Antibacterial and anti-drilling fabric and preparation method thereof
By using low-melting point fine denier polyester and low-elastic cladding wire in ultra-lightweight down jacket fabrics, and through nano-density treatment of zinc oxide quantum dots, the drilling and washing resistance of the fabric is solved, achieving efficient drilling resistance Fleece effect and antibacterial properties.
Patent Information
- Application Number
- CN202310131457.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-17
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-02-17
AI Technical Summary
The existing anti-drilling velvet fabrics are prone to hardening, breathable, defilm after use, and the anti-drilling velvet effect is not resistant to water washing, which cannot effectively solve the problem of drilling velvet in ultra-thin down jacket fabrics.
Low melting point fine denier polyester and low elastic coated wire interwoven into twill woven textiles, and immersed caustic soda solution and ultrasonic dispersed zinc oxide quantum dot solution, combined with rolling-baking-baking and hot pressing technology, it is embedded on the nanoscale Zinc oxide quantum dots and dense fabrics prevent down from drilling out.
It has achieved antibacterial and anti-drilling fabrics with an anti-bacterial rate of more than 99%, excellent anti-drilling and washing resistance, while maintaining the feel and breathability, making it suitable for industrial production.
Smart Images

Figure CN116289173B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an antibacterial and anti-downy fabric and a preparation method thereof, belonging to the technical field of functional textiles. Background Art
[0002] In recent years, down jackets made of ultra-light fabrics are more popular in the market. Lightweight down jackets have multiple properties such as warmth, lightness, fashion, etc., and are also convenient to carry. However, its disadvantage is that down drilling often occurs. In order to solve the problem that ultra-light down jacket fabrics with fiber fineness below 30D and warp and weft density below 380T are particularly prone to down drilling, through the synergistic effect of dyeing, shaping, calendering, laminating and other processes, the fabric width is repeatedly stretched and retracted during the processing process, and the weft is bent into an S shape to fill the gaps between fibers, achieving a better anti-drilling effect. At the same time, chemical additives are added during the calendering process to make the filaments of the fabric fiber more dispersed and smooth, able to withstand higher calendering temperatures, easier to be flattened, better fill the gaps between fibers, and reduce light scattering, thereby improving the anti-drilling performance, glossiness and softness of the fabric at the same time. At the same time, the influence of factors such as yarn fineness, density, down content, sewing needles, sewing technology and filling technology on the anti-drilling effect is studied.
[0003] Most of the existing studies have solved the problem of down drilling by gluing or resin finishing. For example, Chinese invention patent CN111134408A discloses a down drilling-proof fabric and preparation method, wherein the surface cloth and the base cloth are respectively glued with a layer of polymer film and hot-pressed to obtain two layers of down-proof membrane layers, and then the surface cloth and the base cloth (the surface cloth faces up and the base cloth faces down) are sent to the three-dimensional engraved roller of the hot press for hot-pressing bonding process to achieve the bonding of the surface cloth and the base cloth. After the three-dimensional engraved roller pattern is presented, flushing is injected into the cavity to obtain the down drilling-proof fabric. Chinese invention patent CN110029504A discloses a down drilling-proof fabric, including a base cloth layer and a porous resin layer, and the porous resin layer contains acrylic resin and silicone resin. Chinese invention patent CN107245880A discloses a method for preventing down from penetrating into down jacket fabrics. The method selects a fabric made of soft, wrinkle-resistant, thin, and high-strength mercerized cotton, uses a water-repellent finishing agent composed of silica and zinc octoate to perform a water-repellent treatment on the fabric, and then uses high-pressure friction calendering to maintain the softness and glossiness of the fabric, and then applies a modified coating adhesive.
[0004] Although the existing anti-down drilling technology involves a variety of solutions and has reduced the down drilling phenomenon to a certain extent, it still has shortcomings such as hardening after use, airtightness, film peeling, and the anti-down drilling effect is not resistant to water washing, which continues to trouble the majority of producers and consumers. Summary of the invention
[0005] In view of the deficiencies in the prior art, the present invention provides an antibacterial and anti-downy fabric with excellent hand feel, anti-downy property, washing resistance and air permeability and a simple preparation process, and a preparation method thereof.
[0006] The technical solution to achieve the purpose of the present invention is to provide a method for preparing an antibacterial and anti-downy fabric, comprising the following steps:
[0007] (1) Using low-melting-point fine-denier polyester twisted low-elastic yarn as warp yarn and fine-denier chemical fiber low-elastic covered yarn as weft yarn, sizing and interweaving into 50-80gsm twill woven textiles;
[0008] (2) Immerse the textile in a caustic soda solution with a concentration of 20 to 40 g / l, roll it up and pile it at room temperature for 24 to 48 hours, wash and dry it for later use;
[0009] (3) Dispersing zinc acetate dihydrate in dimethyl sulfoxide, and preparing a zinc source solution with a molar concentration of 0.03-0.3M after ultrasonic dispersion treatment; dispersing tetramethylammonium hydroxide in anhydrous ethanol, and preparing a tetramethylammonium hydroxide ethanol solution with a molar concentration of 0.15-0.5M after ultrasonic dispersion treatment; placing the zinc source solution in a heat-collecting constant temperature heating magnetic stirrer, adding the tetramethylammonium hydroxide ethanol solution dropwise at a temperature of 60-70°C and a pH of 7-7.5, reacting for 2-2.5 hours, and then slowly dropping ethyl acetate until the solution becomes white turbid, thereby obtaining a self-dispersed zinc oxide quantum dot solution;
[0010] (4) diluting the self-dispersed zinc oxide quantum dot solution into a 5-10% milling solution, placing the textile prepared in step (2) in the milling solution for milling-baking-baking treatment, wherein the milling rate is 100-150%, the pre-baking temperature is 80-110°C, and the baking temperature is 120-140°C, to obtain a textile containing zinc oxide quantum dots;
[0011] (5) The reverse side of the textile prepared in step (4) is subjected to hot pressing in a hot pressing device at a temperature of 150 to 180° C. to obtain an antibacterial and anti-downy fabric.
[0012] The invention discloses a method for preparing an antibacterial and anti-down drilling down jacket fabric, wherein the low-melting-point fine-denier polyester is 20-50D polyester with a melting point of 245-250°C; the fine-denier chemical fiber low-elastic coated yarn is 20-50D polyester and nylon coated with 20-30D spandex.
[0013] The technical solution of the present invention also includes an antibacterial and anti-downy fabric obtained according to the above preparation method.
[0014] The drilling out of down is mainly related to the density of the fabric itself and the electrostatic adsorption during use. The present invention uses the micropore filling and anti-static effect of zinc oxide quantum dots at the nanoscale, and cooperates with the hot pressing and densification of low-melting point polyester to build a down protection wall, which is an effective way to solve the shortcomings of the prior art in preventing down from drilling out of fabrics. By solving the problem of the density of the fabric itself and the electrostatic drilling of down during use, the drilling out of down is prevented, and the number of down that drills out can reach less than 5. The nano-micropore effect does not affect the feel and breathability. At the same time, the antibacterial rate of the antibacterial and anti-drilling down down jacket fabric reaches more than 99%, and it has excellent anti-drilling and washing resistance.
[0015] Compared with the prior art, the invention has the following beneficial effects: the antibacterial and anti-down drilling fabric provided has an antibacterial rate of more than 99% and has excellent anti-down drilling and washing resistance. The preparation method of the antibacterial and anti-down drilling down jacket fabric provided by the invention has the advantages of being simple and fast, requiring low equipment, and is conducive to industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 , 2 They are EDS and SEM images of the fabric prepared in Example 1 of the present invention;
[0017] Figure 3 This is a distribution diagram of C, O and Zn on the fabric prepared in Example 1 of the present invention;
[0018] Figure 4 The infrared spectra of the fabric prepared in Example 1 of the present invention and the comparative example;
[0019] Figure 5 This is a diagram showing the antibacterial effects of the fabric prepared in Example 1 of the present invention and the comparative example. Implementation
[0020] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments. Example 1
[0021] Using low-melting-point fine-denier polyester twisted low-elastic yarn 30D36F as warp yarn (polyester melting point is 245-250°C), fine-denier polyester low-elastic coated yarn 20D24F / 20D as weft yarn (polyester, nylon coated spandex) (the above raw materials are products provided by Jiangsu Nanodun Technology Co., Ltd.), using PVA for sizing, with a sizing rate of 10%, interweaving into a 1 / 3 twill woven textile with a gram weight of 50gsm; immersing the textile in a caustic soda solution with a concentration of 20g / l, rolling and stacking at room temperature for 24h, washing and drying for use;
[0022] 30 mmol of zinc acetate dihydrate was dispersed in 30 ml of dimethyl sulfoxide, and 55 mmol of tetramethylammonium hydroxide was dispersed in 100 ml of anhydrous ethanol. After ultrasonic dispersion treatment, a zinc source solution and an ethanol solution of tetramethylammonium hydroxide were obtained. The zinc source solution was placed in a heat-collecting constant temperature heating magnetic stirrer, the temperature was set to 60-70°C, the pH was adjusted to 7.5, and the ethanol solution of tetramethylammonium hydroxide was added dropwise. The reaction was continued for 2 hours, and then 240 ml of ethyl acetate was slowly added dropwise until the solution became white and turbid, thereby obtaining a self-dispersed zinc oxide quantum dot solution.
[0023] The textiles pre-treated by washing and drying were subjected to a rolling-baking-baking treatment in a quantum dot solution diluted to a concentration of 5-10% as a rolling liquid, with a rolling liquid rate of 100%, a pre-baking temperature of 80°C, and a baking temperature of 130°C to obtain a textile containing zinc oxide quantum dots. The reverse side of the textile was hot-pressed in a hot-pressing device at a controlled temperature of 170°C to obtain an antibacterial and anti-drilling down (down) fabric.
[0024] See attached Figure 1 , 2 , are EDS and SEM images of the fabric prepared in this example, respectively. Figure 1 In the figure, Figure a is a scanning electron microscope image of the fabric not rolled with the quantum dot solution, and Figure b is a scanning electron microscope image of the fabric treated with the rolled quantum dot solution; Figure 2 Energy spectrum.
[0025] See attached Figure 3 , which are distribution diagrams of C\O\Zn, C, O and Zn on the fabric prepared in this embodiment; wherein, Figure d is the C\O\Zn distribution diagram, Figure e is the C distribution diagram, Figure f is the O distribution diagram, and Figure g is the Zn distribution diagram.
[0026] Depend on Figure 1 , 2 From the results in Figure 3 and Figure 4, it can be seen that the fabric surface is covered with a uniform layer of material, and part of the material enters the fiber pores, with good adhesion.
[0027] See attached Figure 4 , is the infrared spectrum of the fabric prepared in this embodiment. Among them, curves a, b and c are ordinary polyester fabric, fabric before zinc oxide quantum dots impregnation and fabric after zinc oxide quantum dots impregnation, respectively. The results show that zinc oxide quantum dots are successfully grafted on the fabric.
[0028] See attached Figure 5, which are the antibacterial effect diagrams of the fabric prepared in this embodiment. Among them, Figure a, Figure b and Figure c are the antibacterial effect diagrams of blank fabric, fabric before impregnation with zinc oxide quantum dots and fabric after impregnation with zinc oxide quantum dots on Escherichia coli respectively; Figure e, Figure d and Figure f are the antibacterial effect diagrams of blank fabric, fabric before impregnation with zinc oxide quantum dots and fabric after impregnation with zinc oxide quantum dots on Staphylococcus aureus respectively; it can be seen that the fabric provided in this embodiment has excellent antibacterial effect.
[0029] The prepared fabric was tested according to Method B in Appendix E of GB / T14272-2011, and the number of down drilling was 4, indicating that the fabric had good anti-down drilling properties. Example 2
[0030] The low-melting-point fine-denier polyester twisted low-elastic yarn 30D48F was used as the warp yarn, and the fine-denier polyester low-elastic coated yarn 20D36F / 20D was used as the weft yarn. PVA was used for sizing, and the sizing rate was 10%. The textile was interwoven into a 1 / 3 twill woven textile with a gram weight of 50gsm; the textile was immersed in a caustic soda solution with a concentration of 15g / l, rolled and stacked at room temperature for 36h, washed and dried for use; 30mmol of zinc acetate dihydrate was dispersed in 30ml of dimethyl sulfoxide. Then 55mmol of tetramethylammonium hydroxide was dispersed in 100ml of anhydrous ethanol. After dispersion and ultrasonication, the zinc source solution was placed in a heat-collecting constant-temperature heating magnetic stirrer, the temperature was set to 60~-70℃, the pH was adjusted to 7.5, and then the ethanol solution of tetramethylammonium hydroxide was added dropwise, reacted for 2h, and then 240ml of ethyl acetate was slowly dripped until the solution became white and turbid, and finally a self-dispersed zinc oxide quantum dot solution was obtained. The textiles after washing and drying pretreatment were subjected to a rolling-baking-baking treatment in a rolling liquid diluted with a quantum dot solution to a concentration of 5-10%, with a rolling liquid rate of 100%, a prebaking temperature of 80°C, and a baking temperature of 130°C to obtain a textile containing zinc oxide quantum dots. The single side of the textile was hot-pressed in a hot-pressing device at a controlled temperature of 160°C to obtain an antibacterial and anti-drilling down jacket fabric. Example 3
[0031] The low-melting-point fine-denier polyester twisted low-elastic yarn 30D48F was used as the warp yarn, and the fine-denier nylon low-elastic coated yarn 20D36F / 20D was used as the weft yarn. PVA was used for sizing, and the sizing rate was 15%, and the 1 / 3 twill woven textile with a gram weight of 50gsm was interwoven; the textile was immersed in a caustic soda solution with a concentration of 15g / l, rolled and stacked at room temperature for 48h, washed and dried for use; 30mmol of zinc acetate dihydrate was dispersed in 30ml of dimethyl sulfoxide. Then 55mmol of tetramethylammonium hydroxide was dispersed in 100ml of anhydrous ethanol. After dispersion and ultrasonication, the zinc source solution was placed in a heat-collecting constant-temperature heating magnetic stirrer, the temperature was set to 70℃, the pH was adjusted to 7.5, and then the ethanol solution of tetramethylammonium hydroxide was added dropwise, and the reaction was carried out for 2.5h, and then 240ml of ethyl acetate was slowly dripped until the solution became white and turbid, and finally a self-dispersed zinc oxide quantum dot solution was obtained. The textiles after washing and drying pretreatment were subjected to a rolling-baking-baking treatment in a rolling liquid diluted with a quantum dot solution to a concentration of 5-10%, with a rolling liquid rate of 100%, a prebaking temperature of 80°C, and a baking temperature of 130°C to obtain a textile containing zinc oxide quantum dots. The single side of the textile was hot-pressed in a hot-pressing device at a controlled temperature of 160°C to obtain an antibacterial and anti-drilling down jacket fabric. Example 4
[0032] The low-melting-point fine-denier polyester twisted low-elastic yarn 30D36F was used as the warp yarn, and the fine-denier nylon low-elastic coated yarn 30D36F / 30D was used as the weft yarn. PVA was used for sizing, and the sizing rate was about 15%, and the 1 / 2 twill woven textile with a gram weight of 58gsm was interwoven; the textile was immersed in a caustic soda solution with a concentration of 15g / l, rolled and stacked at room temperature for 24h, washed and dried for use; 20mmol of zinc acetate dihydrate was dispersed in 20ml of dimethyl sulfoxide respectively. Then 30mmol of tetramethylammonium hydroxide was dispersed in 50ml of anhydrous ethanol. After dispersion and ultrasonication, the zinc source solution was placed in a heat-collecting constant-temperature heating magnetic stirrer, the temperature was set to 60℃, the pH was adjusted to 7.5, and then the ethanol solution of tetramethylammonium hydroxide was added dropwise, reacted for 2h, and then 120ml of ethyl acetate was slowly dripped until the solution became white and turbid, and finally a self-dispersed zinc oxide quantum dot solution was obtained. The textiles pre-treated by washing and drying were subjected to a rolling-baking-baking treatment in a rolling liquid diluted with a quantum dot solution with a concentration of 5-10%, with a rolling liquid rate of 100%, a pre-baking temperature of 80°C, and a baking temperature of 130°C to obtain a textile containing zinc oxide quantum dots. The single side of the textile was hot-pressed in a hot-pressing device at a controlled temperature of 170°C to obtain an antibacterial and anti-drilling down jacket fabric.
Claims
1. A method for preparing an antibacterial and anti-drilling down fabric, characterized in that The following steps are involved: (1) Using low-melting-point fine-denier polyester twisted low-elastic yarn as warp yarn and fine-denier chemical fiber low-elastic covered yarn as weft yarn, sizing and interweaving into 50-80gsm twill woven textiles; (2) Immerse the textile in a caustic soda solution with a concentration of 20 to 40 g / l, roll it up and pile it at room temperature for 24 to 48 hours, wash and dry it for later use; (3) Dispersing zinc acetate dihydrate in dimethyl sulfoxide, and preparing a zinc source solution with a molar concentration of 0.03 to 0.3 M after ultrasonic dispersion treatment; dispersing tetramethylammonium hydroxide in anhydrous ethanol, and preparing a tetramethylammonium hydroxide ethanol solution with a molar concentration of 0.15 to 0.5 M after ultrasonic dispersion treatment; The zinc source solution is placed in a heat-collecting constant temperature heating magnetic stirrer, and an ethanol solution of tetramethylammonium hydroxide is added dropwise at a temperature of 60 to 70°C and a pH of 7 to 7.5, and the reaction is carried out for 2 to 2.5 hours, and then ethyl acetate is slowly added dropwise until the solution becomes white and turbid, thereby obtaining a self-dispersed zinc oxide quantum dot solution; (4) diluting the self-dispersed zinc oxide quantum dot solution into a 5-10% milling solution, placing the textile prepared in step (2) in the milling solution for milling-baking-baking treatment, wherein the milling rate is 100-150%, the pre-baking temperature is 80-110°C, and the baking temperature is 120-140°C, to obtain a textile containing zinc oxide quantum dots; (5) The reverse side of the textile prepared in step (4) is subjected to hot pressing in a hot pressing device at a temperature of 150 to 180° C. to obtain an antibacterial and anti-downy fabric.
2. The method for preparing an antibacterial and anti-down drilling down jacket fabric according to claim 1, characterized in that: The low-melting-point fine-denier polyester is 20-50D polyester with a melting point of 245-250°C; the fine-denier chemical fiber low-elasticity coated yarn is 20-50D polyester and nylon coated with 20-30D spandex.
3. An antibacterial and anti-downy fabric obtained by the preparation method according to claim 1.