A Bi2S3 / VS2 / S composite material and its preparation method and application

Bi2S3/VS2/S composite materials were prepared by heat treatment of Bi(NO3)3·5H2O and NH4VO3 and sulfur powder, which solved the problems of low VS2 capacity and poor stability of Bi2S3 in magnesium ion batteries, and achieved long-term stable cycle of magnesium ion batteries and high electrochemical properties.

CN116282147BActive Publication Date: 2024-11-22SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310105866.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-13
Publication Date
2024-11-22
Estimated Expiration
2043-02-13

AI Technical Summary

Technical Problem

The theoretical capacity of VS2 in magnesium ion batteries is low and the structural stability of Bi2S3 is poor, resulting in repeated embedding and detachment of magnesium ions, and the long-term stable circulation cannot be achieved.

Method used

Using Bi(NO3)3·5H2O and NH4VO3 as raw materials, powder E is prepared by solvothermal method, and Bi2S3/VS2/S composite material is formed with sulfur powder in heat treatment to construct an interwoven composite structure of sheet-like and nanorod-like structure , enhance the stability of the material and magnesium storage properties.

Benefits of technology

It improves the electrochemical performance of magnesium ion batteries, realizes long-term and stable circulation of magnesium ions, reduces production costs and energy consumption, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116282147B_ABST
    Figure CN116282147B_ABST
Patent Text Reader

Abstract

The invention discloses a Bi2S3 / VS2 / S composite material and a preparation method and application thereof, belonging to the technical field of energy storage material preparation, using Bi(NO3)3·5H2O and NH4VO3 as raw materials, adopting a simple solvent thermal method to prepare Bi2S3 / VS2, further growing sulfur in situ on the surface of Bi2S3 / VS2 by a heat treatment method, preparing a Bi2S3 / VS2 / S composite material, wherein VS2 is a lamellar structure, and the lamellar structure is conducive to the interlayer deintercalation of magnesium ions, and Bi2S3, as a semiconductor material, has the advantage of high capacity, and by compounding the two materials, the physical and chemical properties of a single material can be adjusted, and the synergistic effect of different components can be exerted, and the strong interaction between the two components can also enhance the structural stability, improve the charge transfer kinetics of the material, and the sulfur can further lay the foundation for high capacity. The whole preparation method is simple, has high repeatability, short preparation cycle, low reaction temperature, reduces energy consumption and production cost, and is suitable for large-scale production and preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of energy storage material preparation, and specifically relates to a Bi2S3 / VS2 / S composite material and a preparation method and application thereof. Background Art

[0002] With the continuous development of my country's economy and science and technology, people's lives are getting better and better, and the demand for energy is also increasing. At present, the main energy used in the world is non-renewable fossil fuels. Due to the limited reserves of fossil energy on the earth and the fact that this fuel will inevitably release a large amount of harmful gases during combustion, it causes a serious environmental crisis. Therefore, the development of various green renewable energy sources, such as wind energy and solar energy, has become an effective means. However, these renewable energy sources are intermittent in nature, which makes the development of feasible energy storage devices crucial. As a kind of secondary battery, lithium-ion batteries have the advantages of high energy density, long cycle life, low self-discharge and high power density. They are now widely used in electric vehicles, consumer electronics, large-scale energy storage, aerospace and other aspects. However, due to the low abundance and uneven distribution of lithium elements in the earth's crust, the cost of lithium salts is high, which affects the supply and demand of lithium resources in the market, and it is difficult to meet the application of lithium-ion batteries in the field of large-scale energy storage. Therefore, finding new energy storage devices that can replace lithium-ion batteries has become a research hotspot in the battery field. Magnesium is an active metal. The content of magnesium in the earth's crust ranks fifth, with a density of 1.74 g / cm 3 , has good thermal conductivity and electrical conductivity. Magnesium has similar chemical properties to lithium. However, magnesium is not as active as lithium, easy to operate, safe, low price (1 / 24 of Li), pollution-free, and magnesium negative electrode does not produce dendrites. Mg 2+ / Mg has a relatively negative potential (–2.37 V vs. standard hydrogen electrode), and its theoretical volume energy density (3833 mA h / cm 3 ) is much higher than Li (2046 mA h / cm 3 ). Based on this, the development of low-cost, high-performance rechargeable magnesium-ion batteries is regarded as an important direction for the development of secondary energy storage technology. Therefore, conducting research on magnesium-ion batteries is of great significance to the sustainable development of future energy.

[0003] However, the research and development of magnesium ion batteries is still relatively slow at this stage, mainly because: 1) Magnesium divalent ions have a high charge density and a small ionic radius (0.072 nm), and a strong solvation effect, making it difficult to +1) It is easy to embed into the matrix, making the selection of positive electrode materials more difficult; 2) The embedding and extraction of magnesium ions will cause serious damage to the structure. Therefore, exploring and obtaining suitable electrode materials is the key to realizing high-performance practical magnesium-ion batteries in the future. Vanadium disulfide (VS2) is a typical layered transition metal sulfide with a layered structure similar to graphene. Its layers are bound by weak van der Waals forces, and different atoms are bound by covalent bonds. The interlayer spacing is large and the structure is stable. It has attracted everyone's attention in magnesium-ion batteries. Bismuth sulfide (Bi2S3) is an important semiconductor material with a band gap of 1.2~1.7e V and a unique layered structure. In recent years, it has been widely used in the fields of photothermal, photoelectric, and photocatalysis. The reaction of Bi2S3 material is divided into three steps, namely insertion reaction, conversion reaction, and alloy reaction. Therefore, compared with inactive metal sulfides that only have insertion reaction and conversion reaction, bismuth sulfide has a higher theoretical specific capacity (625 mAh g -1 ).

[0004] However, the theoretical capacity of VS2 is relatively low, which limits its wide application in practice. In addition, Bi2S3 has the advantages of low cost and high capacity, but its structural stability is poor. In the practical application of magnesium ion batteries, Mg 2+ Repeated insertion and removal will cause structural damage, making long-term stable circulation impossible. Summary of the invention

[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a Bi2S3 / VS2 / S composite material and its preparation method and application, so as to solve the problem of Mg in magnesium ion batteries caused by the low theoretical capacity of VS2 and the poor structural stability of Bi2S3. 2+ Repeated insertion and removal make it impossible to achieve long-term stable circulation.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention discloses a method for preparing a Bi2S3 / VS2 / S composite material, comprising the following steps:

[0008] 1) Dissolve Bi(NO3)3·5H2O and NH4VO3 in ethylene glycol solution, disperse them uniformly by ultrasonication, add anhydrous ethanol, stir them uniformly, carry out hydrothermal reaction, cool them to room temperature, wash them, and freeze-dry them to obtain powder E;

[0009] The mass ratio of Bi(NO3)3·5H2O to NH4VO3 is 1:(1-10);

[0010] 2) The powder E prepared in step 1) is fully mixed with sulfur powder, calcined under an inert atmosphere, and cooled to room temperature to obtain a Bi2S3 / VS2 / S composite material;

[0011] The mass ratio of the powder E to the sulfur powder is 1:(0.5~2).

[0012] Preferably, in step 1), the temperature of the hydrothermal reaction is 120-180° C., and the time of the hydrothermal reaction is 6-16 h.

[0013] Preferably, in step 2), the calcination temperature is 400-700°C, and the calcination time is 2 h.

[0014] Preferably, in step 1), the freeze-drying temperature is -30 to -40 °C, and the freeze-drying time is 8 to 12 h.

[0015] Preferably, in step 1), the ultrasonic dispersion time is 15 to 60 min.

[0016] Preferably, in step 1), the stirring time is 15-50 min, and the stirring speed is 200-500 r / min.

[0017] Preferably, in step 1), ethanol and water are used for centrifugal washing respectively.

[0018] Preferably, in step 2), the heating rate during calcination is 5°C / min, and the cooling rate is 10°C / min.

[0019] The invention also discloses a Bi2S3 / VS2 / S composite material obtained by the preparation method. The Bi2S3 / VS2 / S composite material is a composite structure formed by interweaving a lamellar structure and a nanorod-like structure.

[0020] The present invention also discloses the application of the Bi2S3 / VS2 / S composite material in the preparation of anode materials for magnesium ion batteries. The cathode sheet for magnesium ion batteries is prepared from the Bi2S3 / VS2 / S composite material: binder: conductive agent in a mass ratio of 7:2:1.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The invention discloses a preparation method of a Bi2S3 / VS2 / S composite material. The method comprises taking Bi(NO3)3·5H2O and NH4VO3 as raw materials, adopting a simple solvent thermal method to prepare a powder E, taking powder E and sulfur powder as raw materials, and further growing sulfur element in situ on the surface of powder E by a heat treatment method to prepare a Bi2S3 / VS2 / S composite material. By controlling the content of each raw material, reaction temperature, reaction time, etc., the morphology of the product can be well regulated, so that the prepared Bi2S3 / VS2 / S composite material presents a composite structure formed by interweaving a lamellar structure and a nanorod-like structure, wherein VS2 is a lamellar structure. Bi2S3 is a nanorod structure, VS2 is an intercalation mechanism in magnesium ion batteries, and a larger interlayer spacing is conducive to the intercalation and deintercalation of magnesium ions between layers. Bi2S3 is a semiconductor material with good conductivity and high theoretical capacity. It reacts with magnesium ions and has a conversion reaction. In addition, compared with pure phase VS2, the two mechanisms in the composite material work together to promote the magnesium storage performance and further improve the capacity of VS2, so that the Bi2S3 / VS2 / S composite material has good magnesium ion storage performance and improves the electrochemical performance of magnesium ion batteries. Sulfur can further lay the foundation for high capacity and achieve long-term stable circulation of magnesium ion batteries. Its composite structure can adjust the physical and chemical properties of a single material and give play to the synergistic effect of different components. The strong interaction between the two components can also enhance the structural stability of Bi2S3. The entire preparation method is simple, highly repeatable, short preparation cycle, low reaction temperature, reduced energy consumption and production cost, and suitable for large-scale production.

[0023] The present invention also discloses a Bi2S3 / VS2 / S composite material obtained by the above-mentioned preparation method. In the composite material, VS2 has a lamellar structure, which is conducive to the intercalation and deintercalation of magnesium ions between layers. Bi2S3, as a semiconductor material, has the advantage of high capacity. Its composite structure can adjust the physical and chemical properties of a single material and give play to the synergistic effect of different components. The strong interaction between the two components can also enhance the structural stability and improve the charge transfer kinetics of the material. In addition, sulfur can further lay the foundation for high capacity.

[0024] The present invention also discloses the application of the Bi2S3 / VS2 / S composite material in the preparation of anode materials for magnesium ion batteries. When the Bi2S3 / VS2 / S composite material is used as anode materials for magnesium ion batteries, it has good magnesium ion storage performance. The Bi2S3 / VS2 / S composite material is mixed with a binder and a conductive agent at a mass ratio of 7:2:1 to prepare a cathode sheet. The binder is carboxymethyl cellulose CMC and the conductive agent is Super P. At present, the application of VS2 in magnesium ion batteries is not mature enough and needs further exploration. The Bi2S3 / VS2 / S composite material prepared by the present invention and the conversion reaction between Bi2S3 and magnesium, and the mechanism of VS2 as an intercalation reaction, provide new ideas for the research of magnesium ion batteries and have important reference value. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The X-ray diffraction (XRD) pattern of the Bi2S3 / VS2 / S composite material prepared in Example 1 of the present invention;

[0026] Figure 2 This is a scanning electron microscope (SEM) photograph of the Bi2S3 / VS2 / S composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0028] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0029] The present invention is further described in detail below in conjunction with the accompanying drawings:

[0030] The present invention provides a method for preparing a Bi2S3 / VS2 / S composite material, which specifically comprises the following steps:

[0031] Step 1) 4-10 mL of ethylene glycol solution was measured and placed in a beaker, and bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and ammonium metavanadate (NH4VO3) were dissolved in ethylene glycol in a mass ratio of 1: (1-10) to obtain solution A. The mixture was completely dissolved by ultrasonication for 15-60 min to obtain solution B; 15-45 mL of anhydrous ethanol was slowly dripped into the mixed solution B, and stirred with a magnetic stirrer for 15-50 min to obtain a mixed solution C; the mixed solution C was transferred to a reactor, placed in an oven, and then reacted at 120-180 °C for 6-16 h to obtain a mixed solution D; the mixed solution D was repeatedly centrifuged and washed several times with ethanol and water, and then freeze-dried at -30--40 °C for 8-12 h to obtain powder E;

[0032] Step 2) Weigh powder E and sulfur powder in a mass ratio of 1: (0.5~2), mix the two thoroughly, and then put them into a tubular furnace. Under the protection of a nitrogen atmosphere, heat them to 400~700 ℃ at 5 ℃ / min, then react at 400~700 ℃ for 2 h, reduce the temperature to 100~300 ℃ at a rate of 10 ℃ / min, and cool to room temperature with the furnace to obtain a black powder, which is the Bi2S3 / VS2 / S composite material.

[0033] Preferably, the stirring speed is 200-500 r / min; and the filling degree of the reactor is controlled at 50%-80%.

[0034] The present invention prepares a Bi2S3 / VS2 / S composite material, wherein the VS2 composite material is a lamellar structure, which is conducive to the intercalation and deintercalation of magnesium ions between layers, and Bi2S3 is a semiconductor material with the advantage of high capacity. The construction of a composite structure can not only adjust the physical and chemical properties of a single material and exert the synergistic effect of different components, but also the strong interaction between the two components can enhance the structural stability and improve the charge transfer kinetics of the material. Sulfur can further lay the foundation for high capacity.

[0035] The present invention also provides an application of the above-mentioned Bi2S3 / VS2 / S composite material. When used as a negative electrode of a magnesium ion battery, the Bi2S3 / VS2 / S composite material is mixed with a binder and a conductive agent in a mass ratio of 7:2:1 to prepare a negative electrode sheet, the binder is carboxymethyl cellulose CMC, and the conductive agent is Super P.

[0036] The present invention is described below in conjunction with specific embodiments.

[0037] Embodiment 1:

[0038] A method for preparing a Bi2S3 / VS2 / S composite material, specifically comprising the following steps:

[0039] Step 1) 4 mL of ethylene glycol solution was measured and placed in a beaker, and bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and ammonium metavanadate (NH4VO3) were dissolved in ethylene glycol in a mass ratio of 1:1 to obtain solution A. The mixture was completely dissolved by ultrasonication for 15 min to obtain solution B; 15 mL of anhydrous ethanol was slowly dripped into the mixed solution B, and stirred with a magnetic stirrer for 15 min to obtain a mixed solution C; the mixed solution C was transferred to a reactor, placed in an oven, and then reacted at 120 ° C for 6 h to obtain a mixed solution D; the mixed solution D was repeatedly centrifuged and washed several times with ethanol and water, and then freeze-dried at -30 ° C for 8 h to obtain powder E;

[0040] Step 2) Weigh powder E and sulfur powder at a mass ratio of 1:0.5, mix them thoroughly, and then put them into a tube furnace. Under nitrogen atmosphere protection, heat to 400 °C at 5 °C / min, then react at 400 °C for 2 h, then reduce to 100 °C at a rate of 10 °C / min, and cool to room temperature with the furnace, and finally obtain black powder, which is Bi2S3 / VS2 / S composite material.

[0041] See also Figure 1 X-ray diffraction (XRD) spectrum of Bi2S3 / VS2 / S prepared in Example 1; the structure of the Bi2S3 / VS2 / S composite material was analyzed using Rigaku D / max2000PC X-ray diffractometer. It can be seen from the figure that the structure of the Bi2S3 / VS2 / S composite material is consistent with that of VS2 with JCPDS No. 89-1640, Bi2S3 with JCPDS No. 84-0279, and S with JCPDS No. 78-1889, indicating that the Bi2S3 / VS2 / S composite material was successfully prepared.

[0042] See also Figure 2This is a scanning electron microscope (SEM) photograph of Bi2S3 / VS2 / S prepared in Example 1. The Bi2S3 / VS2 / S was observed using a field emission scanning electron microscope (FESEM), wherein (a) is a SEM image under a high-power microscope, and (b) is a SEM image under a low-power microscope. It can be seen from the figures that VS2 in the Bi2S3 / VS2 / S presents a flaky structure, which is conducive to the intercalation and deintercalation of magnesium ions between layers. Bi2S3 presents a nanorod structure, and the VS2 flaky structure is intertwined with the Bi2S3 nanorod structure. The constructed composite structure can not only adjust the physicochemical properties of a single material and exert the synergistic effect of different components, but also the strong interaction between the two components can enhance the structural stability and improve the charge transfer kinetics of the material. In addition, elemental sulfur can further lay the foundation for high capacity.

[0043] Embodiment 2:

[0044] A method for preparing a Bi2S3 / VS2 / S composite material, specifically comprising the following steps:

[0045] Step 1) 6 mL of ethylene glycol solution was measured and placed in a beaker, and anhydrous bismuth nitrate (Bi(NO3)3·5H2O) and ammonium metavanadate (NH4VO3) were dissolved in ethylene glycol in a mass ratio of 3:1 to obtain solution A. The mixture was completely dissolved by ultrasonication for 30 min to obtain solution B; 25 mL of anhydrous ethanol was slowly dripped into the mixed solution B, and stirred with a magnetic stirrer for 25 min to obtain a mixed solution C; the mixed solution C was transferred to a reactor, placed in an oven, and then reacted at 140 °C for 10 h to obtain a mixed solution D; the mixed solution D was repeatedly centrifuged and washed several times with ethanol and water, and then freeze-dried at -40 °C for 10 h to obtain powder E;

[0046] Step 2) Weigh powder E and sulfur powder in a mass ratio of 1:1, mix them thoroughly, and then put them into a tube furnace. Under nitrogen atmosphere protection, heat to 500 °C at 5 °C / min, then react at 500 °C for 2 h, and finally reduce to 300 °C at a rate of 10 °C / min. Finally, cool to room temperature with the furnace and collect the powder, and finally obtain black powder, which is Bi2S3 / VS2 / S composite material.

[0047] Embodiment 3:

[0048] A method for preparing a Bi2S3 / VS2 / S composite material, specifically comprising the following steps:

[0049] Step 1) 8 mL of ethylene glycol solution was measured and placed in a beaker, and bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and ammonium metavanadate (NH4VO3) were dissolved in ethylene glycol in a certain mass ratio (5:1) to obtain solution A. The mixture was completely dissolved by ultrasonication for 45 min to obtain solution B; 35 mL of anhydrous ethanol was slowly dripped into the mixed solution B, and stirred with a magnetic stirrer for 35 min to obtain a mixed solution C; the mixed solution C was transferred to a reactor, placed in an oven, and then reacted at 160°C for 13 h to obtain a mixed solution D; the mixed solution D was repeatedly centrifuged and washed several times with ethanol and water, and then freeze-dried at -40°C for 12 h to obtain powder E;

[0050] Step 2) Weigh powder E and sulfur powder at a mass ratio of 1:1.5, mix them thoroughly, and then put them into a tube furnace. Under nitrogen atmosphere protection, heat to 600 °C at 5 °C / min, then react at 600 °C for 2 h, and finally reduce to 300 °C at a rate of 10 °C / min. Finally, cool to room temperature with the furnace and collect the powder, and finally obtain black powder, which is Bi2S3 / VS2 / S composite material.

[0051] Embodiment 4:

[0052] A method for preparing a Bi2S3 / VS2 / S composite material, specifically comprising the following steps:

[0053] Step 1) 10 mL of ethylene glycol solution was measured and placed in a beaker, and bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) and ammonium metavanadate (NH4VO3) were dissolved in ethylene glycol in a certain mass ratio (10:1) to obtain solution A. The mixture was completely dissolved by ultrasonication for 60 min to obtain solution B; 45 mL of anhydrous ethanol was slowly dripped into the mixed solution B, and stirred with a magnetic stirrer for 50 min to obtain a mixed solution C; the mixed solution C was transferred to a reactor, placed in an oven, and then reacted at 180°C for 16 h to obtain a mixed solution D; the mixed solution D was repeatedly centrifuged and washed several times with ethanol and water, and then freeze-dried at -30°C for 12 h to obtain powder E;

[0054] Step 2) Weigh powder E and sulfur powder in a mass ratio of 1:2, mix them thoroughly, and then put them into a tube furnace. Under nitrogen atmosphere protection, heat to 700 °C at 5 °C / min, then react at 700 °C for 2 h, and finally reduce to 300 °C at a rate of 10 °C / min. Finally, cool to room temperature with the furnace and collect the powder, and finally obtain black powder, which is Bi2S3 / VS2 / S composite material.

[0055] The present invention not only can play the synergistic effect of different components by designing composite materials, but the strong interaction between the two components can also enhance the structural stability. Combining the advantages of the two materials is a very promising strategy. Further in-situ growth of sulfur on the surface can further increase its capacity. Constructing a composite structure can not only adjust the physicochemical properties of a single material and play the synergistic effect of different components, but also the strong interaction between the two components can enhance the structural stability and improve the charge transfer kinetics of the material. Bi2S3 has the advantages of low cost and high capacity, but its structural stability is poor. In practical applications, Mg 2+ Repeated insertion and extraction will cause structural damage, so long-term stable cycling cannot be achieved. VS2 has a unique layered structure that facilitates Mg 2+ Insertion and extraction make it an ideal negative electrode material. Therefore, designing Bi2S3 / VS2 / S composite materials to improve magnesium storage performance has very important practical significance.

[0056] The present invention prepares a Bi2S3 / VS2 / S composite material, wherein the VS2 composite material is a lamellar structure, and the lamellar structure is conducive to the intercalation and deintercalation of magnesium ions between layers. Bi2S3 is a semiconductor material and has the advantage of high capacity. The construction of a composite structure can not only adjust the physicochemical properties of a single material and give play to the synergistic effect of different components, but also the strong interaction between the two components can enhance the structural stability and improve the charge transfer kinetics of the material. Sulfur can further lay the foundation for high capacity. At present, the research on magnesium ion batteries is not mature enough, and the composite material prepared by the present invention provides a reference for the research on magnesium ion batteries.

[0057] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a Bi2S3 / VS2 / S composite material, characterized in that: The following steps are involved: 1) Dissolve Bi(NO3)3·5H2O and NH4VO3 in ethylene glycol solution, disperse them uniformly by ultrasonication, add anhydrous ethanol, stir them uniformly, carry out hydrothermal reaction, cool them to room temperature, wash them, and freeze-dry them to obtain powder; The mass ratio of Bi(NO3)3·5H2O to NH4VO3 is 1:(1-10); 2) fully mixing the powder obtained in step 1) with sulfur powder, calcining under an inert atmosphere, and cooling to room temperature to obtain a Bi2S3 / VS2 / S composite material; The mass ratio of the powder to sulfur powder is 1:(0.5~2); In step 1), the temperature of the hydrothermal reaction is 120-180 °C, and the time of the hydrothermal reaction is 6-16 h.

2. The method for preparing the Bi2S3 / VS2 / S composite material according to claim 1, characterized in that: In step 2), the calcination temperature is 400-700 °C and the calcination time is 2 h.

3. The method for preparing the Bi2S3 / VS2 / S composite material according to claim 1, characterized in that: In step 1), the freeze-drying temperature is -30~-40°C, and the freeze-drying time is 8~12 h.

4. The method for preparing the Bi2S3 / VS2 / S composite material according to claim 1, characterized in that: In step 1), the ultrasonic dispersion time is 15 to 60 min.

5. The method for preparing the Bi2S3 / VS2 / S composite material according to claim 1, characterized in that: In step 1), the stirring time is 15-50 min, and the stirring speed is 200-500 r / min.

6. The method for preparing the Bi2S3 / VS2 / S composite material according to claim 1, characterized in that: In step 1), ethanol and water are used for centrifugal washing respectively.

7. The method for preparing the Bi2S3 / VS2 / S composite material according to claim 1, characterized in that: In step 2), the heating rate during calcination is 5°C / min and the cooling rate is 10°C / min.

8. The Bi2S3 / VS2 / S composite material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The Bi2S3 / VS2 / S composite material is a composite structure formed by interweaving a lamellar structure and a nanorod-like structure.

9. Use of the Bi2S3 / VS2 / S composite material according to claim 8 in preparing anode materials for magnesium ion batteries, characterized in that: The negative electrode sheet of the magnesium ion battery is prepared from Bi2S3 / VS2 / S composite material: binder: conductive agent in a mass ratio of 7:2:1.