A flame retardant masterbatch and a highly impact-resistant flame retardant polymer material

By using components such as acrylonitrile-acrylamide copolymer and black phosphorus in PC/ABS materials, the dispersion of the flame retardant masterbatch is improved, the problem of flame retardant properties reducing mechanical properties is solved, and the material's high impact resistance is achieved. and excellent flame retardant properties.

CN116285190BActive Publication Date: 2024-10-29GUANGDONG A & B NEW MATERIAL CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310108210.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-14
Publication Date
2024-10-29
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

When existing technology imparts flame retardant properties to PC/ABS materials, it usually reduces its mechanical properties, making it difficult to achieve a balance between flame retardancy and mechanical properties.

Method used

Using acrylonitrile-acrylamide copolymer as the masterbatch carrier, combined with black phosphorus and inorganic magnesium compounds, by improving the dispersion uniformity of the material and improving the dispersion of the flame-retardant masterbatch in PC/ABS, the mechanical properties and Flame retardant properties.

Benefits of technology

It achieves the synergistic improvement of the mechanical properties and flame retardant properties of PC/ABS materials, ensuring the material's excellent performance in high impact resistance and flame retardancy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004075774390000051
    Figure BDA0004075774390000051
  • Figure BDA0004075774390000061
    Figure BDA0004075774390000061
  • Figure BDA0004075774390000062
    Figure BDA0004075774390000062
Patent Text Reader

Abstract

The invention belongs to the field of flame retardant materials, and discloses a flame retardant masterbatch, including acrylonitrile-acrylamide copolymer, black phosphorus, inorganic magnesium compound, and organic magnesium compound; the weight ratio of acrylonitrile-acrylamide copolymer, black phosphorus, inorganic magnesium compound, and organic magnesium compound is 20:5-10:10-15:5-10. The masterbatch of the present invention adopts acrylonitrile-acrylamide copolymer as a masterbatch carrier, and the organic magnesium compound is generally a polyhydroxy compound, which has good affinity with acrylamide. At the same time, the acrylonitrile-acrylamide copolymer has good compatibility with black phosphorus and inorganic magnesium compound, which can improve the dispersion uniformity of the flame retardant masterbatch in PC / ABS, and finally effectively guarantee the mechanical properties and flame retardant properties of the material. At the same time, the present invention also provides a flame retardant polymer material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of flame retardant materials, and in particular relates to a flame retardant masterbatch and a highly impact-resistant flame retardant polymer material. Background Art

[0002] CN112011147A discloses a long glass fiber reinforced flame retardant ABS composite material and its preparation method, which includes components such as polycarbonate, ABS, flame retardant, modified fiber, modified graphene oxide, etc., wherein the surface of the modified graphene oxide is treated with a silane coupling agent to improve the compatibility of graphene oxide and matrix components (polycarbonate, ABS), so that it can be evenly dispersed in the system; the modified fiber is mainly prepared by black phosphorene, dopamine, anhydrous ethanol, and pretreated fiber; the pretreated fiber is a glass fiber with carbon nanowires grown on the surface, and the glass fiber is a continuous glass fiber. The synergistic effect of aluminum hydroxide, magnesium hydroxide, polysiloxane, modified graphene oxide and black phosphorene is used to make the ABS composite material have excellent flame retardant properties, and low smoke and low toxicity when burning, and higher practicality.

[0003] CN115386214A discloses a weather-resistant halogen-free flame-retardant polycarbonate alloy material and a preparation method thereof. The alloy material comprises: polycarbonate, styrene-acrylonitrile-based binary or ternary copolymer, modified graphene oxide weather-resistant halogen-free flame retardant, and optionally a processing aid. The modified graphene oxide weather-resistant halogen-free flame retardant comprises: graphene oxide matrix, benzotriazole group, phenylphosphonic acid group. The alloy material has excellent flame retardant and weather resistance properties, and can simultaneously increase the heat deformation temperature and maintain the mechanical strength without decreasing.

[0004] PC / ABS itself is a plastic material with high impact resistance. When it is given flame retardant properties, its mechanical properties are often reduced. In the prior art, in order to solve this problem, most of them use the addition of graphene and fiber materials in combination with the optimization of flame retardant materials to achieve a balance between flame retardancy and mechanical properties.

[0005] Therefore, the technical problem to be solved in this case is: how to further optimize the mechanical properties and flame retardant properties of PC / ABS. Summary of the invention

[0006] In view of the shortcomings and deficiencies of the current prior art, the primary purpose of the present invention is to provide a flame retardant masterbatch. The masterbatch of the present invention uses acrylonitrile-acrylamide copolymer as a masterbatch carrier. The organic magnesium compound is generally a polyhydroxy compound, which has good affinity with acrylamide. At the same time, the acrylonitrile-acrylamide copolymer has good compatibility with black phosphorus and inorganic magnesium compounds, which can improve the dispersion uniformity of the flame retardant masterbatch in PC / ABS, and ultimately effectively guarantee the mechanical properties and flame retardant properties of the material.

[0007] Another object of the present invention is to provide a flame retardant polymer material.

[0008] The specific plan is as follows:

[0009] A flame retardant masterbatch comprises acrylonitrile-acrylamide copolymer, black phosphorus, an inorganic magnesium compound and an organic magnesium compound; the weight ratio of the acrylonitrile-acrylamide copolymer, the black phosphorus, the inorganic magnesium compound and the organic magnesium compound is 20:5-10:10-15:5-10.

[0010] In the present invention, acrylonitrile-acrylamide copolymer is used as the masterbatch carrier. The reason is that the organic magnesium compound is generally a polyhydroxy compound, which has good affinity with acrylamide. At the same time, the acrylonitrile-acrylamide copolymer has good compatibility with black phosphorus and inorganic magnesium compounds, which can improve the dispersion uniformity of the flame retardant masterbatch in PC / ABS, and ultimately effectively guarantee the mechanical properties and flame retardant properties of the material.

[0011] In some embodiments of the present invention, the weight ratio of acrylonitrile-acrylamide copolymer, black phosphorus, inorganic magnesium compound and organic magnesium compound can be selected as 20:5:10:5, 20:6:12:7, 20:8:14:8, 20:10:15:10, 20:5:15:10, 20:5:10:10, 20:5:15:5, 20:10:10:5, 20:10:15:10 or 20:10:15:5;

[0012] In some embodiments of the present invention, when the acrylonitrile-acrylamide copolymer is 20 parts by weight, the black phosphorus can be selected to be 5, 6, 7, 8, 9 or 10 parts by weight;

[0013] When the acrylonitrile-acrylamide copolymer is 20 parts by weight, the inorganic magnesium compound can be selected to be 10, 11, 12, 13, 14 or 15 parts by weight;

[0014] When the acrylonitrile-acrylamide copolymer is 20 parts by weight, the organic magnesium compound can be selected to be 5, 6, 7, 8, 9 or 10 parts by weight;

[0015] As a further preferred embodiment of the present invention, the weight ratio of acrylonitrile-acrylamide copolymer, black phosphorus, inorganic magnesium compound and organic magnesium compound is 20:7-9:12-14:5-7.

[0016] In the flame retardant masterbatch, the inorganic magnesium compound is magnesium hydroxide or magnesium oxide; the organic magnesium is hydrated magnesium citrate, magnesium glycinate, magnesium gluconate or magnesium L-aspartate.

[0017] In the flame retardant masterbatch, the weight ratio of acrylonitrile units to acrylamide units in the acrylonitrile-acrylamide copolymer is 10:1-5, preferably 10:2-3.

[0018] In some embodiments of the present invention, the weight ratio of acrylonitrile units to acrylamide units may be selected as: 10:1, 10:2, 10:3, 10:4 or 10:5;

[0019] In the above-mentioned flame retardant masterbatch, the acrylonitrile-acrylamide copolymer is prepared by the following method:

[0020] Add acrylonitrile and acrylamide to tetrahydrofuran, and add an oil-soluble initiator dropwise under an inert atmosphere, wherein the weight of the initiator is 0.1-0.5% of the total weight of acrylonitrile and acrylamide; the reaction temperature is 70-80°C, and the reaction time is 4-8h; after the reaction is completed, cool to room temperature, introduce the product solution into methanol, and collect the precipitate in the methanol.

[0021] It should be noted that, in the present invention, the organic solvent is not limited to tetrahydrofuran, for example, ethyl acetate, benzene, toluene, n-hexane, cyclohexane, etc. are all optional organic solvents.

[0022] In the flame retardant masterbatch, the tetrahydrofuran is 1-3 times, preferably 2-3 times, of the total weight of acrylonitrile and acrylamide. In some implementation cases, the tetrahydrofuran is 1, 1.5, 2, 2.5 or 3 times of the total weight of acrylonitrile and acrylamide; the initiator is an azo initiator.

[0023] In the above-mentioned flame retardant masterbatch, the preparation method of the flame retardant masterbatch is: after drying acrylonitrile-acrylamide copolymer, black phosphorus, inorganic magnesium compound and organic magnesium compound, add them into a screw extruder for mixing and granulation to obtain the flame retardant masterbatch.

[0024] At the same time, the present invention also discloses a highly impact-resistant flame-retardant polymer material, comprising a PC / ABS composite masterbatch and a flame-retardant masterbatch as described in any one of claims 1 to 7; the PC / ABS composite masterbatch is composed of 10 to 30 parts of polycarbonate and 70 to 90 parts of ABS; the weight ratio of the PC / ABS composite masterbatch to the flame-retardant masterbatch is 50 to 80:20 to 50.

[0025] In some implementation cases, the total weight of polycarbonate and ABS in the PC / ABS composite masterbatch is 100 parts by weight, and the weight of polycarbonate can be 10, 15, 20, 25 or 30 parts by weight; the weight of ABS can be 70, 75, 80, 85 or 90 parts by weight;

[0026] In some embodiments, the weight ratio of the PC / ABS composite masterbatch to the flame retardant masterbatch is 50:50, 55:45, 60:40, 65:35, 70:30, 75:25 or 80:20.

[0027] The above-mentioned high impact resistant flame retardant polymer material also includes appropriate amounts of plasticizer and compatibilizer.

[0028] In the above-mentioned high impact-resistant flame-retardant polymer material, the PC / ABS composite masterbatch is composed of 20-30 parts of polycarbonate and 70-80 parts of ABS; the weight ratio of the PC / ABS composite masterbatch to the flame-retardant masterbatch is 65-75:25-35.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The masterbatch of the present invention adopts acrylonitrile-acrylamide copolymer as the masterbatch carrier. The organic magnesium compound is generally a polyhydroxy compound, which has good affinity with acrylamide. At the same time, the acrylonitrile-acrylamide copolymer has good compatibility with black phosphorus and inorganic magnesium compounds, which can improve the dispersion uniformity of the flame retardant masterbatch in PC / ABS, and finally effectively guarantee the mechanical properties and flame retardant properties of the material.

[0031] At the same time, the present invention also provides a flame retardant polymer material, which uses PC / ABS as a base material and adopts the flame retardant masterbatch of the present invention, and can achieve synergy of mechanical properties and flame retardant properties. DETAILED DESCRIPTION

[0032] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0033] Part I Preparation of Acrylonitrile-Acrylamide Copolymer

[0034] Example 1-1

[0035] 100 g of acrylonitrile and acrylamide in total were added to 250 g of tetrahydrofuran, and 0.2 g of an oil-soluble initiator azobisisoheptanenitrile was added dropwise under an inert atmosphere; the reaction temperature was 75°C and the reaction time was 6 h; after the reaction was completed, the reaction was cooled to room temperature, the product solution was introduced into methanol, and the precipitate in the methanol was collected;

[0036] The weight ratio of acrylonitrile to acrylamide is 10:1;

[0037] Polymer 1 was obtained.

[0038] Example 1-2

[0039] 100 g of acrylonitrile and acrylamide in total were added to 250 g of tetrahydrofuran, and 0.2 g of an oil-soluble initiator azobisisoheptanenitrile was added dropwise under an inert atmosphere; the reaction temperature was 75°C and the reaction time was 6 h; after the reaction was completed, the reaction was cooled to room temperature, the product solution was introduced into methanol, and the precipitate in the methanol was collected;

[0040] The weight ratio of acrylonitrile to acrylamide is 10:3;

[0041] Polymer 2 was obtained.

[0042] Examples 1-3

[0043] 100 g of acrylonitrile and acrylamide in total were added to 250 g of tetrahydrofuran, and 0.2 g of an oil-soluble initiator azobisisoheptanenitrile was added dropwise under an inert atmosphere; the reaction temperature was 75°C and the reaction time was 6 h; after the reaction was completed, the reaction was cooled to room temperature, the product solution was introduced into methanol, and the precipitate in the methanol was collected;

[0044] The weight ratio of acrylonitrile to acrylamide is 10:5;

[0045] Polymer 3 was obtained.

[0046] Part II Preparation of Flame Retardant Masterbatch (Flame Retardant Masterbatch 1-8)

[0047] The flame retardant masterbatch is prepared as follows:

[0048] After drying, acrylonitrile-acrylamide copolymer, black phosphorus, inorganic magnesium compound and organic magnesium compound are added into a screw extruder for mixing and granulation to obtain flame retardant masterbatch;

[0049] The formula can be referred to in Table 1 below;

[0050] Table 1 Recipe

[0051]

[0052]

[0053] Part 3 Preparation of flame retardant masterbatch (comparative masterbatch 1-6)

[0054] The flame retardant masterbatch is prepared as follows:

[0055] After drying, acrylonitrile-acrylamide copolymer, black phosphorus, inorganic magnesium compound and organic magnesium compound are added into a screw extruder for mixing and granulation to obtain flame retardant masterbatch;

[0056] The formula can be referred to in Table 2 below;

[0057] Table 2 Recipe

[0058]

[0059]

[0060] Part IV Preparation of flame retardant polymer materials

[0061] The PC / ABS composite masterbatch, the flame retardant masterbatch, the plasticizer, the compatibilizer and the antioxidant are added into a twin-screw extruder for processing to prepare a flame retardant polymer material;

[0062] The temperature of the first zone of the twin-screw extruder is 200°C, the temperature of the second zone is 230°C, the temperature of the third zone is 230°C, the temperature of the fourth, fifth and sixth zones is 240°C, and the temperature of the seventh zone is 230°C; the rotation speed of the twin-screw extruder is 200-300rpm.

[0063] The formula of flame retardant polymer materials refers to Tables 3 and 4;

[0064] Table 3 Formula Weight: g

[0065]

[0066] Note: PC / ABS composite masterbatch 1 contains 25 parts of polycarbonate and 75 parts of ABS.

[0067] In Table 4, the formula weight is the same as that in Example 3, except that different PC / ABS composite masterbatch and flame retardant masterbatch are used, as shown in Table 4;

[0068] Table 4 Recipe

[0069] Example 7 PC / ABS composite masterbatch 1 Flame retardant masterbatch 1 Example 8 PC / ABS composite masterbatch 1 Flame retardant masterbatch 3 Example 9 PC / ABS composite masterbatch 1 Flame retardant masterbatch 4 Example 10 PC / ABS composite masterbatch 1 Flame retardant masterbatch 5 Embodiment 11 PC / ABS composite masterbatch 1 Flame retardant masterbatch 6 Example 12 PC / ABS composite masterbatch 1 Flame retardant masterbatch 7 Example 13 PC / ABS composite masterbatch 1 Flame retardant masterbatch 8 Embodiment 14 PC / ABS composite masterbatch 2 Flame retardant masterbatch 2 Embodiment 15 PC / ABS composite masterbatch 3 Flame retardant masterbatch 2 Comparative Example 1 PC / ABS composite masterbatch 1 Comparison masterbatch 1 Comparative Example 2 PC / ABS composite masterbatch 1 Comparison Masterbatch 2 Comparative Example 3 PC / ABS composite masterbatch 1 Comparison Masterbatch 3 Comparative Example 4 PC / ABS composite masterbatch 1 Comparison Masterbatch 4 Comparative Example 5 PC / ABS composite masterbatch 1 Comparison Masterbatch 5 Comparative Example 6 PC / ABS composite masterbatch 1 Comparison Masterbatch 6

[0070] Performance Testing

[0071] 1. Tensile strength: Use universal tensile testing machine and implement standard 527-2 / T1040.

[0072] 2. Elongation at break: Use universal tensile testing machine and implement standard 527-2 / T1040.

[0073] 3. Impact strength: Use cantilever beam impact testing machine, implement standard 180 / 1A / T1843.

[0074] 4. Oxygen index: Use intelligent oxygen index tester and implement standard GB / T2406.2-2009.

[0075] 5. Flame retardant evaluation: Evaluated according to UL94 flame retardant grade standard

[0076] Table 5 Test results

[0077]

[0078]

[0079] Result analysis:

[0080] 1. From the flame retardancy and mechanical properties of Example 3 and Comparative Examples 1-6, the order of flame retardancy is Example 3>Comparative Example 6>Comparative Example 1>Comparative Example 3≈Comparative Example 4>Comparative Example 2>Comparative Example 5; the order of mechanical properties is Example 3>Comparative Example 5>Comparative Example 2>Comparative Example 4>Comparative Example 3>Comparative Example 1>Comparative Example 6;

[0081] The greater the amount of black phosphorus used, the better the flame retardant properties but the worse the mechanical properties; excessive organic magnesium has little effect on the mechanical properties, but a greater impact on the flame retardant properties; the use of polyacrylamide and polyacrylonitrile alone is not beneficial to the improvement of flame retardant and mechanical properties. We believe that the dispersion properties of flame retardant materials and parent materials can have a significant impact on the mechanical properties and flame retardant uniformity. The use of polyacrylamide and polyacrylonitrile alone is not beneficial to the dispersion of flame retardant materials; the lack of magnesium hydroxide has a negative impact on flame retardant properties.

[0082] 2. Through the comparison of Examples 1-6, it can be seen that when the ratio of PC / ABS composite masterbatch to flame retardant masterbatch is 65:35, its mechanical properties and flame retardant properties can achieve the best performance and synergy.

[0083] 3. Through the comparison of Examples 7-15, it can be seen that when the PC / ABS composite masterbatch 1 and the flame retardant masterbatch 2 are combined, their mechanical properties and flame retardant properties can achieve the best performance and synergy.

Claims

1. A flame retardant masterbatch, characterized in that: The invention comprises acrylonitrile-acrylamide copolymer, black phosphorus, an inorganic magnesium compound and an organic magnesium compound; the weight ratio of the acrylonitrile-acrylamide copolymer, black phosphorus, the inorganic magnesium compound and the organic magnesium compound is 20:5-10:10-15:5-10, the inorganic magnesium compound is magnesium hydroxide or magnesium oxide; the organic magnesium is hydrated magnesium citrate, magnesium glycinate, magnesium gluconate or magnesium L-aspartate; The acrylonitrile-acrylamide copolymer is prepared by the following method: Add acrylonitrile and acrylamide to tetrahydrofuran, and add an oil-soluble initiator dropwise under an inert atmosphere, wherein the weight of the initiator is 0.1-0.5% of the total weight of acrylonitrile and acrylamide; the reaction temperature is 70-80°C, and the reaction time is 4-8h; after the reaction is completed, cool to room temperature, introduce the product solution into methanol, and collect the precipitate in the methanol; The weight ratio of acrylonitrile to acrylamide in the acrylonitrile-acrylamide copolymer is 10:2-3.

2. The flame retardant masterbatch according to claim 1, characterized in that: The weight ratio of acrylonitrile-acrylamide copolymer, black phosphorus, inorganic magnesium compound and organic magnesium compound is 20:7-9:12-14:5-7.

3. The flame retardant masterbatch according to claim 2, characterized in that: The tetrahydrofuran is 1-3 times the total weight of acrylonitrile and acrylamide; and the initiator is an azo initiator.

4. The flame retardant masterbatch according to claim 1, characterized in that: The preparation method of the flame retardant masterbatch is as follows: after drying acrylonitrile-acrylamide copolymer, black phosphorus, inorganic magnesium compound and organic magnesium compound, the mixture is added into a screw extruder for mixing and granulation to obtain the flame retardant masterbatch.

5. A highly impact-resistant flame-retardant polymer material, characterized in that: The invention comprises a PC / ABS composite masterbatch and a flame retardant masterbatch as claimed in any one of claims 1 to 4; the PC / ABS composite masterbatch is composed of 10 to 30 parts of polycarbonate and 70 to 90 parts of ABS; and the weight ratio of the PC / ABS composite masterbatch to the flame retardant masterbatch is 50 to 80:20 to 50.

6. The highly impact-resistant flame-retardant polymer material according to claim 5, characterized in that: It also includes appropriate amounts of plasticizers and compatibilizers.

7. The highly impact-resistant flame-retardant polymer material according to claim 5, characterized in that: The PC / ABS composite masterbatch is composed of 20-30 parts of polycarbonate and 70-80 parts of ABS; the weight ratio of the PC / ABS composite masterbatch to the flame retardant masterbatch is 65-75:25-35.

Citation Information

Patent Citations

  • Long glass fiber reinforced flame-retardant ABS composite material and preparation method thereof

    CN112011147A

  • Weather-resistant halogen-free flame-retardant polycarbonate alloy material and preparation method thereof

    CN115386214A

  • Polycarbonate composition with flame retardation function

    CN106497000A

  • Glass fiber reinforced plastic composite material and preparation method thereof

    CN110128787A

  • High-strength MPP pipe and preparation method thereof

    CN112226006A