A low smoke density, scratch-resistant polycarbonate material and its preparation method and application

By using synergistic blending of phosphate flame retardants and phosphorus compound-modified nano-MoS2 hollow materials in polycarbonate materials, the problem of both flame retardancy and scratch resistance of polycarbonate materials is solved when reducing smoke density. , achieving the effects of high flame retardant level and low smoke density.

CN116285294BActive Publication Date: 2024-10-18WANHUA CHEMICAL (NINGBO) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310486813.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-10-18
Estimated Expiration
2043-05-04

AI Technical Summary

Technical Problem

It is difficult for existing polycarbonate materials to achieve both flame retardancy and scratch resistance while reducing smoke density. Flame-retardant treated materials increase the amount of smoke generated, and the addition of rubber tougheners or inorganic blends will reduce the flame retardancy. performance.

Method used

Synergistic blending of polycarbonate resin, phosphate ester flame retardants and phosphorus compound-modified nano-MoS2 hollow materials is used to improve the flame retardancy and scratch resistance of the material through a combination of specific proportions, and the phosphorus compound is modified by preparing Nano-MoS2 hollow material to achieve low smoke density and high scratch resistance.

Benefits of technology

It achieves low smoke density and high scratch resistance of polycarbonate materials at high flame retardant levels, meeting the needs of automobiles, home appliances and other products for low smoke density and high scratch resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116285294B_ABST
    Figure CN116285294B_ABST
Patent Text Reader

Abstract

The present invention discloses a low smoke density, scratch-resistant polycarbonate material and its preparation method and application, wherein the polycarbonate material comprises the following raw materials in parts by weight: 75-90 parts of polycarbonate resin, preferably 80-88 parts; 2-12 parts of phosphate flame retardant, preferably 5-10 parts; 2-10 parts of phosphorus compound modified nano MoS2 hollow material, preferably 4-7 parts; 0-8 parts of other additives, preferably 1-5 parts. The present invention can ensure that the polycarbonate has good flame retardancy while also having lower smoke suppression performance and higher scratch resistance through the synergistic blending of specific raw materials in a specific proportion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a polycarbonate material, in particular to a low smoke density, scratch-resistant polycarbonate material and a preparation method and application thereof. Background Art

[0002] Polycarbonate (PC) has good performance advantages in terms of impact resistance, creep resistance, dimensional stability and electrical insulation. It is widely used in the manufacture of windshields and driving windows of aircraft and vehicles, as glass for transportation and housing, and in the manufacture of various lamps and safety masks, mechanical parts, medical equipment, and electrical equipment housings. Polycarbonate itself has certain flame retardancy, but polycarbonate is required to have lower smoke suppression performance and higher scratch resistance in closed environments such as high-speed railways, aircraft, automobiles, and buildings. The smoke generation of some flame-retardant treated polycarbonates often increases. For example, the halogen antimony system can inhibit oxidation and promote smoke generation, while some smoke suppressants that help oxidation interfere with flame retardancy, that is, the functions of flame retardants and smoke suppressants conflict with each other; and the addition of rubber toughening agents to improve the scratch resistance of the product also has the problem of poor smoke suppression. If inorganic substances are added for blending and modification, the flame retardancy of the product will be reduced. Therefore, providing solutions to the above problems is of great significance for the development of high-performance polycarbonates.

[0003] In the prior art, in order to reduce the smoke density of polycarbonate alloys, most methods are to add inorganic minerals for modification. For example, patent CN109777073B uses sulfonates and phosphorus-containing compounds to reduce the smoke density and heat release rate of polycarbonate; patent CN105849171B uses poly (carbonate-bisphenol aromatic compound ester) raw materials with special structures, adds 10wt% to 40wt% of glass fiber, and obtains a low smoke density and low heat release polycarbonate composition that meets HL2 or HL3; patent CN112409770A uses organosilicon / phenoxy polyphosphazene copolymer raw materials, adds 10-20wt% mineral powder, and achieves low smoke density and low heat release effects. However, none of the above solutions fully solves the technical problem that it is difficult to balance the flame retardancy, smoke suppression and scratch resistance of polycarbonate. Summary of the invention

[0004] In order to solve the above technical problems, the present invention first proposes a low smoke density, scratch-resistant polycarbonate material, which comprises a polycarbonate resin, a phosphate flame retardant and a phosphorus compound-modified nano-MoS2 hollow material. The synergistic blending of the above components in a specific proportion can ensure that the polycarbonate has good flame retardancy while also having lower smoke suppression performance and higher scratch resistance.

[0005] The invention also provides a method for preparing a low-smoke-density and scratch-resistant polycarbonate material.

[0006] The present invention also provides a low smoke density, scratch-resistant polycarbonate material for use in rail transit interior materials, electrical appliance housings and other products.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] Based on the first aspect of the present invention, a low smoke density, scratch-resistant polycarbonate material is first provided, which comprises the following raw materials in parts by weight:

[0009]

[0010] Among them, the weight parts of polycarbonate resin include but are not limited to 75 parts, 76 parts, 77 parts, 78 parts, 79 parts, 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts, 90 parts, etc.

[0011] The weight parts of phosphate flame retardants include but are not limited to 2 parts, 3 parts, 4 parts, 0.4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, etc.

[0012] The weight parts of phosphorus compound modified nano MoS2 hollow material include but are not limited to 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc.

[0013] The weight parts of other additives include but are not limited to 1 part, 2 parts, 3 parts, 4 parts, 5 parts, etc.

[0014] As a preferred embodiment of the present invention, the polycarbonate resin is a linear bisphenol A type aromatic polycarbonate with a weight average molecular weight of 20,000-40,000, for example, including but not limited to 25,000, 28,000, 30,000, 32,000, 37,000, etc.

[0015] As a preferred embodiment of the present invention, the phosphate flame retardant is one or more of triphenyl phosphate, bisphenol A-bis(diphenyl phosphate), and resorcinol bis(diphenyl phosphate).

[0016] As a preferred embodiment of the present invention, the phosphorus compound modified nano MoS2 hollow material is prepared by the following method:

[0017] 1) dissolving ammonium molybdate, thiourea, hydroxylamine hydrochloride and a surfactant in water, adjusting the pH to 5-6.5 and transferring to a polytetrafluoroethylene reactor, reacting at 140-200° C., preferably 190-210° C., for at least 24 h, preferably 24-30 h, cooling to room temperature and filtering, washing and drying to obtain a solid product, i.e., nano-MoS2 hollow microspheres;

[0018] 2) mixing the solid product obtained in step 1) and the intercalation agent in a solvent, reacting at 25-100° C. for 2-6 hours, filtering, washing, and drying to obtain intercalated MoS2 hollow microspheres;

[0019] 3) adding the intercalated MoS2 hollow microspheres into water, and ultrasonically dispersing to obtain a suspension of intercalated MoS2 hollow microspheres with surface electronegativity; adding the phosphorus-containing compound solution into the above suspension, and ultrasonically mixing at room temperature for 5-100 minutes, filtering, washing, and drying to obtain a phosphorus-compound-modified nano-MoS2 hollow material.

[0020] As a preferred embodiment of the present invention, in step 1), the molar ratio of ammonium molybdate, thiourea and hydroxylamine hydrochloride is 1:(2-6):(1-4);

[0021] Preferably, in step 1), the surfactant is selected from nonionic surfactants and / or cationic surfactants. The surfactants described in the present invention are not specifically limited, and any nonionic surfactants and cationic surfactants known to those skilled in the art can realize the present invention. The nonionic surfactant is preferably one or more of F127, F108, and P123, and the cationic surfactant is preferably one or more of benzyltriethylammonium chloride, octadecyldimethyl tertiary amine, and dodecyldimethylbenzylammonium bromide;

[0022] Preferably, the amount of the surfactant is 0.1-0.5 times the molar amount of ammonium molybdate;

[0023] Preferably, in step 1), 0.5-2 mol / L hydrochloric acid is used to adjust the pH.

[0024] As a preferred embodiment of the present invention, in step 2), the intercalation agent is at least one of n-butyl lithium and lithium hydride;

[0025] Preferably, the amount of the intercalant used is 1-3 times the mass of the solid product obtained in step 1).

[0026] Preferably, the solvent in step 2) is selected from at least one of n-hexane and ethylene glycol.

[0027] As a preferred embodiment of the present invention, in step 3), the phosphorus-containing compound is one or more of (4-carboxybutyl)triphenylphosphonium bromide, melamine phosphate, butyltriphenylphosphonium bromide, and tetradecyltriphenylphosphonium bromide;

[0028] Preferably, the mass ratio of the phosphorus-containing compound to the intercalated MoS2 hollow microspheres is (1-10):1.

[0029] As a preferred embodiment of the present invention, the other auxiliary agent is optionally at least one of a lubricant, an antioxidant, and a light stabilizer.

[0030] Preferably, the lubricant may be selected from conventional lubricants in the art, such as at least one of silane polymers, paraffin wax, fatty acid salts, stearates or polytetrafluoroethylene.

[0031] Preferably, the antioxidant can be selected from conventional antioxidants in the art, such as at least one of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (antioxidant 1010), β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate octadecyl alcohol (antioxidant 1076) and tris(2,4-di-tert-butylphenyl)phosphite (antioxidant).

[0032] Preferably, the light stabilizer can be selected from conventional light stabilizers in the art, such as at least one compound of triazine, benzotriazole, and cyanoacrylate ultraviolet absorbers.

[0033] Based on the second aspect of the present invention, there is also provided a method for preparing the low smoke density and scratch-resistant polycarbonate material as described above, characterized in that it comprises the following steps:

[0034] a. Add polycarbonate resin, phosphate flame retardant, phosphorus compound modified nano MoS2 hollow material and optionally other additives into a high mixer and mix to obtain a premix; preferably, the mixing conditions in the high mixer are: stirring and mixing at 400-600 rpm for 2-4 minutes.

[0035] b. Add the premix into an extruder, melt-extrude and granulate the premix at a screw temperature of 250-280° C. and a screw speed of 300-500 rpm to obtain the polycarbonate material.

[0036] Based on the third aspect of the present invention, there is also provided an application of the low smoke density and scratch-resistant polycarbonate material as described above in rail transportation and electrical equipment.

[0037] The present invention can achieve a lower smoke density at a high flame retardant level of polycarbonate through the coordinated coordination of multiple components, while having improved scratch resistance, and can meet the requirements of polycarbonate products such as automobiles and home appliances for low smoke density and high scratch resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 TEM image of phosphorus compound modified nano-MoS2 hollow material A prepared in Example 1.

[0039] Figure 2 TEM image of phosphorus compound modified nano-MoS2 material D prepared in Comparative Example 1. DETAILED DESCRIPTION

[0040] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.

[0041] The main raw material information involved in the following examples of the present invention is shown in Table 1:

[0042] Table 1. Main raw material information

[0043] raw material Key Information factory Polycarbonate A1105 Molecular weight 28000 Wanhua Chemical Group Co., Ltd. Polycarbonate A1030 Molecular weight 37000 Wanhua Chemical Group Co., Ltd. Bisphenol A-bis(diphenyl phosphate) (BDP) 99% Zhejiang Wansheng Co., Ltd. Triphenyl phosphate (TPP) 99% Zhangjiagang Fengtong Chemical Co., Ltd. Resorcinol bis(diphenyl phosphate)(RDP) 99% AVIC New Materials (Shandong) Co., Ltd. Ammonium molybdate 99.9% Aladdin Thiourea 99% Aladdin Hydroxylamine hydrochloride 98% Aladdin Anhydrous ethanol AR Aladdin Dilute hydrochloric acid 2mol / L Aladdin n-Butyllithium in hexane 15% Aladdin Anhydrous lithium hydroxide 99% Aladdin Ethylene glycol 99% Aladdin Surfactant F127 / Sigma-Aldrich Benzyltriethylammonium chloride 99% Beijing Inotech Technology Co., Ltd. (4-Carboxybutyl)triphenylphosphonium bromide 98% Aladdin Melamine Phosphate ≥99% Aladdin Butyltriphenylphosphonium bromide 98% Beijing Inotech Technology Co., Ltd. Tetradecyltriphenylphosphonium bromide 97% alpha <![CDATA[MoS2]]> 98% Beijing Inotech Technology Co., Ltd. paraffin Licowax E Clariant Antioxidant 1010 / Tianjin Lianlong Antioxidant 1076 / Tianjin Lianlong UV326 / Tianjin Lianlong

[0044] Unless otherwise specified, other raw materials and reagents were purchased from commercial products.

[0045] The product performance testing method prepared by the present invention is as follows:

[0046] ①UL94 vertical combustion test: The material is injection molded into 130mm×13mm×1.5mm specimens and tested in a horizontal vertical combustion box, referring to UL94-2022.

[0047] ② Smoke density test: The material is injection molded into a 75mm×75mm×3.0mm sample and tested in a smoke density box with a radiant heat source of 50kw / m 2 , flameless conditions, record the smoke density data at the 4th minute and the maximum smoke density data during the entire test time. The entire test time is 10 minutes; refer to ISO 5659-2:2017.

[0048] ③ Simply supported beam notched impact strength test: The material is injection molded into 80mm×10mm×4mm specimens, and the simply supported beam notch is washed out using a notch sample making machine. The specimen is conditioned in a -30℃ refrigerator for at least 24h, and tested on a universal material testing machine within 10s after being taken out; refer to ISO 180:2019.

[0049] ④Tensile strength test: The material is injection molded into 1A type specimens, and after modulation, it is tested on a universal material testing machine at a tensile speed of 1.0mm / min; refer to ISO 527-2:2012.

[0050] ⑤ Flexural modulus test: The material was injection molded into 80mm×10mm×4mm strips, and after modulation, tested on a universal material testing machine at a bending speed of 2.0mm / min; refer to ISO 178:2019.

[0051] ⑥ Scratch resistance test: The material is injection molded into a 60mm×100mm×3mm leather grain sample plate, and tested on a cross scratch tester after modulation. The test conditions are 1mm scratch head, 10N load, 1000mm / min speed, 20mm×2 grids, and a portable spectrophotometer is used to test the change in brightness (L*) before and after scratching, marked as dL*; refer to PV3952.

[0052] [Preparation Example 1] Preparation of phosphorus compound modified nano MoS2 hollow material A

[0053] (1) At room temperature, weigh 161g F127 and dissolve it in 700mL deionized water. Weigh 14g thiourea, 7.25g hydroxylamine hydrochloride, and 8.8g ammonium molybdate and add them to the deionized water. After complete dissolution, adjust the pH value to about 6 with 2mol / L HCl. After stirring for 30 minutes, transfer the solution to a 1000mL polytetrafluoroethylene reactor and react at 180℃ for 24h under sealed conditions. Then cool it to room temperature naturally, centrifuge, collect the black precipitate, and wash it with deionized water and anhydrous ethanol for several times to remove impurities. The product is vacuum dried at 80℃ for 10h to obtain a black powder as nano MoS2 hollow microspheres.

[0054] (2) 14 g of nano-MoS2 hollow microspheres and 250 mL of 15% n-butyl lithium n-hexane solution were added to a 500 mL reactor, reacted at 90° C. for 4 h, centrifuged, washed to obtain a solid product and dried to obtain intercalated MoS2 hollow microspheres.

[0055] (3) Weigh 10g of intercalated MoS2 hollow microspheres and add them to 1000mL of deionized water for ultrasonic hydrolysis to obtain a suspension of intercalated MoS2 hollow microspheres with surface electronegativity. Dissolve 90g (4-carboxybutyl) triphenylphosphine (TPP) in 500ml of deionized water and stir to form a transparent solution of phosphorus-containing compounds. After mixing the suspension and the transparent solution, ultrasonic treatment was performed at room temperature for 30 minutes. The dispersion was centrifuged, the product was washed several times with anhydrous ethanol, and vacuum dried at 60°C for 12h to obtain a phosphorus-modified nano-MoS2 hollow material.

[0056] The TEM image of the phosphorus compound modified nano MoS2 hollow material prepared in this embodiment is as follows: Figure 1 As shown, it can be clearly seen that the nano-ions are hollow and similar to a core-shell structure.

[0057] [Preparation Example 2] Preparation of phosphorus compound modified nano MoS2 hollow material B

[0058] (1) At room temperature, weigh 1.03g of benzyltriethylammonium chloride and dissolve it in 600mL of deionized water. Weigh 7g of thiourea, 3.3g of hydroxylamine hydrochloride and 8.8g of ammonium molybdate and dissolve them in the above deionized water. After they are completely dissolved, adjust the pH value to about 5.5 with 2mol / L HCl. Transfer the solution to a 1000mL polytetrafluoroethylene reactor and react at 200℃ for 30h under sealed conditions. Then cool it naturally to room temperature, centrifuge it, collect the black precipitate, and wash it with deionized water and anhydrous ethanol for many times to remove impurities. Dry the product in vacuum at 80℃ for 10h to obtain a black powder as nano MoS2 hollow microspheres.

[0059] (2) 14 g of nano-MoS2 hollow microspheres, 14 g of lithium hydroxide and 400 mL of ethylene glycol were added to a 500 mL reactor, reacted at 30 °C for 6 h, centrifuged, washed to obtain a solid product and dried to obtain intercalated MoS2 hollow microspheres.

[0060] (3) Weigh 10g of intercalated MoS2 hollow microspheres and add them to 1000mL of deionized water for ultrasonic hydrolysis to obtain a suspension of intercalated MoS2 hollow microspheres with surface electronegativity. Dissolve 10g of melamine phosphate in 500ml of deionized water and stir to form a transparent solution of phosphorus-containing compounds. After mixing the suspension and the transparent solution, ultrasonic treatment was performed at room temperature for 30 minutes. The dispersion was centrifuged, the product was washed several times with anhydrous ethanol, and vacuum dried at 60°C for 12h to obtain phosphorus compound-modified nano MoS2 hollow material B.

[0061] [Preparation Example 3] Preparation of phosphorus compound modified nano MoS2 hollow material C

[0062] (1) At room temperature, weigh 5.15g of benzyltriethylammonium chloride and dissolve it in 600mL of deionized water. Weigh 20.5g of thiourea, 12.5g of hydroxylamine hydrochloride and 8.8g of ammonium molybdate and dissolve them in the above deionized water. After they are completely dissolved, adjust the pH value to about 6.5 with 2mol / L HCl. Transfer the solution to a 1000mL polytetrafluoroethylene reactor and react at 210℃ for 24h under sealed conditions. Then cool it naturally to room temperature, centrifuge it, collect the black precipitate, and wash it with deionized water and anhydrous ethanol for many times to remove impurities. Dry the product in vacuum at 80℃ for 10h to obtain a black powder as nano MoS2 hollow microspheres.

[0063] (2) 14 g of nano-MoS2 hollow microspheres, 28 g of lithium hydroxide and 400 mL of ethylene glycol were added to a 500 mL reactor, reacted at 100 °C for 2 h, centrifuged, washed to obtain a solid product and dried to obtain intercalated MoS2 hollow microspheres.

[0064] (3) Weigh 10g of intercalated MoS2 hollow microspheres and add them to 1000mL of deionized water for ultrasonic hydrolysis to obtain a suspension of intercalated MoS2 hollow microspheres with surface electronegativity. Dissolve 50g of butyl triphenyl phosphonium bromide and 50g of tetradecyl triphenyl phosphonium bromide in 800ml of deionized water and stir to form a transparent solution of phosphorus-containing compounds. After mixing the suspension and the transparent solution, ultrasonic treatment was performed at room temperature for 30 minutes. The dispersion was centrifuged, the product was washed several times with anhydrous ethanol, and vacuum dried at 60°C for 12h to obtain phosphorus compound-modified nano MoS2 hollow material C.

[0065] [Comparative Example 1] Preparation of phosphorus compound modified nano MoS2 material D

[0066] (1) Weigh 14 g of nano-MoS2 and 14 g of lithium hydroxide, add 400 mL of ethylene glycol into a 500 mL reactor, react at 30 ° C for 6 h, centrifuge, wash to obtain a solid product and dry it to obtain intercalated MoS2.

[0067] (2) Weigh 10g of intercalated MoS2 and add it to 1000mL of deionized water for ultrasonic hydrolysis to obtain an intercalated MoS2 suspension with surface electronegativity. Dissolve 10g of melamine phosphate in 500ml of deionized water and stir to form a transparent solution of phosphorus-containing compound. After mixing the suspension and the transparent solution, ultrasonic treatment was performed at room temperature for 30 minutes. The dispersion was centrifuged, the product was washed several times with anhydrous ethanol, and vacuum dried at 60°C for 12h to obtain phosphorus compound-modified nanomaterial D.

[0068] The TEM image of the phosphorus compound modified nano MoS2 material D prepared in this comparative example is as follows: Figure 2 As shown, it can be seen that the nano-ions are opaque solid structures.

[0069] [Example 1]

[0070] In parts by weight, the raw materials of polycarbonate material are prepared according to the following formula:

[0071]

[0072] The above raw material components are added into a high-speed mixer, mixed at 500 rpm for 3 minutes to obtain a premix; the premix is ​​added into a twin-screw extruder, melt-extruded and granulated at a screw temperature of 250-260°C for zone 1, 260-270°C for zone 2, 270-280°C for zone 3, and a rotation speed of 400 rpm to obtain a polycarbonate material.

[0073] [Example 2-6]

[0074] Different polycarbonate materials were prepared by referring to the process in Example 1 and the raw material components shown in Table 2.

[0075] Table 2. Raw material components and contents in each example (parts)

[0076]

[0077] [Comparative Example 1]

[0078] The polycarbonate material was prepared in substantially the same manner as in Example 1, except that the raw material did not contain the phosphorus compound-modified nano-MoS2 hollow material A.

[0079] [Comparative Example 2]

[0080] The polycarbonate material was prepared in substantially the same manner as in Example 1, except that the phosphorus compound-modified nano-MoS2 hollow material A in the raw material was replaced with the nano-MoS2 hollow microspheres provided in Preparation Example 1 in an equal amount.

[0081] [Comparative Example 3]

[0082] The polycarbonate material was prepared in substantially the same manner as in Example 1, except that the phosphorus compound-modified nano-MoS2 hollow material A in the raw material was replaced with the phosphorus compound-modified nano-MoS2 material D in the same mass fraction.

[0083] [Comparative Example 4]

[0084] The polycarbonate material was prepared in substantially the same manner as in Example 1, except that the raw material did not contain BDP.

[0085] The polycarbonate materials prepared in the embodiments and comparative examples were placed at a temperature of 23±2° C. and a humidity of 50±5% for 48 hours, and the performance tests in Table 3 were performed. The test results are shown in Table 3.

[0086] From the performance tests of comparative examples 1-6 and comparative examples 1-4, it can be seen that the addition of phosphorus-containing compounds to modify the nano MoS2 hollow material in the present invention can ensure the excellent mechanical properties of the material while achieving the flame retardant effect of the UL94 standard V0 level, and at the same time achieve the effects of low smoke density Ds4 (<300) and high scratch resistance (dL*<1.5).

[0087] Table 3. Performance test results

[0088]

Claims

1. A low smoke density, scratch-resistant polycarbonate material, characterized in that: The invention comprises the following raw materials in parts by weight: The phosphorus compound modified nano MoS2 hollow material is prepared by the following method: 1) dissolving ammonium molybdate, thiourea, hydroxylamine hydrochloride and surfactant in water, adjusting the pH to 5-6.5 and transferring to a polytetrafluoroethylene reactor, reacting at 140-200° C. for at least 24 hours, cooling to room temperature and filtering, washing and drying to obtain a solid product, i.e., nano-MoS2 hollow microspheres; 2) mixing the solid product obtained in step 1) and the intercalation agent in a solvent, reacting at 25-100° C. for 2-6 hours, filtering, washing, and drying to obtain intercalated MoS2 hollow microspheres; 3) adding the intercalated MoS2 hollow microspheres into water and performing ultrasonic dispersion to obtain a suspension of intercalated MoS2 hollow microspheres with surface electronegativity; The phosphorus compound solution is added to the above suspension, ultrasonically mixed for 5-100 minutes at room temperature, filtered, washed and dried to obtain a phosphorus compound modified nano MoS2 hollow material.

2. The low smoke density, scratch-resistant polycarbonate material according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight:

3. The low smoke density, scratch-resistant polycarbonate material according to claim 1, characterized in that: The polycarbonate resin is a linear bisphenol A type aromatic polycarbonate with a weight average molecular weight of 20,000-40,000.

4. The low smoke density, scratch-resistant polycarbonate material according to any one of claims 1 to 3, characterized in that: The phosphate flame retardant is one or more of triphenyl phosphate, polybisphenol A-bis(diphenyl phosphate), and resorcinol bis(diphenyl phosphate).

5. The low smoke density, scratch-resistant polycarbonate material according to any one of claims 1 to 3, characterized in that: In step 1), the raw materials are transferred to a polytetrafluoroethylene reactor and reacted at a constant temperature of 190-210° C. for 24-30 hours.

6. The low smoke density, scratch-resistant polycarbonate material according to claim 1, characterized in that: In step 1), the molar ratio of ammonium molybdate, thiourea and hydroxylamine hydrochloride is 1:(2-6):(1-4).

7. The low smoke density, scratch-resistant polycarbonate material according to claim 6, characterized in that: In step 1), the surfactant is selected from nonionic surfactants and / or cationic surfactants.

8. The low smoke density, scratch-resistant polycarbonate material according to claim 7, characterized in that: The nonionic surfactant is selected from one or more of F127, F108, and P123.

9. The low smoke density, scratch-resistant polycarbonate material according to claim 7, characterized in that: The cationic surfactant is selected from one or more of benzyltriethylammonium chloride, octadecyldimethyl tertiary amine, and dodecyldimethylbenzylammonium bromide.

10. The low smoke density, scratch-resistant polycarbonate material according to claim 6, characterized in that: The amount of the surfactant used is 0.1-0.5 times the molar amount of ammonium molybdate.

11. The low smoke density, scratch-resistant polycarbonate material according to claim 6, characterized in that: Step 1) pH is adjusted using 0.5-2 mol / L hydrochloric acid.

12. The low smoke density, scratch-resistant polycarbonate material according to claim 1, characterized in that: In step 2), the intercalant is at least one of n-butyl lithium and lithium hydride.

13. The low smoke density, scratch resistant polycarbonate material according to claim 12, characterized in that: The amount of the intercalant used is 1-3 times the mass of the solid product obtained in step 1).

14. The low smoke density, scratch resistant polycarbonate material according to claim 1, characterized in that: In step 3), the phosphorus-containing compound is one or more of (4-carboxybutyl)triphenylphosphonium bromide, melamine phosphate, butyltriphenylphosphonium bromide, and tetradecyltriphenylphosphonium bromide.

15. The low smoke density, scratch resistant polycarbonate material according to claim 14, characterized in that: The mass ratio of phosphorus-containing compound to intercalated MoS2 hollow microspheres is (1-10):

1.

16. The low smoke density, scratch-resistant polycarbonate material according to any one of claims 1 to 3, characterized in that: The other auxiliary agent is optionally at least one of a lubricant, an antioxidant, and a light stabilizer.

17. A method for preparing a low smoke density, scratch-resistant polycarbonate material according to any one of claims 1 to 16, characterized in that: The following steps are involved: a. Add polycarbonate resin, phosphate flame retardant, phosphorus compound modified nano MoS2 hollow material, and optionally other additives into a high-speed mixer to obtain a premix; b. Add the premix into an extruder, melt-extrude and granulate the premix at a screw temperature of 250-280° C. and a screw speed of 300-500 rpm to obtain the polycarbonate material.

18. Use of the low smoke density and scratch-resistant polycarbonate material according to any one of claims 1 to 16 in rail transportation and electrical equipment.

Citation Information

Patent Citations

  • Train interior components with low smoke and low heat release and their manufacturing methods

    CN105849171B

  • Applications of polycarbonate compositions and sulfonates and phosphorus-containing compounds in reducing polycarbonate smoke and heat release

    CN109777073B

  • Architectural high-insulativity low-smoke halogen-free flame-retardant cable material and preparation method thereof

    CN104945749A

  • Preparation method and application of hollow MoS2 microspheres

    CN109650450A