Composite nanofiber membrane cloth and preparation method thereof

By coating the adhesive layer on the non-woven fabric support substrate and preparing the nanofiber membrane using electrospinning technology, the problems of complex processes and uneven bonding effects in the prior art are solved, and efficient production of nanofiber membrane cloth is achieved and excellent performance.

CN118910811APending Publication Date: 2024-11-08GUANG DONG HOU HAI RUI MO XIN CAI LIAO KE JI YOU XIAN GONG SI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411289154.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, the production process of nanofiber membrane cloth is complex and can easily damage the microstructure of nanofibers, affecting its physical and chemical properties, and the bonding effect is uneven, which cannot meet the actual application needs.

Method used

The glue scraper drum is used to coat the adhesive layer in a dot or layer on the non-woven supporting substrate, and prepare nanofiber membranes on the adhesive layer through electrospinning technology to adjust the spinning speed and material proportion to ensure adhesion. and breathability, avoid hot pressing process, and simplify production process.

Benefits of technology

The uniform adhesive layer and efficient spinning of the nanofiber membrane cloth are achieved, which protects the nanofiber structure without affecting its breathability and moisture permeability, simplifies the production process and improves the bonding strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910811A_ABST
    Figure CN118910811A_ABST
Patent Text Reader

Abstract

The invention provides composite nanofiber membrane cloth and a preparation method thereof, and particularly relates to the technical field of nanofiber membranes. The composite nanofiber membrane cloth comprises a non-woven fabric supporting substrate, and the non-woven fabric supporting substrate is coated with a glue attaching layer in a dotted or layered mode through a roller of a glue scraper; the nanofiber membrane is prepared on the adhesive layer through an electrostatic spinning technology; wherein the glue applying amount of the glue scraping machine is 4 g / m < 2 >-6 g / m < 2 >, and the thickness of the glue attaching layer is 0.2-3 mm; the electrostatic spinning process parameters are as follows: the voltage is 8kV-90kV, the aperture of a nozzle is 0.2 mm-3mm, the flow velocity of a solution is 1ml / min-1500ml / min, the spinning environment temperature is 20 DEG C-80 DEG C, and the solution comprises LiCl with the mass fraction of 0.01%-1%. In the preparation process of the composite nanofiber membrane cloth, dot-shaped or layered adhesive attachment is adopted, a hot pressing process is not needed, the production process is simplified, the nanofiber membrane structure is protected, and the air permeability and moisture permeability of the nanofiber membrane are not affected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nanofiber membranes, and in particular to a composite nanofiber membrane cloth and a preparation method thereof. Background Art

[0002] Nanofiber refers to a linear material with a nanometer diameter and a relatively long length with a certain aspect ratio. In addition, ordinary fibers modified by filling nanoparticles into them are also called nanofibers. In a narrow sense, the diameter of nanofibers is between 1nm and 100nm, but in a broad sense, fibers with a diameter below 1000nm are called nanofibers.

[0003] Nanofiber membranes are generally non-woven membranes obtained by optimizing electrospinning processes using polymer materials with certain functions and activities. Such non-woven membranes usually have good air permeability, good water vapor permeability, good liquid absorption, etc. At the same time, they can have structures and functions similar to extracellular matrix, which can promote the rapid repair of damaged tissues. Therefore, multifunctional nanofiber membranes have broad application prospects in the fields of medical wound dressings, tissue scaffolds, and in vivo drug carriers.

[0004] The main methods of combining traditional non-woven fabrics with nanofiber membranes are hot melt composite technology and lamination technology. The hot melt composite technology uses hot melt adhesive as an adhesive to heat and melt the nanofiber membrane and press it together with the non-woven fabric substrate. The lamination technology is to laminate the prefabricated nanofiber membrane and non-woven fabric under a certain temperature and pressure through physical pressure and / or heat treatment to form a stable composite structure. Hot melt adhesive or other adhesives can be used during the lamination process to enhance the bonding force.

[0005] The prior art has the following problems:

[0006] 1. Hot-melt composite technology: After the nanofiber membrane is heated and melted, the microstructure of the nanofiber will be destroyed, affecting the physical and chemical properties of the nanofiber membrane cloth;

[0007] 2. Lamination technology, which has a complicated process and requires a hot press for compounding, and the pressure control can easily affect the structural function of the nanofiber membrane cloth.

[0008] The invention patent with application number 200880018620.0 discloses a method for forming a laminate of a nanofiber web and a substrate and a filter using the laminate. The method includes providing a carrier layer with a collection surface, forming a nanofiber web on the collection surface of the carrier layer, providing a flexible porous substrate with two main surfaces, applying an adhesive layer to at least a portion of one surface of the substrate, contacting the adhesive layer with the nanofiber web and bonding the nanofiber web to the substrate, and optionally removing the carrier layer to form a composite sheet. The use of a molten adhesive requires applying the adhesive at a temperature higher than the softening point or melting point of the adhesive and contacting the nanofiber web with the substrate. However, the disadvantage of this method is that the bonding effect between the nanofibers and the non-woven fabric base layer is uneven and the bonding strength is limited, which cannot meet the needs of practical applications.

[0009] Therefore, how to provide a method for producing nanofiber membrane cloth with a simple process and without affecting the functional properties of the nanofiber membrane cloth is a technical problem that needs to be urgently solved by technical personnel in this field. Summary of the invention

[0010] In order to solve the above problems, the present invention provides a method for producing a nanofiber membrane cloth, aiming to solve the technical problems in the prior art that the production process is complicated and the production process will affect the efficacy of the nanofiber membrane cloth.

[0011] In order to solve the above technical problems, the present invention provides a composite nanofiber membrane cloth in a first aspect, comprising:

[0012] A non-woven fabric support substrate, comprising a glue layer applied in dots or layers on the non-woven fabric support substrate by a glue scraper roller;

[0013] A nanofiber membrane is prepared on the adhesive layer by electrospinning technology;

[0014] The glue application rate of the scraper is 4g / m 2 ~6g / m 2 The thickness of the adhesive layer is 0.2 to 3 mm; the electrospinning process parameters are a voltage of 8 kV to 90 kV, a nozzle aperture of 0.2 mm to 3 mm, a solution flow rate of 1 mL / min to 1500 ml / min, and a spinning environment temperature of 20°C to 80°C. The solution includes a mass fraction of 0.1% to 1% LiCl; as an example, 0.01% to 0.05% is preferred.

[0015] The ratio of the glue scraping machine speed to the electrospinning speed is 1:1, and the entire production process is adjusted based on the electrospinning capacity. Currently, the most suitable process is 0.1mm / s-5mm / s. After the non-woven fabric is glued, it directly enters the electrospinning machine for spinning, so that the nanofibers will not separate from the substrate.

[0016] In some embodiments, after the colloid is melted in the scraper, a thin layer is spread, and then the non-woven fabric support substrate is coated with dots or layers by a roller; after the heating rod in the scraper heats the colloid to 100° C., the non-woven fabric support substrate is coated with dots or layers by a roller. Taking ethylene-vinyl acetate copolymer melt as an example, the amount of a thin layer is 1 to 3 g / m 2 to increase the adhesion of the adhesive layer.

[0017] According to the specific requirements of the non-woven fabric substrate and the adhesive layer, adjust the speed and pressure of the scraper roller to ensure that the total adhesive amount is 4-6g / m 2 To achieve a uniform and moderate adhesive layer. At the same time, in order to control the thickness of the adhesive layer between 0.5μm and 2000μm, the viscosity of the adhesive and the gap between the rollers need to be precisely controlled.

[0018] In certain embodiments, in the composite nanofiber membrane cloth, the spinning speed of electrospinning is 0.1 m / min to 5 m / min.

[0019] The winding speed is the same as the electrospinning speed. Combined with the gluing-electrospinning-winding composite process, the winding speed is adjusted mainly according to the thickness requirements of the electrospun nanofibers, with a ratio of 1:1.

[0020] In certain embodiments, in the composite nanofiber membrane cloth, the scraping speed of the scraper on the non-woven fabric support substrate is 0.2 m / min to 3 m / min.

[0021] In certain embodiments, in the composite nanofiber membrane cloth, the material of the non-woven fabric supporting substrate is at least one of PP, PE, EP, ES, ET and PET.

[0022] In certain embodiments, in the composite nanofiber membrane cloth, the colloid used in the glue scraper is at least one of hot melt adhesive, PU, ​​acrylic glue, and ethylene-vinyl acetate copolymer.

[0023] In certain embodiments, in the composite nanofiber membrane cloth, the nanofiber membrane uses at least one of TPU, PVDF, PVA, PEG, PVP, and PAN as an electrospinning raw material; preferably, a compound of PVDF, PAN, and PVA is in a ratio of 1:1:1.

[0024] In certain embodiments, in the composite nanofiber membrane cloth, the solution includes 20% to 30% by mass of the electrospinning raw material.

[0025] In certain embodiments, in the composite nanofiber membrane cloth, the solution includes an oily solvent and an aqueous solvent; the oily solvent is one of DMF, toluene, DMAC, and DCM, and the aqueous solvent is deionized water.

[0026] Another aspect of the present invention further provides a method for preparing a composite nanofiber membrane cloth, which comprises the following steps:

[0027] preparing a nonwoven support substrate;

[0028] An electrospinning solution is prepared, wherein the solution comprises 20% to 30% by mass of an electrospinning raw material, 0.01% to 1% by mass of LiCl, an oily solvent and an aqueous solvent; as an example, 0.01% to 0.05% is preferred.

[0029] The glue scraper is preheated to heat the colloid in the glue scraper to 100° C. The glue scraper roller applies the colloid in dots or layers on the non-woven fabric support substrate at a linear speed of 0.1 m / min-5 m / min to form an adhesive layer on the non-woven fabric support substrate;

[0030] The nanofiber membrane is prepared on the adhesive layer by electrostatic spinning technology; the electrostatic spinning process parameters are voltage 8kV-90kV, nozzle aperture 0.2mm-3mm, solution flow rate 1mL / min-1500ml / min.

[0031] Beneficial effects:

[0032] The present invention finds the most suitable parameters for preparing nanofiber membranes by screening spinning speed and electrospinning materials, and by first spreading a thin layer of colloid and then spot coating or layer coating, on the one hand, the adhesion can be increased, and on the other hand, the air permeability and moisture permeability of the nanofiber membrane are not affected.

[0033] The composite nanofiber membrane cloth and preparation method thereof described in the present invention adopts point-shaped or layer-shaped adhesive attachment in the preparation process of the composite nanofiber membrane cloth, and does not need to go through a hot pressing process, thereby simplifying the production process, protecting the nanofiber membrane structure, and not affecting the air permeability and moisture permeability of the nanofiber membrane. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 Schematic diagram of the composite nanofiber membrane forming process provided in an embodiment of the present invention.

[0035] Figure 2 Schematic diagram of the bonding method of glue and non-woven fabric provided in an embodiment of the present invention, wherein A is in the form of dots and B is in the form of layers. DETAILED DESCRIPTION

[0036] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0037] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that the upper and lower limits of the scope and each intermediate value therebetween are specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art described in the present invention are generally understood. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or verification of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0039] As used herein, "include", "including", "have", "contain", etc. are all open terms, which means including but not limited to. As used herein, "and / or" includes any or all combinations of the things mentioned. Unless otherwise specified, % refers to mass volume percentage.

[0040] DMF - dimethylformamide;

[0041] DMAC-dimethylacetamide;

[0042] DCM - dichloromethane;

[0043] PP-polypropylene; PE-polyethylene; EP-epoxy resin; ES-vinyl sulfate; ET-ethanol; PET-polyethylene terephthalate; PU-polyurethane;

[0044] TPU-thermoplastic polyurethane elastomer (Product No.: BASF 1195A);

[0045] VDF-polyvinylidene fluoride; PVA-polyvinyl alcohol; PEG-polyethylene glycol; PVP-polyvinyl pyrrolidone; PAN-polyacrylonitrile.

[0046] like Figure 1 and Figure 2 As shown, the present invention provides a composite nanofiber membrane cloth on one hand, which comprises:

[0047] A non-woven fabric support substrate, comprising a glue layer applied in dots or layers on the non-woven fabric support substrate by a glue scraper roller;

[0048] A nanofiber membrane is prepared on the adhesive layer by electrospinning technology;

[0049] The glue application rate of the scraper is 4g / m 2 ~6g / m 2 The thickness of the adhesive layer is 0.2 μm to 3000 μm; the electrospinning process parameters are voltage 8 kV to 90 kV, nozzle aperture 0.2 mm to 3 mm, solution flow rate 1 mL / min to 100 μl / min, spinning environment temperature 20°C to 80°C, and the solution includes LiCl with a mass fraction of 0.01% to 1%; preferably 0.01%-0.05%.

[0050] like Figure 2 As shown, the second aspect of the present invention also provides a method for preparing a composite nanofiber membrane cloth, which comprises:

[0051] preparing a nonwoven support substrate;

[0052] Preparing an electrospinning solution, the solution comprising 20% ​​to 30% by mass of an electrospinning raw material, 0.05% to 0.08% by mass of LiCl, an oily solvent, and an aqueous solvent;

[0053] Preheat the scraper, heat and melt the colloid in the scraper, and spread a thin layer of colloid. The amount of a thin layer is 2-5g / m 2 Dosage, and then continue to heat to 100 ℃, such as Figure 1 As shown, the scraper roller is at a linear speed of 0.1m / min-3m / min, and a dot-shaped (such as Figure 2 -A) or layered (e.g. Figure 2 -B) coating the colloid to form an adhesive layer on the non-woven fabric support substrate, with a total adhesive amount of 4 g / m 2 ~6g / m 2 between;

[0054] The nanofiber membrane is prepared on the adhesive layer by electrostatic spinning technology; the electrostatic spinning process parameters are voltage 8kV-90kV, nozzle aperture 0.2mm-3mm, solution flow rate 1mL / min-100μl / min.

[0055] Using the data in Examples 1 to 6 in Table 1 as technical parameters, a composite nanofiber membrane cloth was prepared according to the method for preparing a composite nanofiber membrane cloth of the present invention:

[0056] GB / T1499.2—2018 standard maximum force / maximum deformation test, GB / T 5453-1997 air permeability and GB / T40910-2021 water pressure resistance.

[0057] Parameter screening:

[0058] 1. Screening of spinning speed

[0059] As shown in Table 1, other parameters are the same, and the spinning speed V is changed. The indicators are shown in Table 2.

[0060] Table 1

[0061]

[0062] Table 2

[0063]

[0064]

[0065] It can be seen from Table 2 that the spinning speed is best at 0.2 mm / s-1 mm / s, and the subsequent experiments are carried out at 0.5 mm / s.

[0066] 2. Screening of electrospinning materials

[0067] As shown in Table 3, other parameters are the same, and the electrospinning materials are changed. The indicators are shown in Table 4. From the preliminary verification, it can be known that PVDF has good mechanical properties. In order to ensure the mechanical properties of the fiber membrane cloth, the spinning solution must contain at least PVDF. Therefore, in the subsequent screening experiments, PVDF is screened.

[0068] Table 3

[0069]

[0070]

[0071] Table 4

[0072]

[0073] As shown in Table 4, the optimal electrospinning material is PVDF:PAN:PVA=1, and this ratio was used in all subsequent experiments.

[0074] The parameters of Examples 1-6 are shown in Table 5, and the parameters of the comparative example are shown in Table 6;

[0075] The measurement results of Examples 1 to 6 and Comparative Examples 1 to 6 are shown in Table 7.

[0076] Table 5

[0077]

[0078]

[0079] Table 6

[0080]

[0081]

[0082] Table 7

[0083]

[0084] As can be seen from the above, 1. Different spinning materials, spinning speeds, glue coating amounts and treatment methods have certain effects on the nanofiber composite membrane cloth, among which 0.2mm / s-1mm / s has a better effect; PVDF:PAN:PVA=1 is the best electrospinning material.

[0085] 2. The spinning speed and gluing speed will seriously affect the amount of gluing. The faster the speed, the lower the amount of gluing, the better the corresponding air permeability, the worse the mechanical properties, the lower the maximum deformation, and the lower the water seepage pressure.

[0086] 3. Different concentrations of PVDF have an impact on the composite effect, mainly affecting the amount of electrospinning, so PVDF is added to the electrospinning material, but the concentration needs to be controlled. Too high a concentration will affect the spinning effect, so the total amount of PVDF, PAN and PVA in the electrospinning material does not exceed 30%.

[0087] 4. During the spinning process, LiCl and NaCl can be appropriately added to enhance the conductivity, but the effect of KCl is not good. LiCl and NaCl are preferred, which will be more conducive to the spinning process.

[0088] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

Claims

1. A composite nanofiber membrane cloth, characterized in that: The steps include: A non-woven fabric support substrate, comprising a glue layer applied in dots or layers on the non-woven fabric support substrate by a glue scraper roller; A nanofiber membrane is prepared on the adhesive layer by electrospinning technology; Among them, the glue application amount of the scraper is 4g / m2~6g / m2, the thickness of the adhesive layer is 0.2~3mm; the electrospinning process parameters are voltage 8kV~90kV, nozzle aperture 0.2mm~3mm, solution flow rate 1mL / min~1500ml / min, spinning environment temperature 20℃~80℃, and the solution includes LiCl or NaCl with a mass fraction of 0.01%~1%.

2. The composite nanofiber membrane cloth according to claim 1, characterized in that: After the colloid is melted in the scraper, a thin layer is spread and then coated on the non-woven fabric support substrate in a dot or layered manner through a roller.

3. The composite nanofiber membrane cloth according to claim 1, characterized in that: The spinning speed of electrospinning is 0.1 m / min to 5 m / min.

4. The composite nanofiber membrane cloth according to claim 3, characterized in that: The scraping speed of the scraper on the non-woven fabric support substrate is 0.1 m / min to 5 m / min.

5. The composite nanofiber membrane cloth according to claim 1, characterized in that: The material of the non-woven fabric supporting substrate is at least one of PP, PE, EP, ES, ET and PET.

6. The composite nanofiber membrane cloth according to claim 1, characterized in that: The colloid used in the scraper is at least one of hot melt adhesive, PU, ​​acrylic glue, and ethylene-vinyl acetate copolymer.

7. The composite nanofiber membrane cloth according to claim 1, characterized in that: The nanofiber membrane uses at least one of TPU, PVDF, PVA, PEG, PVP and PAN as an electrospinning raw material.

8. The composite nanofiber membrane cloth according to claim 7, characterized in that: The solution comprises 20% to 30% of the electrospinning raw material by mass.

9. The composite nanofiber membrane cloth according to claim 1, characterized in that: The solution comprises an oily solvent and an aqueous solvent; the oily solvent is one of DMF, toluene, DMAC and DCM, and the aqueous solvent is deionized water.

10. A method for preparing the composite nanofiber membrane cloth according to any one of claims 1 to 9, characterized in that: The steps include: preparing a nonwoven support substrate; An electrospinning solution is prepared, wherein the solution comprises 20% to 30% by mass of an electrospinning raw material, 0.05% to 0.1% by mass of LiCl, an oily solvent and an aqueous solvent; The glue scraper is preheated to heat the colloid in the glue scraper to 100° C. The glue scraper roller applies the colloid in dots or layers on the non-woven fabric support substrate at a linear speed of 0.1 m / min-5 m / min to form an adhesive layer on the non-woven fabric support substrate; The nanofiber membrane is prepared on the adhesive layer by electrostatic spinning technology; the electrostatic spinning process parameters are voltage 8kV-90kV, nozzle aperture 0.2mm-3mm, solution flow rate 1mL / min-1500ml / min.

Citation Information

Patent Citations

  • Nanofibre hyperfiltration membrane and preparation method thereof

    CN101559326A

  • Compounding method for electrospinning nanometer composite nonwoven fabric

    CN102922858A

  • Anti-haze window gauze and preparation method thereof

    CN106639844A

  • Composite separator, method for making the same, and lithium ion battery using the same

    US20180034027A1

  • AU2003200405A1