, 15:8, 15:10, 20:5, 20:8 and 20:10 or a range between any two of them.
[0063] In this embodiment, the mass ratio of the collagen fibers and the transition metal salt is limited to a specific range, so that the two can have a suitable usage ratio, so that the transition metal can be better coordinated and bonded with the collagen fibers.
[0064] It should be noted that the parameters during the heating reaction can be adjusted considering the binding effect between collagen fibers and transition metals.
[0065] As an example, in the heating reaction step, the processing temperature is 35-45°C, for example but not limited to the temperature of any one of 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C and 45°C, or a range between any two of them; the processing time is 5-7h, for example but not limited to the time of any one of 5h, 6h and 7h, or a range between any two of them.
[0066] In this embodiment, the treatment temperature and time in the heating reaction step are limited to specific ranges, respectively, so that the heating reaction can be carried out at a suitable temperature and duration, thereby allowing the collagen fibers and the transition metal salt to be better combined together.
[0067] It should be noted that the type of transition metal is not limited and can be adjusted according to actual needs.
[0068] As an example, the metal ions in the transition metal salt include Fe 3+ 、Co 2+ and Cu 2+ At least one of .
[0069] In this embodiment, the several transition metals provided in the examples of the present application are the most commonly used metals in persulfate activators and can be applied to most organic pollutant systems in this field, thereby facilitating the promotion and application of the technical solutions provided in the examples of the present application.
[0070] As an example, in the step of heating carbonization, a first stage carbonization is performed first, and then the temperature is increased to perform a second stage carbonization.
[0071] In this embodiment, a two-stage carbonization method is adopted, which can increase the carbonization rate of the material and thus improve the activation performance of the material compared to a one-stage carbonization method.
[0072] It is understandable that the treatment temperature and treatment time in the two-stage carbonization process can be adjusted in consideration of the carbonization effect.
[0073] As an example, during the first stage carbonization process, the treatment temperature is 300-500°C, for example but not limited to any one of 300°C, 350°C, 400°C, 450°C and 500°C, or a range between any two of them; the treatment time is 2-4h, for example but not limited to any one of 2h, 3h and 4h, or a range between any two of them; and / or, during the second stage carbonization process, the treatment temperature is 700-900°C, for example but not limited to any one of 700°C, 750°C, 800°C, 850°C and 900°C, or a range between any two of them; the treatment time is 2-4h, for example but not limited to any one of 2h, 3h and 4h, or a range between any two of them.
[0074] In this embodiment, the temperature and time in the two carbonization processes are respectively limited to specific ranges, so that the two carbonization processes can be carried out under more suitable conditions, which can improve the carbonization effect of the material compared to when the temperature and time are not within the specific range.
[0075] As an example, between the first stage carbonization and the second stage carbonization, an activation treatment is further included using an alkaline solution to the solid phase reaction intermediate after the first stage carbonization treatment.
[0076] In this embodiment, an activation treatment is added between the first stage carbonization and the second stage carbonization, which can promote the formation of pores inside the material and increase the specific surface area of the material, thereby providing more catalytic sites.
[0077] It should be noted that the type of alkaline solution is not limited and can be selected according to routine practice in the art.
[0078] As an example, the alkaline solution includes at least one of potassium hydroxide, potassium carbonate and potassium bicarbonate.
[0079] It is understood that the ratio of the alkaline solution to the solid phase reaction intermediate and the time of the activation treatment can be adjusted in consideration of the activation effect.
[0080] As an example, the mass ratio of the alkaline solution to the solid phase reaction intermediate is (3-5):1, such as but not limited to any one of 3:1, 4:1 and 5:1 or a range between any two of the mass ratios.
[0081] As an example, the activation treatment time is 2 to 4 hours, for example but not limited to any one of 2 hours, 3 hours and 4 hours or a range between any two of them.
[0082] In this embodiment, the mass ratio of the alkaline solution to the solid phase reaction intermediate and the activation time are limited within a specific range, so that the two can have a suitable dosage ratio, thereby being able to better activate the solid phase reaction intermediate.
[0083] It should be noted that, in the preparation process of the transition metal catalyst, any step not specifically described or limited may be arranged according to conventional selection in the art.
[0084] As an example, after obtaining the solid phase reaction intermediate and before heating and carbonization, the method further includes the steps of alternately washing and drying the solid phase reaction intermediate with ethanol and deionized water.
[0085] As an example, the heating carbonization process is performed under an inert atmosphere.
[0086] As an example, the process flow chart of a method for preparing a transition metal catalyst provided in an embodiment of the present application is exemplarily as follows: Figure 1 shown.
[0087] In a second aspect, an embodiment of the present application provides an application of a transition metal catalyst in the degradation of organic pollutants, wherein the transition metal catalyst is prepared using the preparation method of the transition metal catalyst provided in the embodiment of the first aspect.
[0088] It should be noted that the types of organic pollutants are not limited and can be set according to routine selection in the art.
[0089] As an example, the degradation of organic pollutants includes the following steps:
[0090] The persulfate is first activated with a transition metal catalyst, and then the activated persulfate is used to degrade organic pollutants.
[0091] In this embodiment, persulfate activated by a transition metal catalyst is used to degrade organic pollutants, which has the advantages of being green and efficient.
[0092] It should be noted that the concentration ratio of the transition metal catalyst to the persulfate may be adjusted in consideration of the activation effect.
[0093] As an example, in the activation solution system of persulfate activated by a transition metal catalyst, the concentration ratio of the transition metal catalyst to the persulfate is (0.02-0.08) g / L: (1-3) mM, for example but not limited to, the concentration ratio is any one of 0.02 g / L: 1 mM, 0.02 g / L: 3 mM, 0.04 g / L: 1 mM, 0.04 g / L: 3 mM, 0.06 g / L: 1 mM, 0.06 g / L: 3 mM, 0.08 g / L: 1 mM and 0.08 g / L: 3 mM, or a range between any two of them.
[0094] In this embodiment, in the activation solution system for activating persulfate with a transition metal catalyst, the concentration ratio of the transition metal catalyst to the persulfate is limited to a specific range, so that the two can have a suitable dosage ratio, thereby being able to better activate the persulfate.
[0095] It should be noted that the treatment time can be adjusted considering the degradation effect of organic pollutants.
[0096] As an example, in the process of degrading organic pollutants, the treatment time is 30 to 60 minutes, for example but not limited to any one of 30 minutes, 40 minutes, 50 minutes and 60 minutes, or a range between any two of them.
[0097] In this embodiment, during the process of degrading organic pollutants, the treatment time is limited to a specific range. On the one hand, it can effectively avoid the failure to effectively remove organic pollutants due to short treatment time, and on the other hand, it can effectively avoid the waste of time due to too long treatment time (after reaching the degradation saturation, continuing to extend the time will not significantly improve the degradation effect, but will only cause a waste of time).
[0098] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0099] Example 1
[0100] The present invention provides a method for preparing a transition metal catalyst, comprising the following steps:
[0101] The washed and dried collagen fibers are immersed in deionized water to obtain a first reaction precursor; wherein the mass ratio of the collagen fibers to the deionized water is 1.5:30, and the immersion time is 12 hours.
[0102] Dissolve ferric sulfate in deionized water to obtain a second reaction precursor; wherein the mass ratio of ferric sulfate to deionized water is 8:150, and the mass ratio of ferric sulfate to collagen fibers is 2:1.
[0103] The first reaction precursor and the second reaction precursor are mixed and heated to react to obtain a reaction intermediate, and then the reaction intermediate is subjected to solid-liquid separation to obtain a solid-phase reaction intermediate; wherein the treatment temperature is 40° C. and the treatment time is 6 hours.
[0104] The solid-phase reaction intermediate is subjected to the first-stage carbonization, activation treatment and the second-stage carbonization in sequence to obtain a transition metal catalyst; wherein, the treatment temperature of the first-stage carbonization is 400°C, and the treatment time is 2h; the alkaline solution of the activation treatment is 4 mol / L potassium hydroxide, the mass ratio of the activation solution to the solid-phase reaction intermediate is 4:1, and the activation treatment time is 3h; the treatment temperature of the second-stage carbonization is 800°C, and the treatment time is 2h.
[0105] Example 2
[0106] The embodiment of the present application provides a method for preparing a transition metal catalyst, which differs from Embodiment 1 only in that iron sulfate is replaced with cobalt sulfate.
[0107] Example 3
[0108] The embodiment of the present application provides a method for preparing a transition metal catalyst, which differs from Embodiment 1 only in that iron sulfate is replaced by copper sulfate.
[0109] Example 4
[0110] The embodiment of the present application provides a method for preparing a transition metal catalyst, which differs from Embodiment 1 only in that iron sulfate is directly mixed with a first reaction precursor and then heated for reaction.
[0111] Example 5
[0112] The embodiment of the present application provides a method for preparing a transition metal catalyst, which differs from the embodiment 1 only in that cobalt sulfate is directly mixed with a first reaction precursor and then heated for reaction.
[0113] Example 6
[0114] The embodiment of the present application provides a method for preparing a transition metal catalyst, which differs from Embodiment 1 only in that copper sulfate is directly mixed with a first reaction precursor and then heated for reaction.
[0115] Example 7
[0116] This embodiment of the present application provides a method for preparing a transition metal catalyst, which differs from Embodiment 1 only in that no activation treatment is performed.
[0117] Example 8
[0118] This embodiment of the present application provides a method for preparing a transition metal catalyst, which differs from Embodiment 2 only in that no activation treatment is performed.
[0119] Example 9
[0120] This embodiment of the present application provides a method for preparing a transition metal catalyst, which differs from Embodiment 3 only in that no activation treatment is performed.
[0121] Test Example 1
[0122] Activation performance test of transition metal catalysts
[0123] Test method:
[0124] The transition metal catalysts prepared according to the preparation methods of Examples 1 to 9 were numbered respectively, and then, sodium persulfate was used to activate the catalysts with the same dosage standard, and then, the activated sodium persulfate was used to degrade ciprofloxacin, and the residual concentration of ciprofloxacin changing with time was recorded respectively; at the same time, sodium persulfate alone was used as a control example; wherein, in the activation solution system, the concentration of the transition metal catalyst was 0.05 g / L, the concentration of sodium persulfate was 2 mM, and the concentration of ciprofloxacin was 20 mg / L.
[0125] See also Figure 2 It can be seen that the transition metal catalysts prepared in Examples 1 to 3 can effectively activate sodium persulfate to degrade ciprofloxacin, and the more suitable degradation time is 30 to 60 minutes.
[0126] It should be noted that Figure 2 In the embodiment, PDS is a control example, Fe / BC / PDS is a transition metal catalyst prepared in Example 1, Co / BC / PDS is a transition metal catalyst prepared in Example 2, and Cu / BC / PDS is a transition metal catalyst prepared in Example 3.
[0127] See also Figure 2 and Figure 3 It can be seen that, compared with Examples 1 to 3, the sodium persulfate activated by the transition metal catalyst prepared in Examples 4 to 6 can only degrade ciprofloxacin to a small extent, and the transition metal catalyst prepared in Example 4 has a serious metal leaching problem, indicating that preparing the metal salt into a solution and then mixing it with the first reaction precursor can prepare a transition metal catalyst with better performance.
[0128] It should be noted that Figure 3 In the embodiment, PDS is a control example, Fe / BC / PDS is a transition metal catalyst prepared in Example 4, Co / BC / PDS is a transition metal catalyst prepared in Example 5, and Cu / BC / PDS is a transition metal catalyst prepared in Example 6.
[0129] See also Figure 2 and Figure 4It can be seen that compared with Examples 1 to 3, the sodium persulfate activated with the transition metal catalyst prepared in Examples 7 to 9 can basically not degrade ciprofloxacin, indicating that adding an activation treatment between the first stage carbonization and the second stage carbonization can prepare a transition metal catalyst with better performance.
[0130] It should be noted that Figure 4 In this example, PDS is a control example, unactivated-Fe / BC / PDS is a transition metal catalyst prepared in Example 7, unactivated-Co / BC / PDS is a transition metal catalyst prepared in Example 8, and unactivated-Cu / BC / PDS is a transition metal catalyst prepared in Example 9.
[0131] Test Example 2
[0132] Study on the activation mechanism of transition metal catalysts
[0133] Test method:
[0134] The transition metal catalysts prepared according to the preparation methods of Examples 1 to 3 were numbered respectively, and then, each numbered catalyst was activated with sodium persulfate according to the same dosage standard, and then, the activated sodium persulfate was used to degrade ciprofloxacin containing different quenchers, and the residual concentration of ciprofloxacin changing with time was recorded respectively; at the same time, the quencher was not added as a control example; wherein, in the activation solution system, the concentration of the transition metal catalyst was 0.05 g / L, the concentration of sodium persulfate was 2 mM, and the concentration of ciprofloxacin was 20 mg / L; the quenchers included 5 kinds, namely: quenching OH and SO4 ·- Me-OH can quench OH TBA can quench O2 ·- p-BQ can quench 1 L-histidine of O2 and KI which can quench the electron transfer pathway.
[0135] It should be noted that None is a control example, and Fe / BC is the transition metal catalyst prepared in Example 1 (corresponding to Figure 5 ), Co / BC is the transition metal catalyst prepared in Example 2 (corresponding to Figure 6 ), Cu / BC is the transition metal catalyst prepared in Example 3 (corresponding to Figure 7 ).
[0136] See also Figures 5 to 8 It can be seen that Fe / BC can effectively promote the free radical pathway of persulfate (PDS), Cu / BC can effectively promote the non-free radical pathway of PDS, and Co / BC can simultaneously induce the free radical and non-free radical pathways of PDS.
[0137] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
Claims
1. A method for preparing a transition metal catalyst, It is characterized in that The following steps are involved: Soaking collagen fibers in a first solvent to obtain a first reaction precursor, wherein the pH of the first solvent is ≤7; The first reaction precursor is mixed with a second reaction precursor containing a transition metal salt and then heated to react to obtain a reaction intermediate; Performing solid-liquid separation on the reaction intermediate to obtain a solid-phase reaction intermediate; heating and carbonizing the solid phase reaction intermediate to obtain a transition metal catalyst; The metal ion in the transition metal salt is Cu 2+ .
2. The method for preparing a transition metal catalyst according to claim 1, It is characterized in that The second reaction precursor is prepared by dissolving a transition metal salt in a second solvent, wherein the pH of the second solvent is ≤7.
3. The method for preparing the transition metal catalyst according to claim 1, It is characterized in that In the step of immersing the collagen fibers in the first solvent, the mass ratio of the collagen fibers to the first solvent is (1-2):(25-35), and / or the immersion time is 8-12 hours.
4. The method for preparing the transition metal catalyst according to claim 1, It is characterized in that The mass ratio of the collagen fibers to the transition metal salt is (10-20):(5-10).
5. The method for preparing a transition metal catalyst according to any one of claims 1 to 4, It is characterized in that In the heating reaction step, the treatment temperature is 35-45° C. and the treatment time is 5-7 hours.
6. The method for preparing a transition metal catalyst according to any one of claims 1 to 4, It is characterized in that The heating carbonization step includes firstly performing a first stage carbonization and then raising the temperature to perform a second stage carbonization.
7. The method for preparing the transition metal catalyst according to claim 6, It is characterized in that In the first stage carbonization process, the treatment temperature is 300-500°C and the treatment time is 2-4h; and / or, During the second stage carbonization process, the treatment temperature is 700-900° C. and the treatment time is 2-4 hours.
8. The method for preparing the transition metal catalyst according to claim 6, It is characterized in that Between the first stage carbonization and the second stage carbonization, the method further includes using an alkaline solution to activate the solid phase reaction intermediate after the first stage carbonization treatment.
9. The method for preparing the transition metal catalyst according to claim 8, It is characterized in that The mass ratio of the alkaline solution to the solid phase reaction intermediate is (3-5):
1.
10. The method for preparing the transition metal catalyst according to claim 8, It is characterized in that The activation treatment time is 2 to 4 hours.
11. Application of a transition metal catalyst in the degradation of organic pollutants. It is characterized in that The transition metal catalyst is prepared by the preparation method of the transition metal catalyst according to any one of claims 1 to 10.
12. The use according to claim 11, It is characterized in that The following steps are involved: The persulfate is first activated by the transition metal catalyst, and then the activated persulfate is used to degrade organic pollutants.
13. The use according to claim 12, It is characterized in that In the activation solution system for activating the persulfate with the transition metal catalyst, the concentration ratio of the transition metal catalyst to the persulfate is (0.02-0.08) g / L: (1-3) mM.
14. The use according to claim 12, It is characterized in that In the process of degrading organic pollutants, the treatment time is 30 to 60 minutes.