A toughened chromium carbide-based metal ceramic and its preparation method
Composite solid solution powder generated through carbothermal reduction reaction is mixed and sintered with Ni powder, which solves the problem of grain growth and pores of Cr3C2-based cermets, achieves simultaneous improvement in strength, hardness and toughness, and significantly improves performance.
Patent Information
- Application Number
- CN202310114087.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-13
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-13
AI Technical Summary
The problems of sintering densification and abnormal grain growth of Cr3C2-based cermets have limited the improvement of its strength, hardness and toughness, and the existing technology cannot achieve simultaneous improvement.
(Cr, Ti, W) 3C2 composite solid solution powder is generated by performing a carbothermal reduction reaction between Cr2O3, TiO2, WO3 and carbon black, and is mixed with Ni powder and molding agent for granulation, pressing and sintering to form strong and tough chromium carbide. Based on cermets, it inhibits grain growth, eliminates pores, and strengthens the bonding phase.
The strength, hardness and toughness of Cr3C2-based cermets have been simultaneously improved. The flexural strength is 1378MPa, the Vickers hardness is 1273MPa, and the fracture toughness is 12.74MPa·m1/2, overcoming the lack of performance improvement in the existing technology.
Smart Images

Figure CN116287924B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hard materials, and in particular relates to a toughened chromium carbide-based metal ceramic and a preparation method thereof. Background Art
[0002] WC-based cemented carbide is widely used in cutting and mining tools due to its high hardness, high strength and good fracture toughness. However, WC-based cemented carbide has poor acid and alkali corrosion resistance and high temperature oxidation resistance, which limits its further industrial application. In addition, the gradual depletion of W resources urgently requires the development of new hard phase system metal ceramics, so the research on the performance of new metal ceramics without or with less W has attracted much attention.
[0003] Cr3C2-based cermets have a series of unique properties, such as excellent corrosion resistance and high temperature oxidation resistance, and are suitable for service under harsh working conditions such as high temperature and corrosive environment, and can be used as bearings, seals, valve components, measuring tools and high temperature molds. However, Cr3C2-based cermets have technical difficulties such as difficulty in sintering densification and serious abnormal growth of grains, which limits the industrial application of Cr3C2-based cermets. In order to overcome the above-mentioned problems existing in Cr3C2-based cermets, in the prior art, when preparing Cr3C2-based cermets, single component powders such as WC powder, Mo powder, and Cr powder are usually added to the Cr3C2-Ni system, and the long chain structure of Cr3C2-based cermets is changed by adding elements such as W, Mo, and Cr, and the alloy grains are refined, thereby improving the mechanical properties of the alloy. However, the above-mentioned preparation method cannot achieve the simultaneous improvement of the strength, hardness and toughness of Cr3C2-based cermets.
[0004] Therefore, there is an urgent need to provide a preparation method for Cr3C2-based cermets that can effectively inhibit the growth of Cr3C2 grains, eliminate pores and strengthen the bonding phase, and can achieve simultaneous improvement of strength, hardness and toughness. Summary of the invention
[0005] The purpose of the present invention is to provide a toughened chromium carbide-based metal ceramic and a preparation method thereof. The preparation method provided by the present invention can effectively inhibit the growth of Cr3C2 grains, eliminate pores and strengthen the bonding phase, and can achieve the simultaneous improvement of the strength, hardness and toughness of the Cr3C2-based metal ceramic.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a toughened chromium carbide-based cermet, comprising the following steps:
[0008] (1) Cr2O3, TiO2, WO3 and carbon black are mixed and subjected to a carbothermal reduction reaction, and then crushed to obtain a (Cr, Ti, W)3C2 composite solid solution powder with a single phase component;
[0009] (2) The (Cr, Ti, W)3C2 composite solid solution powder, Ni powder and a forming agent obtained in step (1) are mixed, and then granulated, pressed and sintered in sequence to obtain a toughened chromium carbide-based metal ceramic.
[0010] Preferably, in step (1), the mass ratio of Cr2O3, TiO2, WO3 and carbon black is (40-55):(15-30):(3-10):(15-30).
[0011] Preferably, the carbothermal reduction reaction in step (1) is carried out under vacuum conditions.
[0012] Preferably, the temperature of the carbothermal reduction reaction in step (1) is 1300-1500° C., and the time of the carbothermal reduction reaction is 1.5-2.5 h.
[0013] Preferably, in the step (2), the particle size of the (Cr, Ti, W)3C2 composite solid solution powder is 1 to 3 μm; and the particle size of the Ni powder is 0.2 to 1.5 μm.
[0014] Preferably, the molding agent in step (2) comprises at least one of paraffin, rubber and polyethylene glycol.
[0015] Preferably, in step (2), the molding agent accounts for 1-2% of the total mass of the (Cr, Ti, W)3C2 composite solid solution powder and the Ni powder.
[0016] Preferably, in step (2), Ni powder accounts for 15-25% of the total mass of Ni powder and (Cr, Ti, W)3C2 composite solid solution powder.
[0017] Preferably, the sintering process conditions in step (2) are: first, sinter at 500-600°C for 0.3-0.8h; then heat to 1000-1100°C and sinter for 0.3-0.8h; finally heat to 1200-1300°C, when the temperature reaches this temperature, introduce 1-5MPa of inert gas, and finally perform pressure sintering at a temperature of 1200-1300°C and a pressure of 1-5MPa for 0.5-1.5h.
[0018] The present invention also provides a toughened chromium carbide-based metal ceramic prepared by the preparation method described in the above scheme.
[0019] The present invention provides a method for preparing a toughened chromium carbide-based cermet, comprising the following steps:
[0020] (1) Cr2O3, TiO2, WO3 and carbon black are mixed to undergo a carbon thermal reduction reaction, and then crushed to obtain a (Cr, Ti, W)3C2 composite solid solution powder having a single phase composition; (2) The (Cr, Ti, W)3C2 composite solid solution powder, Ni powder and a forming agent obtained in step (1) are mixed, and then granulated, pressed and sintered in sequence to obtain a toughened chromium carbide-based metal ceramic. The present invention uses Cr2O3, TiO2, WO3 and carbon black as raw materials for a carbon thermal reduction reaction, and Ti and W atoms are dissolved into the Cr3C2 lattice under the high temperature of the carbon thermal reduction reaction, and the (Cr, Ti, W)3C2 composite solid solution powder is obtained by crushing; then the (Cr, Ti, W)3C2 composite solid solution powder, Ni powder and a forming agent are used as raw materials to prepare a chromium carbide-based metal ceramic; wherein the (Cr, Ti, W)3C2 composite solid solution powder is used as a hard phase, and the Ni powder is used as a binder. The (Cr, Ti, W) 3C2 composite solid solution powder effectively reduces its dissolution rate in the bonding phase Ni, inhibits the growth of hard phase grains and eliminates pores. At the same time, the lattice distortion effect of (Cr, Ti, W) 3C2 strengthens the carbon fixation ability of the Cr3C2 matrix, effectively inhibits the generation of carbon-deficient phases, and has a positive effect on the formation of a relatively uniform hard phase grain structure, thereby achieving a simultaneous improvement in the strength, hardness and toughness of chromium carbide-based metal ceramics. The experimental results show that the chromium carbide-based metal ceramics obtained by the preparation method provided by the present invention have a bending strength of 1378MPa, a Vickers hardness of 1273MPa, and a fracture toughness of 12.74MPa·m 1 / 2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a SEM image of the (Cr, Ti, W)3C2 composite solid solution powder prepared in Example 1 of the present invention;
[0022] Figure 2 is the XRD pattern of the (Cr, Ti, W)3C2 composite solid solution powder prepared in Example 1 of the present invention;
[0023] Figure 3 This is a microstructure morphology diagram of the 80(Cr,Ti,W)3C2-20Ni metal ceramic prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0024] The present invention provides a method for preparing a toughened chromium carbide-based cermet, comprising the following steps:
[0025] (1) Cr2O3, TiO2, WO3 and carbon black are mixed and subjected to a carbothermal reduction reaction, and then crushed to obtain a (Cr, Ti, W)3C2 composite solid solution powder with a single phase component;
[0026] (2) The (Cr, Ti, W)3C2 composite solid solution powder, Ni powder and a forming agent obtained in step (1) are mixed, and then granulated, pressed and sintered in sequence to obtain a toughened chromium carbide-based metal ceramic.
[0027] The present invention mixes Cr2O3, TiO2, WO3 and carbon black to carry out a carbothermal reduction reaction, and then obtains a (Cr, Ti, W)3C2 composite solid solution powder with a single phase component through crushing.
[0028] The present invention has no special provisions on the sources of the Cr2O3, TiO2, WO3 and carbon black, and conventional commercially available powdered solids in the art can be used.
[0029] In the present invention, the mass ratio of Cr2O3, TiO2, WO3 and carbon black is preferably (40-55): (15-30): (3-10): (15-30), and more preferably (45-50): (20-25): (5-7): (20-25). The present invention limits the amount of Cr2O3, TiO2, WO3 and carbon black to the above range, which can achieve full reduction of Cr2O3, TiO2 and WO3 by carbon black, and obtain (Cr, Ti, W)3C2 composite solid solution powder, which significantly improves the comprehensive mechanical properties of chromium carbide-based cermets.
[0030] In the present invention, the mixing method is preferably ball milling. The present invention has no special provisions on the ball milling method, and the solid materials can be mixed uniformly by using a ball milling method well known to those skilled in the art.
[0031] In the present invention, the carbon thermal reduction reaction is preferably carried out under vacuum conditions. The present invention has no special requirements for the vacuum degree of the vacuum, and it can be selected according to the routine. In the present invention, the device for the carbon thermal reduction reaction is preferably a vacuum carbon tube furnace. The present invention adopts vacuum conditions to carry out the carbon thermal reduction reaction to avoid the adverse effects of oxygen in the air on the carbon thermal reduction reaction.
[0032] In the present invention, the temperature of the carbon thermal reduction reaction is preferably 1300-1500°C, more preferably 1350-1450°C; the time of the carbon thermal reduction reaction is preferably 1.5-2.5h, more preferably 2.0-2.5h. The present invention limits the temperature and time of the carbon thermal reduction reaction to the above range, which is conducive to fully reducing the raw materials Cr2O3, TiO2 and WO3 to obtain a (Cr, Ti, W)3C2 composite solid solution.
[0033] The present invention has no special provisions on the method of crushing. The solid material crushing method well known to those skilled in the art can be used to crush large pieces or large particles of the material to the desired particle size. In the present invention, the crushing method is preferably ball milling. The present invention has no special provisions on the method of ball milling. The large pieces of material can be crushed to the desired particle size using the ball milling method well known to those skilled in the art. In the present invention, drying is also included after the ball milling. The present invention has no special provisions on the drying method. The ball milling aid used in the ball milling process can be removed using the drying method well known to those skilled in the art.
[0034] After obtaining the (Cr, Ti, W) 3 C 2 composite solid solution powder, the present invention mixes the (Cr, Ti, W) 3 C 2 composite solid solution powder, Ni powder and a forming agent, and then sequentially performs granulation, compression molding and sintering to obtain a toughened chromium carbide-based metal ceramic.
[0035] In the present invention, the particle size of the (Cr, Ti, W) 3 C2 composite solid solution powder is preferably 1 to 3 μm, more preferably 1.5 to 2.5 μm. In the present invention, the particle size of the Ni powder is preferably 0.2 to 1.5 μm, more preferably 0.5 to 1.0 μm. The present invention limits the particle sizes of the (Cr, Ti, W) 3 C2 composite solid solution powder and Ni powder to the above range, which is conducive to obtaining a densely structured metal ceramic material.
[0036] In the present invention, the Ni powder preferably accounts for 15-25% of the total mass of the Ni powder and the (Cr, Ti, W)3C2 composite solid solution powder, and more preferably 20-25%. The present invention limits the amount of the Ni powder to the above range, and the comprehensive performance of the obtained chromium carbide-based cermet is better.
[0037] In the present invention, the molding agent preferably includes at least one of paraffin, rubber and polyethylene glycol, more preferably polyethylene glycol. The present invention is conducive to mixing and molding the (Cr, Ti, W) 3 C2 composite solid solution powder and Ni powder by adding a molding agent to the raw materials. In the present invention, the molding agent preferably accounts for 1 to 2% of the total mass of the (Cr, Ti, W) 3 C2 composite solid solution powder and Ni powder, and more preferably 1.5 to 2%. The present invention limits the amount of the molding agent to the above range, which is conducive to fully bonding and molding the (Cr, Ti, W) 3 C2 composite solid solution powder and Ni powder.
[0038] The present invention has no special provisions on the granulation method. The raw materials can be made into granules by using a granulation method well known to those skilled in the art.
[0039] In the present invention, the pressure of the press molding is preferably 5 to 10 MPa, more preferably 8 to 10 MPa. The present invention limits the pressure of the press molding to the above range, which is conducive to obtaining a metal ceramic body. The present invention has no special provisions on the press molding method, and a press molding method well known to those skilled in the art can be used to obtain a metal ceramic body.
[0040] In the present invention, the sintering process conditions are preferably: first, sinter at 500-600°C for 0.3-0.8h; then, heat to 1000-1100°C for 0.3-0.8h; finally, heat to 1200-1300°C, when the temperature reaches this temperature, fill with 1-5MPa of inert gas, and finally, perform pressure sintering at 1200-1300°C and 1-5MPa for 0. 5~1.5h; more preferably, first sinter at 550~600℃ for 0.5~0.8h; then heat to 1000~1100℃, sinter at this temperature for 0.5~0.8h; finally heat to 1200~1250℃, when the temperature reaches this temperature, fill with 3~5MPa of inert gas, and finally perform pressure sintering for 1~1.5h at a temperature of 1200~1250℃ and a pressure of 3~5MPa. The present invention is used to remove the forming agent in the material by sintering at 500~600℃; sinter at 1000~1100℃ to fully carry out the deoxidation reaction in the system and eliminate the adverse effects of oxygen on the performance of metal ceramics; pressure sintering at 1200~1250℃, filled with 3~5MPa of inert gas, is used to eliminate the residual pores that are not completely eliminated during the liquid phase sintering process.
[0041] In the present invention, the heating rate in the sintering process is preferably 3.0-5.0°C / min, more preferably 3.3-4.0°C / min. The present invention limits the heating rate to the above range to avoid the adverse effect of too fast heating rate on the performance of the sintered body.
[0042] The present invention has no special provisions on the type of the inert gas, and any inert gas known to those skilled in the art can be used. In the embodiment of the present invention, the inert gas is preferably Ar gas. The present invention is used to eliminate residual pores that are not completely eliminated during the liquid phase sintering process by filling the inert gas during the sintering process.
[0043] The present invention also provides a toughened chromium carbide-based metal ceramic prepared by the preparation method described in the above scheme. The chromium carbide-based metal ceramic provided by the present invention has a bending strength of 1378MPa, a Vickers hardness of 1273MPa, and a fracture toughness of 12.74MPa·m 1 / 2 .
[0044] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0045] Example 1
[0046] A method for preparing a toughened chromium carbide-based cermet comprises the following steps:
[0047] (1) 91.19 g of Cr2O3 powder, 44.96 g of TiO2 powder, 11.84 g of WO3 powder and 44.96 g of carbon black powder (the mass ratio of Cr2O3, TiO2, WO3 and carbon black is about 47:23:6:23) were weighed and loaded into a ball mill for ball milling at a speed of 80 r / min and a ball milling time of 36 h. The ball milled mixture was placed in a vacuum carbon tube furnace for vacuum carbon thermal reduction at 1400°C for 2 h to obtain a carbon thermal reduction product (Cr, Ti, W)3C2 composite solid solution block, which was loaded into a stainless steel ball mill, and alcohol and cemented carbide grinding balls were added for planetary ball milling at a ball milling frequency of 21.5 Hz and a ball milling time of 15 h. After the ball milling, the ball milled mixture was dried at 60°C for 4 h to obtain a (Cr, Ti, W)3C2 composite solid solution powder (particle size of 1.5 to 2.5 μm);
[0048] Figure 1 The SEM image of the (Cr, Ti, W)3C2 composite solid solution powder prepared in Example 1 is shown in FIG. Figure 1 It can be seen that the crushed compound carbide powder has good dispersibility and relatively uniform particle size, and its particle size is concentrated in the range of 1.5 to 2.5 μm; this will provide favorable conditions for subsequent pressing, sintering processes and mechanical properties of metal ceramics.
[0049] Figure 2 The X-ray diffraction pattern (XRD pattern) of the (Cr, Ti, W)3C2 composite solid solution powder prepared in Example 1 is shown in FIG. Figure 2 It shows that the (Cr,Ti,W)3C2 composite solid solution powder was successfully synthesized, and there was no impurity phase and no carbon-deficient complex carbide in the phase, indicating that the prepared (Cr,Ti,W)3C2 composite solid solution powder has the high purity characteristics of a single phase component.
[0050] (2) Weigh 80 g of the (Cr, Ti, W)3C2 composite solid solution powder prepared in step (1) and 20 g of the binder phase Ni powder (particle size of 0.5-1.0 μm) (the Ni powder accounts for 20% of the total mass of the Ni powder and the (Cr, Ti, W)3C2 composite solid solution powder), put them into a ball mill, add appropriate amount of alcohol and cemented carbide grinding balls on an ordinary ball mill and perform ball milling for 36 h, with the ball milling speed of 80 r / min; after the ball milling, dry the ball milled mixture at 60°C for 4 h, add 1.8 g of polyethylene glycol (PEG4000) molding agent and granulate (the molding agent PEG4000 accounts for 1.8% of the total mass of the (Cr, Ti, W)3C2 composite solid solution powder and Ni powder), and then use a hydraulic press at a pressure of 8 MPa to press the mixture. The pellets are pressed into a metal ceramic body; the metal ceramic body is placed in a low-pressure sintering furnace for sintering, and the sintering process is as follows: first, the temperature is increased to 550°C at a heating rate of 3.3°C / min and kept for sintering for 0.5h, then the temperature is increased to 1100°C at a heating rate of 3.3°C / min and sintered at this temperature for 0.5h, and finally the temperature is increased to 1200°C at a heating rate of 3.3°C / min. When the temperature reaches this temperature, 3MPa of Ar gas is filled, and finally, pressure sintering is carried out at a temperature of 1200°C and a pressure of 3MPa for 1h to obtain a toughened chromium carbide-based metal ceramic with a composition of (57.6Cr3C2-14.4TiC-8WC)-20Ni, which is named 80(Cr,Ti,W)3C2-20Ni metal ceramic.
[0051] Figure 3 The microstructure morphology of the 80(Cr,Ti,W)3C2-20Ni-based cermet prepared in Example 1 is shown in FIG. Figure 3 It can be seen that the hard phase structure and bonding phase in the metal ceramic organization are evenly distributed, and there are no defects such as cracks and pores in the organization.
[0052] Comparative Example 1
[0053] Raw materials: Single component mixed powder
[0054] Three commercial single-component powders (Cr3C2+TiC+WC) were used, with the same alloy composition of 57.6Cr3C2-14.4TiC-8WC-20Ni (the particle size of the raw materials was also equivalent to that in Example 1), and the process conditions were consistent with step (2) in Example 1 to obtain (57.6Cr3C2-14.4TiC-8WC)-20Ni metal ceramics.
[0055] Comparative Example 2
[0056] In order to more intuitively compare the improvement of the performance of Cr3C2-Ni cemented carbide by adding (Cr, Ti, W)3C2 composite solid solution powder, this comparative example did not add any inhibitor powder (the particle size of the raw material was also equivalent to that in Example 1), the metal ceramic composition was 80Cr3C2-20Ni, and the process conditions were consistent with step (2) in Example 1 to obtain 80Cr3C2-20Ni metal ceramic.
[0057] Comparative Example 3
[0058] Two commercial single-component powders (Cr3C2+TiC) are used as raw materials (the particle size of the raw materials is also equivalent to that in Example 1), the alloy composition is 64Cr3C2-16TiC-20Ni, and the process conditions are consistent with step (2) in Example 1 to obtain 64Cr3C2-16TiC-20Ni metal ceramics.
[0059] Comparative Example 4
[0060] The (64Cr3C2-16TiC) composite solid solution powder is used as the hard phase powder (the particle size of the raw material is also equivalent to that in Example 1), the metal ceramic composition is (64Cr3C2-16TiC)-20Ni, and the process conditions are consistent with step (2) in Example 1 to obtain the (64Cr3C2-16TiC)-20Ni metal ceramic.
[0061] Comparative Example 5
[0062] Two commercial single-component powders (Cr3C2+WC) were used as raw materials (the particle size of the raw materials was also equivalent to that in Example 1), the alloy composition was 72Cr3C2-8WC-20Ni, and the process conditions were consistent with step (2) in Example 1 to obtain 72Cr3C2-8WC-20Ni metal ceramics.
[0063] Comparative Example 6
[0064] The (Cr3C2+WC) complex carbide is used as the hard phase powder (the particle size of the raw material is also equivalent to that in Example 1), the metal ceramic composition is (72Cr3C2-8WC)-20Ni, and the process conditions are consistent with step (2) in Example 1 to obtain the (72Cr3C2-8WC)-20Ni metal ceramic.
[0065] The performance of the metal ceramics obtained in Example 1 and Comparative Examples 1 to 6 was tested. The test results are shown in Table 1.
[0066] Among them: 1. Test method for flexural strength: Before the test, the sample is polished to a standard spline and placed on a horizontal special test fixture with a span of 15 mm. Then, a short-term static force is applied at a speed of no more than 1600N per second at the midpoint of the span until the spline breaks. The maximum force when the spline breaks is recorded and the width and height of the cross section near the spline fracture are measured.
[0067] This experiment uses a WDW-50 electronic universal testing machine to test the bending strength of the specimen. The size of the specimen to be tested is 20mm×6.5mm×5.25mm, and the loading speed of the force is 500N·s -1 , the span is 14.5mm, at least 5 specimens are tested in each group and the arithmetic mean is taken, and the value is retained to 10MPa. The calculation formula for flexural strength is:
[0068] TRS=3FL / (2bh 2 )
[0069] Where: TRS is the bending strength (MPa),
[0070] F is the load when the spline breaks (N),
[0071] L is the distance (span) between the two supporting points (mm),
[0072] b is the width of the spline (mm),
[0073] h is the height of the spline (mm).
[0074] 2. Vickers hardness test method:
[0075] The principle of the Vickers hardness tester is to press a right pyramid diamond indenter with a relative angle of 136° into the surface of the sample under the action of a set load P, maintain the pressure for 10 seconds and then remove the load, measure the diagonal length D of the indentation, calculate the surface area of the indentation, and finally calculate the average pressure on the indentation surface, which is the Vickers hardness. This experiment uses the HV-30Z model Vickers hardness tester to measure the hardness. Each group of samples tests at least 5 sample strips, and each sample measures 5 points. The arithmetic mean is taken and retained to the tenth digit. The calculation formula of Vickers hardness is:
[0076] HV=1.8544×P / D 2
[0077] Where: HV is Vickers hardness (Kgf·mm -2 ),
[0078] P is the applied load (Kgf),
[0079] D is the diagonal length of the indentation (mm).
[0080] 3. Fracture toughness test method:
[0081] The fracture toughness of the alloy is tested by the indentation method. The indentation of the Vickers hardness test and the cracks generated are used for calculation. Five points are taken on the surface of each cemented carbide sample for testing, and the arithmetic average of the calculated fracture toughness values is taken as the fracture toughness value of the sample. The calculation formula for fracture toughness is as follows:
[0082] K IC =0.15*(HV 30 / L i ) 1 / 2
[0083] Where: K IC is the fracture toughness (MPa·m 1 / 2 ),
[0084] HV 30 The Vickers hardness of the alloy (Kgf·mm) with a load of 30Kg -2 ),
[0085] L i is the total length of the alloy crack (mm).
[0086] Table 1 Test results of metal ceramic properties obtained in Example 1 and Comparative Examples 1 to 6
[0087]
[0088]
[0089] As can be seen from Table 1, the strength, hardness and toughness of the 80(Cr,Ti,W)3C2-20Ni metal ceramic prepared by (Cr,Ti,W)3C2 composite solid solution powder in Example 1 are significantly improved at the same time, which effectively overcomes the technical deficiency of the prior art that the three mechanical properties cannot be improved at the same time. In addition, through comparative studies, it is found that the (Cr,Ti,W)3C2 addition method is significantly better than the other three component addition methods: (1) no inhibitor powder is added (Comparative Example 2), (2) a single component mixed component (Comparative Examples 1, 3, 5), (3) 64Cr3C2-16TiC, 72Cr3C2-8WC composite solid solution components (Comparative Examples 4, 6). It can be seen that the present invention has obvious effects, and large-scale production can be achieved using traditional cemented carbide production equipment, and its production cost is low, which is convenient for industrial promotion and application.
[0090] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a toughened chromium carbide-based cermet, comprising the following steps: (1) Cr2O3, TiO2, WO3 and carbon black are mixed and subjected to a carbothermal reduction reaction, and then crushed to obtain a (Cr, Ti, W)3C2 composite solid solution powder with a single phase component; (2) mixing the (Cr, Ti, W)3C2 composite solid solution powder obtained in step (1), Ni powder and a forming agent, and then sequentially granulating, pressing and sintering to obtain a toughened chromium carbide-based cermet; In the step (1), the mass ratio of Cr2O3, TiO2, WO3 and carbon black is (40-55):(15-30):(3-10):(15-30).
2. The preparation method according to claim 1, characterized in that: The carbon thermal reduction reaction in step (1) is carried out under vacuum conditions.
3. The preparation method according to claim 1 or 2, characterized in that: The temperature of the carbon thermal reduction reaction in step (1) is 1300-1500° C., and the time of the carbon thermal reduction reaction is 1.5-2.5 hours.
4. The preparation method according to claim 1, characterized in that: In the step (2), the particle size of the (Cr, Ti, W)3C2 composite solid solution powder is 1 to 3 μm; the particle size of the Ni powder is 0.2 to 1.5 μm.
5. The preparation method according to claim 1, characterized in that: The molding agent in step (2) includes at least one of paraffin, rubber and polyethylene glycol.
6. The preparation method according to claim 1, characterized in that: In the step (2), the molding agent accounts for 1-2% of the total mass of the (Cr, Ti, W) 3 C 2 composite solid solution powder and the Ni powder.
7. The preparation method according to claim 1, characterized in that: In the step (2), the Ni powder accounts for 15-25% of the total mass of the Ni powder and the (Cr, Ti, W) 3 C 2 composite solid solution powder.
8. The preparation method according to claim 1, characterized in that: The sintering process conditions in the step (2) are: first, sinter at 500-600°C for 0.3-0.8h; then, heat to 1000-1100°C and sinter for 0.3-0.8h; finally, heat to 1200-1300°C, when the temperature reaches this temperature, introduce 1-5MPa of inert gas, and finally, perform pressure sintering at 1200-1300°C and 1-5MPa for 0.5-1.5h.
9. The toughened chromium carbide-based cermet prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Chromium-zirconium-tungsten compound carbide strengthened and toughened polycrystalline cubic boron nitride material and preparation method thereof
CN116287831A