A method for separating thallium based on sodium carbonate
By adding sodium carbonate to thallium-containing solid waste and performing roasting treatment, the problem of difficulty in thallium separation in the existing technology is solved, efficient thallium separation and resource reuse are achieved, and environmental risks and processing costs are reduced.
Patent Information
- Application Number
- CN202310193061.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-02
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-03-02
AI Technical Summary
The existing technology has the problems of cumbersome operation steps, high equipment requirements and poor applicability in separating thallium from solid waste containing thallium, which makes the separation of thallium difficult.
Using a thallium separation method based on sodium carbonate, the ground thallium-containing solid waste is mixed with sodium carbonate and then roasted. The roasting temperature is controlled at 750-850°C and the duration is not less than 1 hour. The reaction between sodium carbonate and zinc sulfate is used to achieve thallium Selective volatilization and separation.
It improves the separation selectivity of thallium and reduces the processing cost. The thallium-removed residue obtained after separation can be used for secondary utilization, reducing environmental risks and realizing the reuse of thallium resources.
Smart Images

Figure CN116287729B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the treatment of solid waste, and in particular to a thallium separation method based on sodium carbonate. Background Art
[0002] Thallium is a typical rare dispersed element in nature, widely found in primary metal ores. Thallium has many characteristics such as improving alloy strength, improving alloy hardness, and enhancing alloy corrosion resistance. Thallium-containing alloys have potential application value in optical fibers, superconducting materials, infrared optical materials, radiation shielding materials, catalysts, etc. However, the global annual usage of thallium is less than 30 tons, resulting in a lack of enthusiasm among thallium production companies.
[0003] Although there is a large amount of thallium in thallium-containing solid waste, the existing technology for separation and enrichment of thallium is still insufficient and needs to be optimized. For example, the Chinese invention patent with the authorization announcement number CN101314823B discloses a method for extracting metallic thallium from thallium-containing slag, which uses vacuum metallurgy to extract thallium from thallium-containing waste slag. Although the extraction rate of thallium is high, it requires three-stage evaporation separation, which has cumbersome operating steps, high equipment requirements and poor applicability, making it difficult to separate thallium from thallium-containing solid waste.
[0004] In view of this, it is necessary to provide a thallium separation method based on sodium carbonate to solve or alleviate the above-mentioned technical defect that it is difficult to separate thallium from thallium-containing solid waste. Summary of the invention
[0005] The main purpose of the present invention is to provide a thallium separation method based on sodium carbonate, aiming to solve the above-mentioned technical problem that it is difficult to separate thallium from thallium-containing solid waste.
[0006] To achieve the above object, the present invention provides a thallium separation method based on sodium carbonate, comprising the steps of:
[0007] S1, mixing the ground thallium-containing solid waste and sodium carbonate to obtain a mixture to be burned;
[0008] Wherein, the thallium-containing solid waste includes zinc sulfate;
[0009] S2, calcining the mixture to be calcined to obtain thallium-containing volatiles and thallium-free slag;
[0010] The temperature of the calcination treatment is 750-850°C, and the duration of the calcination treatment is not less than 1 hour.
[0011] Furthermore, the thallium-containing solid waste includes thallium-containing smoke generated during zinc smelting.
[0012] Furthermore, the content of thallium in the thallium-containing smoke is 0.5-0.7wt%.
[0013] Furthermore, the particle size of the thallium-containing solid waste after the grinding is no more than 100 meshes.
[0014] Furthermore, the thallium-containing solid waste also includes valuable metal fluorine-chloride compounds, and the valuable metal fluorine-chloride compounds include one or more of lead fluorine-chloride compounds, zinc fluorine-chloride compounds and cadmium fluorine-chloride compounds.
[0015] Furthermore, the mass proportion of the sodium carbonate in the mixture to be burned is not less than 10%.
[0016] Furthermore, the step S1 further comprises: before grinding the thallium-containing solid waste, drying the thallium-containing solid waste.
[0017] Furthermore, in the step S1, the mixing process includes: grinding the ground product and the sodium carbonate together to obtain a primary mixture; and then oscillating the primary mixture to obtain the mixture to be burned.
[0018] Furthermore, the calcination treatment takes 1-3 hours.
[0019] Furthermore, the calcination process is performed in an air atmosphere or an inert atmosphere.
[0020] Compared with the prior art, the present invention has at least the following advantages:
[0021] The present invention provides a thallium separation method based on sodium carbonate. By utilizing zinc sulfate and valuable metal fluorine and chlorine compounds present in thallium-containing solid waste and introducing sodium carbonate, the effective separation of thallium from thallium-containing solid waste and the reuse of thallium resources are achieved; by controlling the roasting temperature, the separation of thallium is further ensured, and the selectivity of thallium separation is improved. Compared with other treatment methods, the treatment cost of the present invention is low, and the selective separation efficiency of thallium is high; the thallium-free slag obtained after separation can be returned to the lead-zinc smelting system for secondary utilization, which greatly reduces the environmental risk of thallium-containing solid waste while ensuring the recovery of thallium. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0023] Figure 1 is the XRD diagram of the thallium-containing soot in Example 1 of the present invention;
[0024] Figure 2 The chemical phase analysis results of water-soluble zinc and oxidized zinc as the roasting temperature changes in Example 2 of the present invention, and the variation law diagram of thallium volatility;
[0025] Figure 3 The chemical phase analysis results of lead chloride, lead sulfate and lead oxidation as the roasting temperature changes in Example 2 of the present invention, and the variation regularity diagram of thallium volatilization rate;
[0026] Figure 4 The chemical phase analysis results of water-soluble zinc and oxidized zinc as the oxygen concentration changes in Example 3 of the present invention, and the variation law diagram of thallium volatility;
[0027] Figure 5 The chemical phase analysis results of lead chloride, lead sulfate and lead oxidation as the oxygen concentration changes in Example 3 of the present invention, and the variation law of thallium volatilization rate are shown.
[0028] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0031] At present, smelting enterprises are faced with the problems of high pollution, high disposal costs and selective separation and recovery of thallium in slag caused by thallium-containing solid waste. However, the existing technology for the treatment of thallium-containing solid waste is not fully suitable for industrial applications, and is not very targeted for specific thallium-containing solid waste (the existing treatment of thallium-containing waste slag does not involve thallium-containing smoke).
[0032] Based on this, in order to achieve the selective separation of thallium from thallium-containing solid waste under the premise of being applicable to industrial applications, complete the enrichment of thallium and the harmlessness and resource utilization of roasted materials, the present invention provides a thallium separation method based on sodium carbonate, comprising the steps of:
[0033] S1, grinding the thallium-containing solid waste to obtain a grinding product; mixing the ground thallium-containing solid waste (grinding product) with sodium carbonate to obtain a mixture to be burned.
[0034] The grinding product may be in granular form. For example, the particle size of the thallium-containing solid waste after grinding may be no larger than 100 mesh, that is, the particle size of the grinding product may be no larger than 100 mesh, specifically 100-400 mesh.
[0035] The thallium-containing solid waste contains thallium element; the thallium-containing solid waste may also contain one or more of lead element, zinc element and cadmium element.
[0036] In terms of specific phase types, the thallium-containing solid waste includes zinc sulfate, and the zinc sulfate contains thallium element, that is, the thallium-containing phase includes or is the zinc sulfate; the thallium-containing solid waste may also include one or more of lead sulfate and cadmium sulfate.
[0037] Furthermore, the thallium-containing solid waste may also include valuable metal fluorine and chlorine compounds; and the thallium-containing solid waste may also include valuable metal oxides. It should be noted that the valuable metal in the present invention refers to other metals except thallium.
[0038] The valuable metal fluorine-chloride compound may include or be one or more of lead fluorine-chloride compounds, zinc fluorine-chloride compounds and cadmium fluorine-chloride compounds; the fluorine-chloride compound may contain one or both of fluorine and chlorine, or may contain both fluorine and chlorine. The metal oxide may include or be one or more of lead oxide, zinc oxide and cadmium oxide.
[0039] The thallium-containing solid waste may specifically include or be thallium-containing smoke generated during zinc smelting. The thallium-containing smoke may include or be thallium-containing high-fluorine and chlorine smoke. The thallium content in the thallium-containing high-fluorine and chlorine smoke (thallium-containing smoke) may be 0.5-0.7wt%, usually 0.6-0.7wt%. The thallium in the thallium-containing high-fluorine and chlorine smoke is basically present in zinc sulfate. The thallium element in the thallium-containing high-fluorine and chlorine smoke includes or is monovalent thallium.
[0040] It should be noted that when the thallium-containing high-fluorine and chlorine smoke or other waste contains thallium in other valence states, it does not affect the implementation of the present application.
[0041] In order to facilitate the treatment of the thallium-containing solid waste, the step S1 may further include: before grinding the thallium-containing solid waste, drying the thallium-containing solid waste to a constant weight; the drying temperature may be 60-100°C, such as 80°C.
[0042] In order to ensure the release of thallium and the conversion of valuable metals, the mass proportion of the sodium carbonate in the mixture to be burned may be no less than 10%, and illustratively, may be 10-20%.
[0043] In order to ensure sufficient contact between the thallium-containing solid waste and the sodium carbonate, in step S2, the mixing process includes: grinding the ground product and sodium carbonate together to obtain a primary mixture; then, oscillating the primary mixture to obtain the mixture to be burned. The particle size standard of the primary mixture can be consistent with that of the ground product, and the oscillation time can be no less than 0.5h, preferably 0.5-3h.
[0044] S3, roasting the mixture to be calcined to obtain separated thallium-containing volatiles and thallium-free slag (roasted slag). Specifically, during the roasting process, the thallium-containing volatiles generated in the roasting process can be collected synchronously to recover the separated thallium.
[0045] The collection process may be: conveying the volatiles to a condenser or other condensation device to condense the volatiles, thereby obtaining thallium-containing recovered materials.
[0046] In order to ensure the selective separation of thallium, the temperature of the roasting treatment is 750-850°C, preferably 800°C, and the duration of the roasting treatment is not less than 1 hour, preferably 1-3 hours. In addition, the roasting treatment is generally carried out in a furnace body, and the temperature increase of the mixture to be fired and the temperature decrease of the residue can be carried out in a furnace-related manner.
[0047] In order to ensure the progress of the reaction during the calcination process, the calcination treatment cannot be carried out in a reducing atmosphere, and the calcination treatment can usually be carried out in an air atmosphere or an inert atmosphere.
[0048] The main principles of the present invention include:
[0049] In order to achieve the selective volatilization of thallium, the volatilization conditions of thallium compounds must be met in thermodynamics and kinetics, that is, the critical temperature for the volatilization of thallium-containing compounds must be reached, and at the same time, the thallium contained in other compounds must be released. Therefore, it is necessary to regulate the reaction, roasting temperature and roasting time in the thallium-containing smoke, and control the relevant conditions and parameters to achieve the selective volatilization of thallium.
[0050] 1. The main reasons why the additive is sodium carbonate include:
[0051] 1) There is a strong correlation between the thallium in the thallium-containing high-fluorine and chlorine smoke (thallium-containing solid waste) and the zinc sulfate phase. The release and selective volatilization of thallium can be achieved by destroying the zinc sulfate structure. Sodium carbonate can react with zinc sulfate phase to convert into zinc carbonate, zinc oxide and sodium sulfate, thus achieving the release of thallium.
[0052] Although other substances may also exist in the thallium-containing high-fluorine and chlorine smoke, since zinc sulfate has a strong correlation with the thallium in the thallium-containing smoke (zinc sulfate and thallium), the thallium in the thallium-containing high-fluorine and chlorine smoke is basically stored in zinc sulfate. Therefore, zinc sulfate needs to be converted to efficiently release thallium.
[0053] 2) Valuable metal fluorine and chlorine compounds have a low volatility point. Sodium carbonate can react with valuable metal fluorine and chlorine compounds to convert them into oxides and carbonates, thereby reducing the volatility of valuable metals during the roasting process.
[0054] 2. The main reasons why the present invention determines the roasting temperature to be about 800°C include:
[0055] 1) After adding sodium carbonate, valuable metals such as lead, zinc and cadmium are converted into carbonates, partially decomposed into oxides at high temperatures, and begin to volatilize in large quantities when the temperature is higher than 800°C (the specific volatilization effect is subject to the embodiment and comparative example).
[0056] 2) The degree of reaction between sodium carbonate and zinc sulfate is controlled by kinetics, and the reaction is almost complete at 800°C.
[0057] In order to facilitate those skilled in the art to understand the present invention in detail, examples are given below:
[0058] Example 1
[0059] Sampling and Analysis of Thallium-Containing Dust
[0060] Take the thallium-containing high-fluorine and chlorine smoke (thallium-containing smoke) generated in the zinc smelting process, dry (80°C forced air drying oven) to constant weight and then grind (grind until it can pass through a 100-mesh sieve), digest the ground thallium-containing smoke, measure the element content in the thallium-containing smoke, and perform phase analysis.
[0061] In this embodiment, the thallium content in the thallium-containing smoke was measured to be 0.66wt%. It should be noted that the thallium element is unevenly distributed in the thallium-containing high-fluorine and chlorine smoke, and the thallium content of the smoke as a whole is between 0.6 and 0.7wt%. The volatilization rate of thallium in the subsequent embodiments and comparative examples is calculated based on the content obtained by this digestion.
[0062] The specific analysis results are as follows:
[0063] 1. See Figure 1 According to the chemical phase analysis, in this embodiment, the main phases of the thallium-containing smoke include zinc oxide, lead oxide, zinc sulfate (water-soluble zinc), lead sulfate, lead chloride, and zinc chloride, and the existing forms include crystalline and amorphous states.
[0064] 2. In this embodiment, the mass percentages of the main elements in the thallium-containing smoke are shown in the following table:
[0065] element Zn Pb S Cd Fe F Tl Cl O content(%) 38.1 17.75 6.135 1.98 3.22 0.93 0.66 4.87 22.5
[0066] It can be seen from the above table that thallium-containing smoke mainly contains valuable metal elements such as Zn and Pb.
[0067] 3. In this embodiment, the chemical phase analysis results (mass percentage) of Zn are shown in the following table:
[0068]
[0069] 4. In this embodiment, the chemical phase analysis results (mass percentage) of Pb are shown in the following table:
[0070]
[0071] Example 2
[0072] Temperature single factor test
[0073] Take 1 kg of a sample of thallium-containing smoke (same as in Example 1) dried (in a blast drying oven at 80° C.) to constant weight and grind it (grind until it can pass through a 100-mesh sieve) to obtain a grinding product.
[0074] The ground products were calcined at temperatures of 600°C, 700°C, 800°C, 900°C, 1000°C and 1100°C, respectively.
[0075] The process of each roasting is as follows: 15 g of the ground product is placed in a vertical tube furnace for roasting under air atmosphere; the temperature of each roasting is controlled to be the above-mentioned temperatures, the insulation time of each roasting is 1 hour, and after roasting, the roasted slag is cooled to room temperature along with the furnace.
[0076] In this embodiment, the chemical phase analysis results of the water-soluble zinc and oxidized zinc in the roasted slag as a function of the roasting temperature (the mass proportion in the roasted slag), and the variation law of the thallium volatility (as a function of the roasting temperature) are all referred to Figure 2 shown.
[0077] The chemical phase analysis results of lead chloride, lead sulfate and lead oxide in the roasted slag (mass proportion in the roasted slag) and the variation law of thallium volatility (varies with roasting temperature) are shown in Figure 3 shown.
[0078] Example 3
[0079] Oxygen concentration single factor experiment
[0080] Take 1 kg of a sample of thallium-containing smoke (same as in Example 1) dried (in a blast drying oven at 80° C.) to constant weight and grind it (grind until it can pass through a 100-mesh sieve) to obtain a grinding product.
[0081] The ground products were calcined at oxygen concentrations of 0%, 10%, 20%, 30%, 40% and 50%, respectively.
[0082] Each roasting process is as follows: 15 g of the ground product is roasted in a vertical tube furnace under the above oxygen concentration; the roasting temperature is controlled to be 900° C., the holding time for each roasting is 1 hour, and after roasting, the roasted slag is cooled to room temperature along with the furnace.
[0083] In this embodiment, the chemical phase analysis results of the water-soluble zinc and oxidized zinc in the roasted slag as a function of oxygen concentration (mass proportion in the roasted slag), and the variation law of the thallium volatilization rate (as a function of oxygen concentration) are all referred to Figure 4 shown.
[0084] The chemical phase analysis results of the change of lead chloride, lead sulfate and lead oxide in the roasted slag with oxygen concentration (mass proportion in the roasted slag), and the change law of thallium volatility (change with oxygen concentration) are shown in Figure 5 shown.
[0085] Example 4
[0086] Water immersion test
[0087] Take 1 kg of a sample of thallium-containing smoke (same as in Example 1) dried (in a blast drying oven at 80° C.) to constant weight and grind it (grind until it can pass through a 100-mesh sieve) to obtain a grinding product.
[0088] Weigh 0.2000 g of the ground product and place it in a centrifuge tube. Add 50 ml of deionized water to the centrifuge tube, place it in a water bath shaker (150 r / min) at room temperature and shake for 2 hours. Take it out and centrifuge it to separate the solid and liquid. Take the supernatant to test the thallium and zinc content.
[0089] The leaching rate is calculated by combining the two. The mass leaching rate is shown in the following table:
[0090] Thallium leaching rate (%) Water-soluble zinc leaching rate (%) 98.61 100
[0091] Analysis example 1
[0092] Combined with Examples 1-4, the presence of thallium was analyzed
[0093] 1. See Figure 2-5 It can be seen that in the analytical test results of the two groups of single-factor experiments, the thallium volatilization rate showed a significant correlation with the zinc-containing phase, but a weaker correlation with the lead-containing phase, and the regularity was not obvious. Therefore, it is speculated that there is a certain correlation between the occurrence of thallium and the zinc-containing phase.
[0094] For further details, see Figure 2 As the temperature increases, the water-soluble zinc phase decreases, the oxidized zinc phase increases, and the thallium volatilization rate increases. It is speculated that during the heating process, the water-soluble zinc phase is transformed into the oxidized zinc phase and thallium is released at the same time.
[0095] See Figure 4 In the single-factor experiment of oxygen concentration, the water-soluble zinc phase first increased and then decreased, while the oxidized zinc phase and thallium volatilization first decreased and then increased. It is also speculated that this is caused by the mutual transformation between the water-soluble zinc phase and the oxidized zinc phase.
[0096] Combined with the data from the water immersion experiment, it can be seen that during the water immersion process, the water-soluble zinc is completely dissolved, and the thallium is almost completely dissolved. Analysis shows that since the physical structure of the water-soluble zinc is destroyed during the water immersion process, the thallium contained in it is released, resulting in the simultaneous dissolution of both.
[0097] Since there is a strong correlation between the dissolution relationship of water-soluble zinc and thallium, as well as the change law during the roasting process, it is believed that there is a strong correlation between the occurrence of thallium and the water-soluble zinc phase.
[0098] 2. Combined with the main elements involved in thallium-containing dust, the water-soluble zinc involved in the present invention should be zinc chloride and zinc sulfate. Among them, the volatilization temperature of zinc chloride is relatively low (it will volatilize significantly at about 500°C), and the decomposition temperature of zinc sulfate is relatively high (it will start to dissociate at 500-600°C and will dissociate violently at about 930°C).
[0099] In the temperature single-factor experiment, as the temperature increases, the water-soluble zinc phase continues to decrease after exceeding 500°C, and the water-soluble zinc phase decreases significantly in the range of 900-1000°C (the violent dissociation temperature of zinc sulfate), while the thallium volatilization rate increases significantly.
[0100] Therefore, it is believed that the occurrence of thallium is correlated with the zinc sulfate phase, and the occurrence phase of thallium in thallium-containing smoke is zinc sulfate.
[0101] Example 5
[0102] Take 1 kg of a sample of thallium-containing smoke (same as in Example 1) dried (in a blast drying oven at 80° C.) to constant weight and grind it (grind until it can pass through a 100-mesh sieve) to obtain a grinding product.
[0103] Weigh 13.5 g of the ground product (thallium-containing smoke after grinding) and 1.5 g of sodium carbonate, add the weighed ground product and sodium carbonate into a mortar and grind and mix to obtain a primary mixture (the primary mixture can pass a 100-mesh sieve); put the primary mixture into a plastic bottle with a cover, place it on a tumbling oscillator (30 r / min) and oscillate for 2 hours to obtain a mixture to be burned.
[0104] The obtained mixture to be sintered is placed in a corundum crucible and sintered in a vertical tube furnace under air atmosphere. During the sintering process, the sintering temperature is controlled to be 800°C and the holding time is 1 hour; after sintering, the slag is cooled to room temperature along with the furnace.
[0105] The roasted residue is digested and the contents of thallium, lead, zinc and cadmium in the digestion solution are determined.
[0106] According to calculation, in this embodiment, the mass volatilization rate of thallium is 97.68%, and the mass volatilization rates of lead, zinc and cadmium are 10.98%, 2.27% and 19.69% respectively.
[0107] Example 6
[0108] Compared with Example 5, in this example, only the weighing amount of the ground product is adjusted to 12 g, and the weighing amount of sodium carbonate is adjusted to 3 g, and other conditions remain unchanged.
[0109] According to calculation, in this embodiment, the mass volatilization rate of thallium is 97.94%, and the mass volatilization rates of lead, zinc and cadmium are 10.26%, 2.13% and 18.69% respectively.
[0110] Comparative Example 1
[0111] Compared with Example 5, in this comparative example, only the calcination temperature is adjusted to 900° C., and other conditions remain unchanged.
[0112] According to calculation, in this comparative example, the mass volatilization rate of thallium is 99.76%, and the mass volatilization rates of lead, zinc and cadmium are 23.21%, 5.80% and 36.86% respectively.
[0113] Based on Comparative Example 1, it can be seen that:
[0114] When the temperature is too high, although the structure of the thallium-containing phase is destroyed and thallium is completely released, the valuable metals evaporate severely under high temperature conditions, making it impossible to achieve selective separation of thallium.
[0115] Therefore, ensuring the calcination temperature at around 800°C is critical for destroying the structure of the thallium-containing phase and achieving selective volatilization of thallium.
[0116] Comparative Example 2
[0117] Compared with Example 5, in this comparative example, only the calcination temperature is adjusted to 700° C., and other conditions remain unchanged.
[0118] According to calculation, in this comparative example, the mass volatilization rate of thallium is 75.23%, and the mass volatilization rates of lead, zinc and cadmium are 9.11%, 0.86% and 11.66% respectively.
[0119] Comparative Example 3
[0120] Compared with Example 5, in this comparative example, only the calcination temperature was adjusted to 500° C., and other conditions remained unchanged.
[0121] According to calculation, in this comparative example, the mass volatilization rate of thallium is 2.20%, and the mass volatilization rates of lead, zinc and cadmium are 0.25%, 1.83% and 5.20% respectively.
[0122] Based on Comparative Examples 2-3, it can be seen that:
[0123] When the temperature is too low, the structure of the thallium-containing phase is not destroyed and thallium cannot be completely released, resulting in a low thallium volatilization rate.
[0124] Therefore, it is necessary to ensure that the calcination temperature is around 800°C in order to destroy the structure of the thallium-containing phase and achieve the selective volatilization of thallium.
[0125] Comparative Example 4
[0126] Compared with Example 5, in this comparative example, only the weighing amount of the ground product was adjusted to 14.5 g, and the weighing amount of sodium carbonate was adjusted to 0.5 g, and other conditions remained unchanged.
[0127] According to calculation, in this comparative example, the mass volatilization rate of thallium is 31.55%, and the mass volatilization rates of lead, zinc and cadmium are 15.16%, 3.12% and 25.13% respectively.
[0128] Based on Comparative Example 4, it can be seen that:
[0129] When the addition ratio of sodium carbonate is low, the structure of the thallium-containing phase is not destroyed and thallium cannot be completely released, resulting in a low thallium volatilization rate.
[0130] Therefore, ensuring the proportion of sodium carbonate is very necessary to destroy the structure of the thallium-containing phase and achieve the selective volatilization of thallium.
[0131] Comparative Example 5
[0132] Compared with Example 5, this comparative example only replaced sodium carbonate with calcium oxide, and other conditions remained unchanged.
[0133] According to calculation, in this comparative example, the mass volatilization rate of thallium is 94.51%, and the mass volatilization rates of lead, zinc and cadmium are 3.79%, 42.12% and 32.53% respectively.
[0134] Based on Comparative Example 5, it can be seen that:
[0135] Sodium carbonate plays a unique role in the present invention. When the roasting temperature is 800° C. and sodium carbonate is replaced by calcium oxide, the volatilization rate of valuable metals will increase, thereby reducing the selectivity of thallium volatilization.
[0136] The above technical solutions of the present invention are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention specification under the technical concept of the present invention, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A thallium separation method based on sodium carbonate, characterized in that: Includes steps: S1, mixing the ground thallium-containing solid waste and sodium carbonate to obtain a mixture to be burned; Wherein, the thallium-containing solid waste includes zinc sulfate; S2, calcining the mixture to be calcined to obtain thallium-containing volatiles and thallium-free slag; The temperature of the calcination treatment is 750-850°C, and the duration of the calcination treatment is not less than 1 hour.
2. The thallium separation method based on sodium carbonate according to claim 1, characterized in that: The thallium-containing solid waste includes thallium-containing smoke generated during zinc smelting.
3. The thallium separation method based on sodium carbonate according to claim 2, characterized in that, The content of thallium in the thallium-containing smoke is 0.5-0.7wt%.
4. The thallium separation method based on sodium carbonate according to claim 1, characterized in that: The particle size of the thallium-containing solid waste after grinding is no more than 100 meshes.
5. The thallium separation method based on sodium carbonate according to claim 1, characterized in that: The thallium-containing solid waste also includes valuable metal fluorine-chloride compounds, and the valuable metal fluorine-chloride compounds include one or more of lead fluorine-chloride compounds, zinc fluorine-chloride compounds and cadmium fluorine-chloride compounds.
6. The thallium separation method based on sodium carbonate according to claim 1, characterized in that: The mass proportion of the sodium carbonate in the mixture to be burned is not less than 10%.
7. The thallium separation method based on sodium carbonate according to claim 1, characterized in that: The step S1 further includes: before grinding the thallium-containing solid waste, drying the thallium-containing solid waste.
8. The thallium separation method based on sodium carbonate according to claim 1, characterized in that: In the step S1, the mixing process includes: grinding the ground thallium-containing solid waste and the sodium carbonate together to obtain a primary mixture; and then oscillating the primary mixture to obtain the mixture to be burned.
9. The thallium separation method based on sodium carbonate according to claim 1, characterized in that: The duration of the calcination treatment is 1-3 hours.