A heteroatom molecular sieve M-HSUZ-4 catalyst and its preparation method and application

By constructing the heteroatom molecular sieve M-HSUZ-4 catalyst, introducing metal atoms and enhancing the B acid and L acid sites, the problems of catalyst stability and low conversion rate in the dimethyl ether carbonylation reaction were solved, and efficient methyl acetate was achieved. Ester synthesis has good industrial application prospects.

CN116273148BActive Publication Date: 2024-10-15SHANXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310139798.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-15
Publication Date
2024-10-15
Estimated Expiration
2043-02-15

AI Technical Summary

Technical Problem

In the prior art, the eight-membered ring-containing molecular sieve catalyst used in the carbonylation reaction of dimethyl ether has problems with low stability and low conversion rate, which limits its industrial application.

Method used

The preparation method of heteroatom molecular sieve M-HSUZ-4 catalyst is used to improve the catalytic performance by introducing metal atoms and constructing B acid and L acid sites.

Benefits of technology

The dimethyl ether carbonylation conversion rate and methyl acetate selectivity were significantly improved from 15.16% to 29.98%, while maintaining the stability and easy regeneration of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116273148B_ABST
    Figure CN116273148B_ABST
Patent Text Reader

Abstract

The present invention discloses a heteroatom molecular sieve M-HSUZ-4 catalyst and a preparation method and application, belonging to the technical field of heterogeneous catalytic materials. In view of the problems of high stability, high selectivity and low conversion rate in the process of dimethyl ether carbonylation reaction catalyzed by ordinary H-SUZ-4, the present invention is to add alkali source and aluminum source to deionized water in sequence, heat it to completely dissolved and then cool it to room temperature to obtain a transparent solution 1; slowly add a directing agent and a silicon source to deionized water in sequence and continuously stir to obtain a colloidal solution 2; slowly add the mixed colloidal solution 2 to the transparent solution 1, continuously stir and age to obtain a mixed gel, move it into a hydrothermal kettle, dynamically crystallize it in a homogeneous reactor, and obtain a K-SUZ-4 molecular sieve after washing, drying and roasting; treat the K-SUZ-4 molecular sieve with an ammonium salt solution to obtain an H-SUZ-4 molecular sieve; take a metal salt solution to treat the H-SUZ-4 molecular sieve to obtain a heteroatom molecular sieve M-SUZ-4. The method of the present invention has simple preparation process, low cost, good catalyst stability, easy regeneration, and broad prospects for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heterogeneous catalytic materials, and specifically relates to a heteroatom molecular sieve M-HSUZ-4 catalyst and a preparation method and application thereof. Background Art

[0002] Fuel ethanol (volume concentration ≥ 99.5%) is an important green energy source. It can be used as a fuel substitute to reduce dependence on petroleum energy; it can also be used as a gasoline additive to greatly improve gasoline combustion efficiency and reduce environmental pollution. At present, my country's apparent gasoline consumption is close to 150 million tons. If fuel ethanol is added at a ratio of 10%, the amount of fuel ethanol required is very large. However, at this stage, 80% of the world's fuel ethanol production is concentrated in the United States and Brazil. my country's fuel ethanol industry started late and has insufficient production capacity. In 2021, fuel ethanol production accounted for only about 3% of global production. Therefore, increasing fuel ethanol production is of great significance to ensuring my country's energy security.

[0003] In view of the resource characteristics of "rich in coal, poor in oil, and little gas" in my country, coal is used as the initial raw material, and synthesis gas is obtained through gasification and reforming. The synthesis gas is used to prepare methanol and dimethyl ether (DME) through copper-zinc catalysts, and DME and CO are used to synthesize methyl acetate (MA) through multiphase catalysis. MA is hydrogenated to ethanol, which can form a new process route for efficient and clean utilization of coal. This route does not involve water or very small amounts of water, and the separated product is directly anhydrous ethanol, which effectively reduces separation energy consumption and production costs. For this process route, the core difficulty lies in how to realize the synthesis of MA continuously, efficiently and greenly, and the key to realizing MA synthesis lies in how to promote the formation of CC bonds by catalyzing the carbonylation of DME. Among them, the octahedral molecular sieve catalyst is considered to be the most promising catalytic system.

[0004] Iglesia et al. first used MOR molecular sieves for dimethyl ether carbonylation and proposed that the unique eight-membered ring channels of MOR may be the main reason for its high activity; Corma et al. further confirmed the shape-selective effect of the eight-membered ring channels in MOR molecular sieves through theoretical calculations, but also confirmed that the twelve-membered ring channels inside the MOR molecular sieves are very conducive to the formation of hydrocarbon macromolecules. The rapid carbon deposition during the reaction leads to its extremely low catalytic life, which greatly restricts the industrial application of MOR catalysts. To this end, in addition to properly regulating MOR, researchers gradually developed molecular sieve systems containing eight-membered ring channels that can be used for carbonylation while avoiding strong side reactions. Among them, Shen Wenjie et al. from Dalian Institute of Chemical Physics found that SUZ-4 molecular sieves composed of ten-membered rings and eight-membered ring channels can partially inhibit the formation of aromatic compounds, the precursor of carbon deposition, and thus show excellent catalytic stability, but its disadvantage is that the catalytic activity is much lower than that of MOR molecular sieves. In summary, there are different defects in the eight-membered ring molecular sieve catalysts used in the dimethyl ether carbonylation reaction, and there are many limitations in industrial application. It is still necessary to further develop high-performance molecular sieve catalyst systems. Summary of the invention

[0005] In view of the problem that the conventional H-SUZ-4 catalyst has high stability and selectivity but low conversion rate in the dimethyl ether carbonylation reaction, the present invention provides a heteroatom molecular sieve M-HSUZ-4 catalyst and a preparation method and application thereof, and it is expected that the DME conversion rate can be effectively improved while maintaining its catalytic stability.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing a heteroatom molecular sieve M-HSUZ-4 catalyst comprises the following steps:

[0008] Step 1, adding an alkali source and an aluminum source into deionized water in sequence, heating the water until the water is completely dissolved and then cooling the water to room temperature to obtain a transparent solution 1;

[0009] Step 2, slowly adding the directing agent and the silicon source into deionized water in sequence and continuously stirring to obtain a mixed colloidal solution 2;

[0010] Step 3, slowly adding the mixed colloidal solution 2 into the transparent solution 1, continuously stirring and aging to obtain a mixed gel, transferring it into a hydrothermal kettle, dynamically crystallizing it in a homogeneous reactor, and obtaining a K-SUZ-4 molecular sieve after washing, drying and calcining;

[0011] Step 4, exchanging, washing, drying and calcining the K-SUZ-4 molecular sieve with an ammonium salt solution to obtain the HSUZ-4 molecular sieve;

[0012] Step 5, take a metal salt solution to exchange, wash and dry the HSUZ-4 molecular sieve to obtain the heteroatom molecular sieve M-HSUZ-4. In this step, calcination cannot be performed, as calcination will cause metal agglomeration or shedding after metal exchange, and after multiple experiments, the results show that the catalytic effect is greatly reduced after calcination.

[0013] Furthermore, the aluminum source is one of aluminum powder, aluminum hydroxide, and aluminum isopropoxide, or a mixture of two or more in any proportion; the alkali source is potassium hydroxide; the directing agent is tetraethylammonium hydroxide, i.e., 25% TEAOH; and the silicon source is one of silica sol and white carbon black, or a mixture of two or more in any proportion.

[0014] Furthermore, the raw materials for preparing the heteroatom molecular sieve M-HSUZ-4 include metal salt, aluminum source, silicon source, alkali source, directing agent, and deionized water. The molar ratio of the raw materials in the heteroatom molecular sieve M-HSUZ-4 is: M:Al2O3:SiO2:KOH:TEAOH:H2O=(0.15~0.25):1:(18~24):(6~13):(2~3):(400~600).

[0015] Furthermore, the molecular sieve preparation process requires that solution 2 be dripped into solution 1 drop by drop, and stirring is continued until the gel is sufficiently uniform, and then dynamically crystallized in a homogeneous reactor, and K-type SUZ-4 raw powder is obtained by washing, drying and calcining; after the colloidal solution 2 is dripped into solution 1 to form a mixed gel, the molar ratio of the raw material composition is Al2O3:SiO2:KOH:TEAOH:H2O=1:(20~24):(8~11):(2~3):(400~600).

[0016] Furthermore, the heating temperature in step 1 is 150-180°C and the duration is 2-3 hours; the crystallization temperature of dynamic crystallization in step 3 is 160-180°C and the crystallization time is 2-5 days; the drying temperature in step 3 is 100-120°C and the drying time is 4-8 hours; the calcination temperature in step 3 is 550-600°C and the calcination time is 6-8 hours; the rotation speed used for washing in step 3 is 15-20rpm.

[0017] Furthermore, the concentration of the ammonium salt solution in step 4 is 0.8-1.2 mol / L; the ratio of K-SUZ-4 to the ammonium salt solution in step 4 is 1 g:50 mL; during the exchange process in step 4, the exchange temperature is 120-150° C., the exchange times are 2 times, and each exchange time is 4 hours; the drying temperature is 100-120° C., and the drying time is 4-8 hours; the roasting temperature is 550-600° C., and the roasting time is 6-8 hours.

[0018] Furthermore, the concentration of the metal salt solution in step 5 is 0.01 mol / L to 0.025 mol / L; during the exchange process in step 5, the ratio of H-SUZ-4 to the metal salt solution is 1 g:50 mL, the exchange temperature is 120 to 150° C., the exchange times are 2 times, and each exchange time is 4 hours; the drying temperature is 100 to 120° C., and the drying time is 4 to 8 hours.

[0019] Furthermore, the metal in the metal salt solution in step 5 includes Zr, Ti, Zn, Co, Ga, In, Ge, Sn, La, and Ce; the salt solution corresponding to the metal in the metal salt solution is one of nitrate, sulfate, and hydrochloride; the composition ratio of metal to molecular sieve in the metal salt solution is: M:Al2O3:SiO2:KOH:TEAOH:H2O=(0.15~0.25):1:(20~24):(8~11):(2~3):(400~600).

[0020] A heteroatom molecular sieve M-HSUZ-4 catalyst prepared by the above preparation method.

[0021] A heteroatom molecular sieve M-HSUZ-4 catalyst prepared by the preparation method is used for synthesizing methyl acetate.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] The present invention introduces metal atoms on the basis of HSUZ-4 molecular sieve to construct heteroatom molecular sieve M-HSUZ-4, which can simultaneously increase B acid and L acid constructed around the metal, effectively improve the catalytic dimethyl ether carbonylation performance, and can increase the dimethyl ether carbonylation conversion rate from 15.16% to 29.98%, and the methyl acetate selectivity from 92.96% to 94.9%; the preparation process is simple, the raw material price is low, the catalyst has good stability, is easy to regenerate, and has broad prospects for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of dimethyl ether carbonylation conversion rate and methyl acetate selectivity of heteroatom molecular sieve M-HSUZ-4. DETAILED DESCRIPTION

[0025] Example 1

[0026] Step 1, weigh 1.92 g KOH and 0.835 g Al(OH)3, add 10 g of each into deionized water, heat to 150°C and dissolve for 5 h until completely dissolved, then take out and cool to room temperature to obtain a transparent solution 1;

[0027] Step 2: add 5.72 g of 25% tetraethylammonium hydroxide solution and 12 g of JN-40 (40% SiO2) silica sol to 12 g of water in sequence, and continue stirring for 2 hours to obtain colloidal solution 2.

[0028] Step 3, add the colloidal solution 2 drop by drop into the transparent solution 1 to form a white gel, keep stirring vigorously, and continue aging for 2 hours to form a mixed gel (the molar composition of the mixed gel is: Al2O3:SiO2:KOH:TEAOH:H2O=1:22:8:2.68:514), then transfer to a 100mL polytetrafluoroethylene reactor, rotate dynamically at a speed of 15r / min, and crystallize at 170°C for 2 days. The obtained sample is washed with deionized water to neutrality, dried at 100°C for 8h, and calcined at 600°C for 6h to obtain K-SUZ-4 molecular sieve.

[0029] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 250mL 1mol / L ammonium nitrate solution for exchange, exchange twice continuously, the exchange temperature is 120°C, and the exchange time is 4h each time. After the exchange, wash, dry at 120°C for 6h, and calcine at 560°C for 6h to obtain H-SUZ-4.

[0030] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150mL 0.01mol / L Zr(NO3)4 solution for exchange, exchange twice continuously, the exchange temperature is 120℃, and the exchange time is 4h each time. After the exchange, wash and dry at 110℃ for 6h to obtain Zr-HSUZ-4.

[0031] The H-SUZ-4 and Zr-HSUZ-4 molecular sieve samples were granulated to obtain 40-60 mesh samples, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. 0.3 g of the sample was weighed and loaded into a stainless steel reaction tube with an inner diameter of 8 mm, and pretreated with hydrogen at 300°C for 2 hours, then the hydrogen was stopped, the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He) was opened, the reaction pressure was increased to 2MPa, the reaction temperature was controlled to 220°C, and the reaction space velocity GHSV was controlled to be 1200h -1 The reaction evaluation time was 36 hours, during which samples were automatically taken every hour for analysis. When H-SUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 15.16%, and the MA selectivity was 92.96%; when Zr-HSUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 29.98%, and the MA selectivity was 94.9%.

[0032] Example 2

[0033] Step 1: weigh 1.92 g KOH, 1.48 g aluminum isopropoxide (C9H 21AlO3) was added in 10 g into deionized water, heated to 170°C and dissolved for 2 h until completely dissolved, then taken out and cooled to room temperature to obtain a transparent solution 1;

[0034] Step 2: add 5.72 g of 25% tetraethylammonium hydroxide solution and 12 g of JN-40 (40% SiO2) silica sol to 12 g of water in sequence, and continue stirring for 1 hour to obtain colloidal solution 2.

[0035] Step 3, add the colloidal solution 2 drop by drop into the transparent solution 1 to form a white gel, keep stirring vigorously, and continue aging for 2 hours to form a mixed gel (the molar composition of the mixed gel is: Al2O3:SiO2:KOH:TEAOH:H2O=1:22:8:2.68:514), then transfer to a 100mL polytetrafluoroethylene reactor, rotate dynamically at a speed of 15r / min, and crystallize at 160°C for 4 days. The obtained sample is washed with deionized water to neutrality, dried at 110°C for 6h, and calcined at 560°C for 7h to obtain K-SUZ-4 molecular sieve.

[0036] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 200mL 1mol / L ammonium chloride solution for exchange, exchange twice continuously, the exchange temperature is 140°C, and the exchange time is 4h each time. After the exchange, wash, dry at 110°C for 6h, and calcine at 570°C for 7h to obtain H-SUZ-4.

[0037] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150mL 0.01mol / L Ti(SO4)2 solution for exchange, exchange twice continuously, the exchange temperature is 120℃, and the exchange time is 4h each time. After the exchange, wash and dry at 100℃ for 10h to obtain Ti-HSUZ-4.

[0038] The H-SUZ-4 and Ti-HSUZ-4 molecular sieve samples were granulated to obtain 40-60 mesh samples, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. 0.3 g of the sample was weighed and loaded into a stainless steel reaction tube with an inner diameter of 8 mm, and pretreated with hydrogen at 300°C for 2 hours, then the hydrogen was stopped, the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He) was opened, the reaction pressure was increased to 2MPa, the reaction temperature was controlled to 220°C, and the reaction space velocity GHSV was controlled to be 1200h -1 The reaction evaluation time was 36 hours, during which samples were automatically taken every hour for analysis. When H-SUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 15.16%, and the MA selectivity was 92.96%; when Ti-HSUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 26.71%, and the MA selectivity was 93.92%.

[0039] Example 3

[0040] Step 1, weigh 2g KOH and 0.2g aluminum powder and add them to 10g deionized water in sequence, and a small amount of hydrogen is generated during the dissolution process, which is introduced into the room through a conduit until the aluminum powder is completely dissolved to obtain a transparent solution 1 (aluminum powder can be dissolved in KOH solution at room temperature without high temperature, and hydrogen is generated during the dissolution process and needs to be released);

[0041] Step 2: 5.72 g of 25% tetraethylammonium hydroxide solution and 4.8 g of white carbon black were added to 19.2 g of water in sequence, and the mixture was stirred for 2 h to obtain a colloidal solution 2.

[0042] Step 3, add the colloidal solution 2 drop by drop into the transparent solution 1 to form a white gel, keep stirring vigorously, and continue aging for 2 hours to form a mixed gel (the molar composition of the mixed gel is: Al2O3:SiO2:KOH:TEAOH:H2O=1:22:8:2.68:514), then transfer to a 100mL polytetrafluoroethylene reactor, rotate dynamically at a speed of 15r / min, and crystallize at 180°C for 2 days. The obtained sample is washed with deionized water to neutrality, dried at 100°C for 8h, and calcined at 600°C for 6h to obtain K-SUZ-4 molecular sieve.

[0043] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 150mL 1mol / L ammonium nitrate solution for exchange, exchange twice continuously, the exchange temperature is 150°C, and the exchange time is 4h each time. After the exchange, wash, dry at 120°C for 6h, and calcine at 600°C for 7h to obtain H-SUZ-4.

[0044] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150mL 0.01mol / L Zn(NO3)2 solution for exchange, exchange twice continuously, the exchange temperature is 110℃, and the exchange time is 4h each time. After the exchange, wash and dry at 120℃ for 6h to obtain Zn-HSUZ-4.

[0045] The H-SUZ-4 and Zn-HSUZ-4 molecular sieve samples were granulated to obtain samples of 40-60 mesh, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. 0.3 g of the sample was weighed and loaded into a stainless steel reaction tube with an inner diameter of 8 mm, and pretreated with hydrogen at 300°C for 2 hours, then the hydrogen was stopped, the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He) was opened, the reaction pressure was increased to 2MPa, the reaction temperature was controlled to 220°C, and the reaction space velocity GHSV was controlled to be 1200h -1The reaction evaluation time was 36 hours, during which samples were automatically taken every hour for analysis. When H-SUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 15.16% and the MA selectivity was 92.96%; when Zn-HSUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 19.07% and the MA selectivity was 95.5%.

[0046] Example 4

[0047] Step 1: weigh 2.4 g KOH, 0.74 g aluminum isopropoxide (C9H 21 AlO3) and 0.427gAl(OH)3 were added in 10g in turn into deionized water, heated to 160℃ and dissolved for 3h until completely dissolved, then taken out and cooled to room temperature to obtain a transparent solution 1;

[0048] Step 2: add 5.72 g of 25% tetraethylammonium hydroxide solution and 12 g of JN-40 (40% SiO2) silica sol to 17.6 g of water in sequence, and continue stirring for 1 hour to obtain colloidal solution 2.

[0049] Step 3, add the colloidal solution 2 drop by drop into the transparent solution 1 to form a white gel, keep stirring vigorously, and continue aging for 2 hours to form a mixed gel (the molar composition of the mixed gel is: Al2O3: SiO2: KOH: TEAOH: H2O = 1: 22: 10: 2.68: 600), then transfer to a 100mL polytetrafluoroethylene reactor, rotate dynamically at a speed of 15r / min, and crystallize at 160°C for 4 days. The obtained sample is washed with deionized water to neutrality, dried at 120°C for 4 hours, and calcined at 560°C for 8 hours to obtain K-SUZ-4 molecular sieve.

[0050] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 250mL 1mol / L ammonium nitrate solution for exchange, exchange twice continuously, the exchange temperature is 150°C, and the exchange time is 4h each time. After the exchange, wash, dry at 100°C for 6h, and calcine at 580°C for 7h to obtain H-SUZ-4.

[0051] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150:mL 0.01:mol / L Co(NO3)2 solution for exchange, exchange twice continuously, the exchange temperature is 110°C, and the exchange time is 4h each time. After the exchange, wash and dry at 100°C for 6h to obtain Co-HSUZ-4.

[0052] The H-SUZ-4 and Co-HSUZ-4 molecular sieve samples were granulated to obtain samples of 40-60 mesh, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. 0.3 g of the sample was weighed and loaded into a stainless steel reaction tube with an inner diameter of 8 mm, and pretreated with hydrogen at 300°C for 2 hours, then the hydrogen was stopped, the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He) was opened, the reaction pressure was increased to 2MPa, the reaction temperature was controlled to 220°C, and the reaction space velocity GHSV was controlled to be 1200h -1 The reaction evaluation time was 36 hours, during which samples were automatically taken every hour for analysis. When H-SUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 15.16% and the MA selectivity was 92.96%; when Co-HSUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 16.72% and the MA selectivity was 92.99%.

[0053] Example 5

[0054] Step 1, weigh 2.16 g KOH and 2.42 g aluminum sulfate 18hydrate (Al2(SO4)3·18H2O), add 10 g of each into deionized water, heat to 180°C and dissolve for 3 h until completely dissolved, take out and cool to room temperature to obtain a transparent solution 1;

[0055] Step 2: add 5.72 g of 25% tetraethylammonium hydroxide solution and 12 g of JN-40 (40% SiO2) silica sol to 12 g of water in sequence, and continue stirring for 3 hours to obtain colloidal solution 2.

[0056] Step 3, add the colloidal solution 2 drop by drop into the transparent solution 1 to form a white gel, keep stirring vigorously, and continue aging for 2 hours to form a mixed gel (the molar composition of the mixed gel is: Al2O3:SiO2:KOH:TEAOH:H2O=1:22:9:2.68:534), then transfer to a 100mL polytetrafluoroethylene reactor, rotate dynamically at a speed of 15r / min, and crystallize at 170°C for 3 days. The obtained sample is washed with deionized water to neutrality, dried at 120°C for 7h, and calcined at 570°C for 8h to obtain K-SUZ-4 molecular sieve.

[0057] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 200mL 1.5mol / L ammonium nitrate solution for exchange, exchange twice continuously, the exchange temperature is 140°C, and the exchange time is 4h each time. After the exchange, wash, dry at 120°C for 6h, and calcine at 560°C for 8h to obtain H-SUZ-4.

[0058] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150mL 0.03mol / L Ga(NO3)3 solution for exchange, exchange twice continuously, the exchange temperature is 140℃, and the exchange time is 4h each time. After the exchange, wash and dry at 120℃ for 6h to obtain Ga-HSUZ-4.

[0059] The H-SUZ-4 and Ga-HSUZ-4 molecular sieve samples were granulated to obtain samples of 40-60 mesh, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. 0.3 g of the sample was weighed and loaded into a stainless steel reaction tube with an inner diameter of 8 mm, and pretreated with hydrogen at 300°C for 2 hours, then the hydrogen was stopped, the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He) was opened, the reaction pressure was increased to 2MPa, the reaction temperature was controlled to 220°C, and the reaction space velocity GHSV was controlled to be 1200h -1 The reaction evaluation time was 36 hours, during which samples were automatically taken every hour for analysis. When H-SUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 15.16%, and the MA selectivity was 92.96%; when Ga-HSUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 20.36%, and the MA selectivity was 93.21%.

[0060] Example 6

[0061] Step 1: weigh 2.16 g KOH, 1.48 g aluminum isopropoxide (C9H 21 AlO3) was added in 10 g into deionized water, heated to 180°C and dissolved for 2 h until completely dissolved, then taken out and cooled to room temperature to obtain a transparent solution 1;

[0062] Step 2: add 5.72 g of 25% tetraethylammonium hydroxide solution and 12 g of JN-40 (40% SiO2) silica sol to 17.6 g of water in sequence, and continue stirring for 1 hour to obtain colloidal solution 2.

[0063] Step 3, add the colloidal solution 2 drop by drop into the transparent solution 1 to form a white gel, keep stirring vigorously, and continue aging for 2 hours to form a mixed gel (the molar composition of the mixed gel is: Al2O3:SiO2:KOH:TEAOH:H2O=1:22:9:2.68:600), then transfer to a 100mL polytetrafluoroethylene reactor, rotate dynamically at a speed of 15r / min, and crystallize at 190°C for 2 days. The obtained sample is washed with deionized water to neutrality, dried at 110°C for 10 hours, and calcined at 560°C for 7 hours to obtain K-SUZ-4 molecular sieve.

[0064] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 250mL 1mol / L ammonium chloride solution for exchange, exchange twice continuously, the exchange temperature is 130°C, and the exchange time is 4h each time. After the exchange, wash, dry at 110°C for 10h, and calcine at 560°C for 7h to obtain H-SUZ-4.

[0065] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150mL 0.005mol / L In(NO3)3 solution for exchange, exchange twice continuously, the exchange temperature is 130℃, and the exchange time is 4h each time. After the exchange, wash and dry at 110℃ for 10h to obtain In-HSUZ-4.

[0066] The H-SUZ-4 and In-HSUZ-4 molecular sieve samples were granulated to obtain 40-60 mesh samples, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. Weigh 0.3 g of the sample into a stainless steel reaction tube with an inner diameter of 8 mm, and pre-treat it with hydrogen at 300°C for 2 hours, then stop introducing hydrogen, open the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He), increase the pressure to 2MPa, control the reaction temperature to 220°C, and control the reaction space velocity GHSV to 1200h -1 The reaction evaluation time was 36 hours, during which samples were automatically taken every hour for analysis. When H-SUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 15.16%, and the MA selectivity was 92.96%; when In-HSUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 18.29%, and the MA selectivity was 92.98%.

[0067] Example 7

[0068] Step 1, weigh 2g KOH and 0.2g aluminum powder and add them to 10g deionized water in sequence, and a small amount of hydrogen is generated during the dissolution process, which is introduced into the room through a conduit until the aluminum powder is completely dissolved to obtain a clear solution 1 (aluminum powder can be dissolved in KOH solution at room temperature without high temperature, and hydrogen is generated during the dissolution process and needs to be released);

[0069] Step 2: add 5.72 g of 25% tetraethylammonium hydroxide solution and 10.9 g of JN-40 (40% SiO2) silica sol to 12 g of water in sequence, and continue stirring for 1 hour to obtain colloidal solution 2.

[0070] Step 3, add the colloidal solution 2 drop by drop into the transparent solution 1 to form a white gel, keep stirring vigorously, and continue aging for 2 hours to form a mixed gel (the molar composition of the mixed gel is: Al2O3:SiO2:KOH:TEAOH:H2O=1:20:11:2.68:514), then transfer to a 100mL polytetrafluoroethylene reactor, rotate dynamically at a speed of 15r / min, and crystallize at 170°C for 2 days. The obtained sample is washed with deionized water to neutrality, dried at 110°C for 6 hours, and calcined at 580°C for 6 hours to obtain K-SUZ-4 molecular sieve.

[0071] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 200mL 1mol / L ammonium chloride solution for exchange, exchange twice continuously, the exchange temperature is 130°C, and the exchange time is 4h each time. After the exchange, wash, dry at 110°C for 6h, and calcine at 580°C for 6h to obtain H-SUZ-4.

[0072] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150mL 0.01mol / L GeCl4 solution for exchange, exchange twice continuously, the exchange temperature is 130℃, and the exchange time is 4h each time. After the exchange, wash and dry at 110℃ for 6h to obtain Ge-HSUZ-4.

[0073] The H-SUZ-4 and Ge-HSUZ-4 molecular sieve samples were granulated to obtain samples of 40-60 mesh, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. 0.3 g of the sample was weighed and loaded into a stainless steel reaction tube with an inner diameter of 8 mm, and pretreated with hydrogen at 300°C for 2 hours, then the hydrogen was stopped, the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He) was opened, the reaction pressure was increased to 2MPa, the reaction temperature was controlled to 220°C, and the reaction space velocity GHSV was controlled to be 1200h -1 The reaction evaluation time was 36 hours, during which samples were automatically taken every hour for analysis. When H-SUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 15.16%, and the MA selectivity was 92.96%; when Ge-HSUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 23.94%, and the MA selectivity was 93.32%.

[0074] Example 8

[0075] Step 1: weigh 2.4 g KOH, 1.48 g aluminum isopropoxide (C9H 21 AlO3) was added in 10 g into deionized water, heated to 160°C and dissolved for 3 h until completely dissolved, then taken out and cooled to room temperature to obtain a transparent solution 1;

[0076] Step 2: add 5.72 g of 25% tetraethylammonium hydroxide solution and 13 g of JN-40 (40% SiO2) silica sol to 17.6 g of water in sequence, and continue stirring for 2 hours to obtain colloidal solution 2.

[0077] Step 3, add the colloidal solution 2 drop by drop into the transparent solution 1 to form a white gel, keep stirring vigorously, and continue aging for 2 hours to form a mixed gel (the molar composition of the mixed gel is: Al2O3:SiO2:KOH:TEAOH:H2O=1:24:10:2.68:600), then transfer to a 100mL polytetrafluoroethylene reactor, rotate dynamically at a speed of 15r / min, and crystallize at 170°C for 2 days. The obtained sample is washed with deionized water to neutrality, dried at 110°C for 8 hours, and calcined at 600°C for 8 hours to obtain K-SUZ-4 molecular sieve.

[0078] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 150mL 1mol / L ammonium nitrate solution for exchange, exchange twice continuously, the exchange temperature is 150°C, and the exchange time is 4h each time. After the exchange, wash, dry at 110°C for 8h, and calcine at 600°C for 8h to obtain H-SUZ-4.

[0079] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150mL 0.01mol / L Sn(NO3)4 solution for exchange, exchange twice continuously, the exchange temperature is 150℃, and the exchange time is 4h each time. After the exchange, wash and dry at 110℃ for 8h to obtain Sn-HSUZ-4.

[0080] The H-SUZ-4 and Sn-HSUZ-4 molecular sieve samples were granulated to obtain 40-60 mesh samples, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. 0.3 g of the sample was weighed and loaded into a stainless steel reaction tube with an inner diameter of 8 mm, and pretreated with hydrogen at 300°C for 2 hours, then the hydrogen was stopped, the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He) was opened, the reaction pressure was increased to 2MPa, the reaction temperature was controlled to 220°C, and the reaction space velocity GHSV was controlled to 1200h -1 The reaction evaluation time was 36 hours, during which samples were automatically taken every hour for analysis. When H-SUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 15.16%, and the MA selectivity was 92.96%; when Sn-HSUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 16.96%, and the MA selectivity was 96.01%.

[0081] Example 9

[0082] Step 1: weigh 1.92 g KOH, 0.417 g Al(OH)3 and 0.74 g aluminum isopropoxide (C9H 21 AlO3) was added in 10 g portions into deionized water, heated to 170°C and dissolved for 2 h until completely dissolved, then taken out and cooled to room temperature to obtain a transparent solution 1;

[0083] Step 2: add 5.72 g of 25% tetraethylammonium hydroxide solution and 12 g of JN-40 (40% SiO2) silica sol to 4.6 g of water in sequence, and continue stirring for 2 hours to obtain colloidal solution 2.

[0084] Step 3, add the colloidal solution 2 drop by drop into the transparent solution 1 to form a white gel, keep stirring vigorously, and continue aging for 2 hours to form a mixed gel (the molar composition of the mixed gel is: Al2O3:SiO2:KOH:TEAOH:H2O=1:22:8:2.68:400), then transfer to a 100mL polytetrafluoroethylene reactor, rotate dynamically at a speed of 15r / min, and crystallize at 190°C for 3 days. The obtained sample is washed with deionized water to neutrality, dried at 120°C for 8h, and calcined at 600°C for 7h to obtain K-SUZ-4 molecular sieve.

[0085] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 200mL 1.5mol / L ammonium nitrate solution for exchange, exchange twice continuously, the exchange temperature is 150°C, and the exchange time is 4h each time. After the exchange, wash, dry at 120°C for 8h, and calcine at 600°C for 7h to obtain H-SUZ-4.

[0086] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150mL 0.02mol / L La(NO3)3 solution for exchange, exchange twice continuously, the exchange temperature is 150℃, and the exchange time is 4h each time. After the exchange, wash and dry at 120℃ for 8h to obtain La-HSUZ-4.

[0087] The H-SUZ-4 and La-HSUZ-4 molecular sieve samples were granulated to obtain samples of 40-60 mesh, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. 0.3 g of the sample was weighed and loaded into a stainless steel reaction tube with an inner diameter of 8 mm, and pretreated with hydrogen at 300°C for 2 hours, then the hydrogen was stopped, the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He) was opened, the reaction pressure was increased to 2MPa, the reaction temperature was controlled to 220°C, and the reaction space velocity GHSV was controlled to be 1200h -1The reaction evaluation time was 36 hours, during which samples were automatically taken every hour for analysis. When H-SUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 15.16%, and the MA selectivity was 92.96%; when La-HSUZ-4 molecular sieve was used as the catalyst, the DME conversion rate was 22.74%, and the MA selectivity was 93.12%.

[0088] Example 10

[0089] Step 1, weigh 1.92 g KOH and 0.835 g Al(OH)3, add 10 g of each into deionized water, heat to 170°C and dissolve for 1 hour until completely dissolved, take out and cool to room temperature to obtain a transparent solution 1;

[0090] Step 2: add 5.72 g of 25% tetraethylammonium hydroxide solution and 12 g of JN-40 (40% SiO2) silica sol to 12 g of water in sequence, and continue stirring for 2 hours to obtain colloidal solution 2.

[0091] Step 3, drip gel solution 2 into transparent solution 1 drop by drop to form white gel, keep vigorous stirring, continue aging for 2h to form mixed gel (molar composition of mixed gel is: Al2O3:SiO2:KOH:TEAOH:H2O=1:22:8:2.68:514), then transfer to 100mL polytetrafluoroethylene reactor, rotate dynamically at 15r / min, crystallize at 180℃ for 2 days. The obtained sample is washed with deionized water to neutrality, dried at 110℃ for 6h, and calcined at 560℃ for 6h to obtain K-SUZ-4 molecular sieve.

[0092] Step 4, take 5g K-SUZ-4 molecular sieve and add it to 250mL 1mol / L ammonium nitrate solution for exchange, exchange twice continuously, the exchange temperature is 140°C, and the exchange time is 4h each time. After the exchange, wash, dry at 110°C for 6h, and calcine at 560°C for 6h to obtain H-SUZ-4.

[0093] Step 5, take 3g H-SUZ-4 molecular sieve and add it to 150mL 0.01mol / L Ce(NO3)3 solution for exchange, exchange twice continuously, the exchange temperature is 140℃, and the exchange time is 4h each time. After the exchange, wash and dry at 110℃ for 6h to obtain Ce-HSUZ-4.

[0094] The H-SUZ-4 and Ce-HSUZ-4 molecular sieve samples were granulated to obtain 40-60 mesh samples, and their dimethyl ether carbonylation performance was tested in a fixed bed reactor. 0.3 g of the sample was weighed and loaded into a stainless steel reaction tube with an inner diameter of 8 mm, and pretreated with hydrogen at 300°C for 2 hours, then the hydrogen was stopped, the raw gas (ratio of 3% DME: 47% CO: 2.5% Ar: 47.5% He) was opened, the reaction pressure was increased to 2MPa, the reaction temperature was controlled to 220°C, and the reaction space velocity GHSV was controlled to be 1200h -1 The reaction evaluation time was 36 h, during which samples were automatically taken and analyzed every hour.

[0095] The Koch mechanism is followed in the carbonylation reaction of dimethyl ether. The B acid site is its main active site. Increasing and enhancing the B acid site helps to enhance its activity. At the same time, the CO insertion process is the rate-determining step of the reaction. If an effective L acid site can be introduced for adsorbing CO without reducing the B acid site, the energy barrier for inserting CO can be reduced, which also helps to improve its catalytic activity. Based on the basic understanding of the current technological progress and reaction mechanism, the present invention has conducted extensive and in-depth research on molecular sieve catalysts in the process of carbonylation of dimethyl ether to methyl acetate. It is found that by constructing a metal (M)-HSUZ-4 type molecular sieve, the B acid site can be increased and enhanced, and the L acid site for enhancing CO adsorption can be provided. While maintaining its catalytic stability, the DME conversion rate can be effectively improved. When the H-SUZ-4 molecular sieve is used as a catalyst, the DME conversion rate is 15.16% and the MA selectivity is 92.96%; when the Ce-HSUZ-4 molecular sieve is used as a catalyst, the DME conversion rate is 17.54% and the MA selectivity is 93.67%.

[0096] Table 1

[0097]

[0098] Evaluation conditions: 220, 2MPa, GHSV = 1200h -1

[0099] It can be seen from Table 1 that the present invention effectively improves the catalytic performance of dimethyl ether carbonylation on HSUZ-4 molecular sieve, and can increase the dimethyl ether carbonylation conversion rate from 15.16% to 29.98%, and the methyl acetate selectivity from 92.96% to 94.9%;

[0100] The method of the present invention has cheap synthetic raw materials, simple process and easy preparation; the catalyst has high stability and can maintain high selectivity for methyl acetate after continuous catalysis for 100 hours; the catalyst will be deactivated due to long reaction time, which is mainly caused by macromolecular carbon deposition, and the activity of the catalyst can be restored by simple calcination.

[0101] The contents not described in detail in the specification of the present invention belong to the prior art known to the professional and technical personnel in the field. Although the illustrative specific embodiments of the present invention are described above to facilitate the understanding of the present invention by the technical personnel in the field, it should be clear that the present invention is not limited to the scope of the specific embodiments. For the ordinary technical personnel in the field, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.

Claims

1. An application of a heteroatom molecular sieve M-HSUZ-4 catalyst, characterized in that: The catalyst is used for catalyzing the carbonylation of dimethyl ether to synthesize methyl acetate. The preparation method of the catalyst comprises the following steps: Step 1, adding an alkali source and an aluminum source into deionized water in sequence, heating the water until the water is completely dissolved and then cooling the water to room temperature to obtain a transparent solution 1; Step 2, slowly adding the directing agent and the silicon source into deionized water in sequence and continuously stirring to obtain a colloidal solution 2; Step 3, slowly adding the mixed colloidal solution 2 into the transparent solution 1, continuously stirring and aging to obtain a mixed gel, transferring it into a hydrothermal kettle, dynamically crystallizing it in a homogeneous reactor, and obtaining a K-SUZ-4 molecular sieve after washing, drying and calcining; Step 4, exchanging, washing, drying and calcining the K-SUZ-4 molecular sieve with an ammonium salt solution to obtain the H-SUZ-4 molecular sieve; Step 5, taking a metal salt solution to exchange, wash, and dry the H-SUZ-4 molecular sieve to obtain a heteroatom molecular sieve M-SUZ-4; The concentration of the metal salt solution in step 5 is 0.01 mol / L to 0.025 mol / L; in the exchange process of step 5, the ratio of H-SUZ-4 to the metal salt solution is 1 g: 50 mL, the exchange temperature is 120-150°C, the exchange times are 2 times, and each exchange time is 4 h; the drying temperature is 100-120°C, and the drying time is 4-8 h; The metal in the metal salt solution in step 5 is Zr, Ti, Zn, Co, Ga, In, Ge, Sn, La or Ce.

2. The use of a heteroatom molecular sieve M-HSUZ-4 catalyst according to claim 1, characterized in that: The aluminum source is one of aluminum powder, aluminum hydroxide, and aluminum isopropoxide, or a mixture of two or more thereof in any proportion; the alkali source is potassium hydroxide; the directing agent is 25% TEAOH; and the silicon source is one of silica sol and white carbon black, or a mixture of two or more thereof in any proportion.

3. The use of a heteroatom molecular sieve M-HSUZ-4 catalyst according to claim 2, characterized in that: The raw materials for preparing the heteroatom molecular sieve M-HSUZ-4 include metal salt, aluminum source, silicon source, alkali source, directing agent and deionized water. The molar ratio of the raw materials in the heteroatom molecular sieve M-HSUZ-4 is: M: Al2O3: SiO2: KOH: TEAOH: H2O=(0.15~0.25): 1: (18~24): (6~13): (2~3): (400~600).

4. The use of a heteroatom molecular sieve M-HSUZ-4 catalyst according to claim 2, characterized in that: The molecular sieve preparation process requires dripping solution 2 into solution 1 drop by drop, continuously stirring until the gel is sufficiently uniform, dynamically crystallizing in a homogeneous reactor, and washing, drying, and calcining to obtain K-type SUZ-4 raw powder; after the colloidal solution 2 is dripped into solution 1 to form a mixed gel, the molar ratio of the raw material composition is Al2O3: SiO2: KOH: TEAOH: H2O=1: (20~24): (8~11): (2~3): (400~600).

5. The use of a heteroatom molecular sieve M-HSUZ-4 catalyst according to claim 1, characterized in that: The heating temperature in step 1 is 150-180°C and the duration is 2-3 hours; the crystallization temperature of dynamic crystallization in step 3 is 160-180°C and the crystallization time is 2-5 days; the drying temperature in step 3 is 100-120°C and the drying time is 4-8 hours; the calcination temperature in step 3 is 550-600°C and the calcination time is 6-8 hours; the speed used for washing in step 3 is 15-20 rpm.

6. The use of a heteroatom molecular sieve M-HSUZ-4 catalyst according to claim 1, characterized in that: The concentration of the ammonium salt solution in step 4 is 0.8-1.2 mol / L; the ratio of K-SUZ-4 to the ammonium salt solution in step 4 is 1 g:50 mL; during the exchange process in step 4, the exchange temperature is 120-150°C, the exchange times are 2 times, and each exchange time is 4 hours; the drying temperature is 100-120°C, and the drying time is 4-8 hours; the roasting temperature is 550-600°C, and the roasting time is 6-8 hours.

7. The use of a heteroatom molecular sieve M-HSUZ-4 catalyst according to claim 2, characterized in that: In the step 5, the salt solution corresponding to the metal in the metal salt solution is one of nitrate, sulfate and hydrochloride; the composition ratio of metal to molecular sieve in the metal salt solution is: M: Al2O3: SiO2: KOH: TEAOH: H2O=(0.15~0.25):1: (20~24): (8~11): (2~3): (400~600).