Anti-static heat sealing cover tape and preparation method thereof

Through the composite modification of the cover tape base layer and the nucleophilic addition reaction of the thermoplastic elastomer, a heat sealed cover tape with anti-static function is formed, which solves the problem of damage to electronic components at high temperatures and achieves a lower level of Effective bonding and anti-static effect at temperature.

CN119039646AActive Publication Date: 2024-11-29GUIXI RUOBANG ELECTRONICS SCI & TECH

Patent Information

Application Number
CN202411254017.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-29
Estimated Expiration
2044-09-09

AI Technical Summary

Technical Problem

The existing heat sealing tape is easily damaged to electronic components when used at high temperatures, and it is difficult to achieve effective anti-static functions, resulting in accumulation of static charges and dust adsorption, which damages the components.

Method used

By composite modification of the base layer of the cover belt, a composite base layer with flexibility and wear resistance was prepared, and a thermoplastic elastomer was used to perform nucleophilic addition reaction to form an anti-static function and good flow performance. Adhesive anti-static coating and prepare heat sealed tape covers in combination with lamination technology.

Benefits of technology

It achieves a good bonding effect at lower temperatures, reduces the risk of damage to electronic components, and has good anti-static properties, ensuring the safety and anti-static functions of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses an anti-static heat-sealing cover tape and a preparation method thereof, and belongs to the technical field of preparation of layered products for electronic component packaging. The preparation method comprises the following step: processing the composite base material layer and the adhesive anti-static coating under the lamination pressure of 0.5-2 MPa. The base material layer of the cover tape is subjected to composite modification to obtain the composite base material layer with good flexibility and wear resistance, then a thermoplastic elastomer with good hot working plasticity is used as an adhesive base material, and through a grafting reaction of nucleophilic addition, the wear resistance of the cover tape is improved. The bonding anti-static coating with the anti-static function and the good flowing property is prepared, finally, the composite base material layer and the bonding anti-static coating form the heat sealing belt cover through the laminating technology, and the heat sealing belt cover has the good low-temperature heat sealing and anti-static functions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of layered products for electronic component packaging, and in particular relates to an antistatic heat-sealing cover tape and a preparation method thereof. Background Art

[0002] Cover tape, commonly known as "cover film" or "package cover tape", is an important material used to protect components during the packaging process of electronic components. It is generally made of plastic, metal or other composite materials, and is mainly used to cover and protect electronic components such as chips, sensors and discrete components. Cover tape is mainly used in the electronic component mounting industry. It is used in conjunction with carrier tape to carry and store electronic components such as resistors, capacitors, transistors, diodes, etc. in the pockets of the carrier tape. The cover tape is sealed above the pockets formed by the carrier tape to form a closed package to protect the electronic components from contamination and damage during transportation. When the electronic components are mounted, the cover tape is peeled off, and the automatic mounting equipment takes out the components in the pockets one by one through the precise positioning of the index holes of the carrier tape, and mounts them on the integrated circuit board.

[0003] The cover tape is usually divided into two types: pressure-sensitive sealing and heat-sensitive sealing. Pressure-sensitive sealing refers to applying continuous pressure through the pressure roller of the sealing machine so that the pressure-sensitive adhesive on the cover tape adheres to the carrier tape to achieve the wrapping of electronic components. However, this method has high requirements on the pressure resistance of the carrier tape material. If the pressure resistance is low, it is easy to cause the carrier tape to be squeezed and crushed during pressure-sensitive sealing, thereby damaging the electronic components. Heat-sensitive sealing is a more commonly used technical method at present. It uses a sealing machine to apply a certain temperature and pressure to melt the hot melt adhesive of the cover tape and press it on the sealing surface of the carrier tape to achieve sealing. The advantage of this method is that the heat-sensitive tape used for heat-sensitive sealing is not sticky at room temperature and only has stickiness when heated. In addition, the sealing pressure required is small and will not cause damage to the carrier tape. When the cover tape is peeled off, it is easy to accumulate charges due to friction, thereby generating static electricity. These static electricity easily lead to the adsorption of dust and damage to electronic components. Therefore, it is of great value to involve a cover tape with anti-static function.

[0004] Patent CN107791638A discloses a cover tape and a method for using the same. The invention provides dotted cuts on the cover tape body near the edges on both sides, the cover tape body between the two dotted cuts is a peeling zone, and the cover tape body outside the two dotted cuts is a heat-sealing zone; the cover tape body includes a substrate layer, an antistatic film and a protective wax layer are sequentially arranged upward on the upper surface of the substrate layer, and an antistatic agent is distributed in the antistatic film; a pressure-sensitive adhesive layer and a mask layer are sequentially arranged downward in the central area of ​​the peeling zone on the lower surface of the substrate layer, the upper surface of the pressure-sensitive adhesive layer is bonded to the lower surface of the substrate layer, and the lower surface of the pressure-sensitive adhesive layer is bonded to the upper surface of the mask layer; a polyurethane glue layer, a composite layer, a bearing layer and a heat-sealing layer are sequentially arranged downward in the two side areas of the lower surface of the substrate layer corresponding to the heat-sealing zones on both sides, and the antistatic function is achieved by adjusting the material proportions of the mask layer, the composite layer, the bearing layer and the heat-sealing layer.

[0005] Patent CN115027115A discloses an environmentally friendly composite cover tape and its preparation process. The invention designs a composite cover tape having a PET layer, a PE layer and a TPE layer, and then composites the raw materials used for the PE layer and the TPE layer, and controls the weight ratio of the ethylene / sodium methacrylate copolymer in the TPE layer raw material, thereby achieving antistatic performance.

[0006] Although the above two patents realize the anti-static function of the cover tape, since the heat sealing temperature is mostly above 100°C, within this temperature range, if the heat cannot be dissipated to the environment in time, it is easy to have a "fatal effect" on the electronic components, causing the electronic components to be damaged and unusable.

[0007] Therefore, it is of great significance to develop an anti-static device that can avoid the adverse effects of excessively high heat sealing temperatures on electronic components. Summary of the invention

[0008] In view of the deficiencies of the prior art, the present invention performs composite modification on the base material layer of the cover tape to obtain a composite base material layer with good flexibility and wear resistance, and then uses a thermoplastic elastomer with good hot processing plasticity as an adhesive base material, and prepares an adhesive antistatic coating with antistatic function and good flow performance through a nucleophilic addition grafting reaction, and finally forms a heat-sealed tape cover by laminating the composite base material layer and the adhesive antistatic coating, thereby solving the technical problems raised in the background technology. Specifically, the technical solution of the present invention includes the following contents: The invention discloses a heat-sealing cover tape capable of preventing static electricity. The heat-sealing bag cover is composed of a composite substrate layer and an adhesive antistatic coating layer.

[0009] Furthermore, the method for preparing the composite substrate layer comprises the following steps: Aramid material, polyurethane material and epoxy resin material are mixed in a weight ratio of 1:2-3:1-2, and then blended in a temperature environment of 170°C-200°C for 10min-15min to obtain a blend, and the blend is poured into a mold and naturally cooled to form the composite substrate layer.

[0010] Furthermore, the aramid material is aramid chopped fibers, the polyurethane material is polyester TPU2, and the epoxy resin material is HY604-810 solid epoxy resin, HY604-820 solid epoxy resin or HY604-850 solid epoxy resin.

[0011] Furthermore, the preparation method of the adhesive antistatic coating comprises the following steps: The thermoplastic elastomer is treated with oxygen plasma to obtain a hydroxylated thermoplastic elastomer; The hydroxylated thermoplastic elastomer, the conductive polymer containing a secondary amine structure and the diisocyanate coupling agent are dispersed in an organic solvent in a weight ratio of 1-2:0.05-0.1:2-4 to form a reaction liquid. The reaction liquid is mixed and stirred with an organic weak base catalyst in a weight ratio of 1:0.1-0.2, and then heated to 70°C-80°C for reaction for 4h-8h to obtain the adhesive antistatic coating.

[0012] Furthermore, the thermoplastic elastomer is polystyrene butadiene copolymer or polystyrene-block-polyisoprene-block-polystyrene.

[0013] Furthermore, the conditions of the oxygen plasma treatment include an oxygen flow rate of 60 sccm to 100 sccm, a voltage of 300 V to 320 V, a treatment distance of 20 mm to 25 mm, and a treatment time of 60 s to 150 s.

[0014] Furthermore, the conductive polymer containing a secondary amine structure is polyaniline or polypyrrole.

[0015] Furthermore, the diisocyanate coupling agent is isophorone diisocyanate, 4,4'-diisocyanate dicyclohexylmethane, hexamethylene diisocyanate or trimethylhexamethylene diisocyanate.

[0016] Furthermore, the organic solvent includes N-methylpyrrolidone or N,N-dimethylformamide.

[0017] Furthermore, the usage amount of the organic solvent is 1 to 2 times of the total weight of the hydroxylated thermoplastic elastomer, the conductive polymer containing a secondary amine structure and the diisocyanate coupling agent.

[0018] Furthermore, the organic weak base catalyst includes triethylamine, diethanolamine or pyridine.

[0019] A method for preparing an antistatic heat-sealing cover tape, the method comprising the following steps: The composite substrate layer and the adhesive antistatic coating are processed by lamination pressure of 0.5MPa~2MPa.

[0020] Compared with the prior art, the present invention has the following beneficial effects: The present invention first modifies the base material layer of the cover tape, and utilizes the characteristics of aramid material with high strength and tear resistance and polyurethane material and epoxy resin material with good flexibility, through compound matching and high-temperature blending, a composite base material layer with both flexibility and strength is obtained. Then, utilizing the property of thermoplastic elastomer that it is easy to process at high temperature, first plasma oxidation is performed on it to obtain hydroxyl groups on its surface, and then utilizing the positive charge of carbon atoms on the isocyanate group of the reactive group of the diisocyanate coupling agent, the secondary amine group on the conductive polymer containing the secondary amine structure can be used as a nucleophilic reagent to initiate nucleophilic addition to the carbon atom of the isocyanate group to form a urea structure, and the hydroxyl group on the hydroxylated thermoplastic elastomer obtained after plasma oxidation acts as a nucleophilic reagent to initiate nucleophilic attack on the carbon atom of another isocyanate group to form an amide structure, and through the nucleophilic addition grafting reaction system, the conductive polymer containing the secondary amine structure with conductive properties is introduced into the thermoplastic elastomer, thereby realizing antistatic modification. Thermoplastic elastomers and diisocyanate coupling agents have flexible structures such as longer carbon chains with greater freedom and saturated carbon ring structures with good freedom, which make it easy for the polymer to bend and rotate freely. As a result, the finally prepared adhesive antistatic coating has good flow properties. The adhesive antistatic coating with good flowability can achieve good adhesion at lower temperatures, reducing the adverse effects of heat sealing at excessively high temperatures that can easily cause damage to electronic components. DETAILED DESCRIPTION

[0021] The technical solution of the present invention will be clearly and completely described below through the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0022] Unless otherwise specified, the raw materials and reagents used in the present invention are commercially available or can be prepared by known methods.

[0023] Aramid chopped fibers were purchased from Yantai Taihexing Materials Technology Co., Ltd.; Polyester TPU2 was purchased from Zhejiang Huafeng Thermoplastic Polyurethane Co., Ltd.; HY604-810 solid epoxy resin, HY604-820 solid epoxy resin or HY604-850 solid epoxy resin is purchased from Anhui Hengyuan Technology Co., Ltd.

[0024] Preparation Example 1: The preparation method of the composite substrate layer specifically includes the following steps: 1 part by weight of aramid chopped fiber, 2 parts by weight of polyester TPU2 and 1 part by weight of HY604-810 solid epoxy resin were placed in a vacuum drying oven at 60°C for 12 hours. Then they were placed in an extruder, the extruder was heated to 170°C, and the mixture was blended at a speed of 50 r / min for 10 minutes. After the blending was completed, the obtained blend was poured into a flat mold and cooled naturally to form a composite substrate layer.

[0025] Preparation Example 2: The preparation method of the composite substrate layer specifically includes the following steps: 1 part by weight of aramid chopped fiber, 2.5 parts by weight of polyester TPU2 and 1 part by weight of HY604-810 solid epoxy resin were placed in a vacuum drying oven at 60°C for 12 hours. Then they were placed in an extruder, the extruder was heated to 180°C, and the mixture was blended at a speed of 50 r / min for 12 minutes. After the blending was completed, the obtained blend was poured into a flat mold and cooled naturally to form a composite substrate layer.

[0026] Preparation Example 3: The preparation method of the composite substrate layer specifically includes the following steps: 1 part by weight of aramid chopped fiber, 2.5 parts by weight of polyester TPU2 and 1.5 parts by weight of HY604-820 solid epoxy resin were placed in a vacuum drying oven at 60°C for 12 hours. Then they were placed in an extruder, the extruder was heated to 190°C, and the mixture was blended at a speed of 100 r / min for 12 minutes. After the blending was completed, the obtained blend was poured into a flat mold and cooled naturally to form a composite substrate layer.

[0027] Preparation Example 4: The preparation method of the composite substrate layer specifically includes the following steps: 1 part by weight of aramid short-cut fiber, 3 parts by weight of polyester TPU2 and 1.5 parts by weight of HY604-820 solid epoxy resin were placed in a vacuum drying oven at 60°C for 12 hours. Then they were placed in an extruder, the extruder was heated to 200°C, and the mixture was blended at a speed of 100 r / min for 14 minutes. After the blending was completed, the obtained blend was poured into a flat mold and cooled naturally to form a composite substrate layer.

[0028] Preparation Example 5: The preparation method of the composite substrate layer specifically includes the following steps: 1 part by weight of aramid chopped fiber, 3 parts by weight of polyester TPU2 and 2 parts by weight of HY604-850 solid epoxy resin were placed in a vacuum drying oven at 60°C for 12 hours. Then they were placed in an extruder, the extruder was heated to 200°C, and the mixture was blended at a speed of 150 r / min for 15 minutes. After the blending was completed, the obtained blend was poured into a flat mold and cooled naturally to form a composite substrate layer.

[0029] Preparation Example 6: The preparation method of the composite substrate layer specifically includes the following steps: 2 parts by weight of aramid chopped fibers, 3 parts by weight of polyester TPU2 and 2 parts by weight of HY604-850 solid epoxy resin were placed in a vacuum drying oven at 60°C for 12 hours. Then they were placed in an extruder, the extruder was heated to 200°C, and the mixture was blended at a speed of 150 r / min for 15 minutes. After the blending was completed, the obtained blend was poured into a flat mold and cooled naturally to form a composite substrate layer.

[0030] Preparation Example 7: The preparation method of the composite substrate layer specifically includes the following steps: 3 parts by weight of polyester TPU2 and 2 parts by weight of HY604-850 solid epoxy resin were placed in a vacuum drying oven at 60°C for 12 hours. Then they were placed in an extruder, the extruder was heated to 200°C, and the mixture was blended at a speed of 150 r / min for 15 minutes. After the blending was completed, the obtained blend was poured into a flat mold and cooled naturally to form a composite substrate layer.

[0031] The composite substrate layers obtained in Preparation Examples 1 to 7 were tested for impact performance and bending performance according to "GB / T 2571-1995 Impact Test Method for Resin Castings" and "GB / T 2570-1995 Bending Performance Test Method for Resin Castings", and the deformation was observed. The results are shown in the following table: in conclusion: (1) It can be seen from the data in the above table that under certain preparation conditions, Preparation Examples 1 to 5 exhibit good bending toughness and impact strength. This property helps to reduce the adverse effects of damage to electronic components caused by deformation or breakage of the cover tape due to external forces.

[0032] (2) In Preparation Example 6, due to the excessive use of high-strength aramid chopped fibers, the strength of the composite substrate layer is increased, but the flexibility is greatly reduced, the impact resistance is reduced, and it is easy to crack and break when impacted.

[0033] (3) In Preparation Example 7, due to the removal of aramid chopped fibers, the obtained composite substrate layer has good impact strength, but due to its high bending toughness, it may cause excessive deformation of the material during stretching or compression, causing damage to electronic components. In addition, the high bending toughness makes it difficult to shape and utilize.

[0034] Preparation Example 8: The preparation method of the adhesive antistatic coating specifically includes the following steps: Oxygen was introduced into the plasma processor at a gas flow rate of 60 sccm, and a voltage of 300 V was turned on for test injection. After adjustment, the polystyrene butadiene copolymer was placed 20 mm below the nozzle of the plasma processor, and then oxygen plasma was injected for 60 seconds. After the treatment, the polystyrene butadiene copolymer was naturally cooled to obtain a hydroxylated polystyrene butadiene copolymer.

[0035] 1 part by weight of hydroxylated polystyrene butadiene copolymer, 0.05 part by weight of polyaniline and 2 parts by weight of isophorone diisocyanate were placed in 3.05 parts by weight of N-methylpyrrolidone and stirred and dispersed uniformly to obtain a reaction solution, and then the reaction solution was mixed with 0.305 parts by weight of triethylamine and stirred and heated to 70°C for a timed reaction of 4 hours. After the reaction was completed, the solution was poured into ice ethanol and allowed to stand for precipitation, and then filtered and separated and naturally dried to obtain an adhesive antistatic coating.

[0036] Preparation Example 9: The preparation method of the adhesive antistatic coating specifically includes the following steps: Oxygen was introduced into the plasma processor at a gas flow rate of 70 sccm, and a voltage of 300 V was turned on for test injection. After adjustment, the polystyrene butadiene copolymer was placed 20 mm below the nozzle of the plasma processor, and then oxygen plasma was injected for 90 seconds. After the treatment, the hydroxylated polystyrene butadiene copolymer was obtained by natural cooling.

[0037] 1 part by weight of hydroxylated polystyrene butadiene copolymer, 0.06 parts by weight of polyaniline and 2.5 parts by weight of isophorone diisocyanate were placed in 3.56 parts by weight of N-methylpyrrolidone and stirred and dispersed uniformly to obtain a reaction solution, and then the reaction solution was mixed with 0.356 parts by weight of triethylamine and stirred and heated to 72°C for a timed reaction of 5 hours. After the reaction was completed, the solution was poured into ice ethanol and allowed to stand for precipitation, and then filtered and separated and naturally dried to obtain an adhesive antistatic coating.

[0038] Preparation Example 10: The preparation method of the adhesive antistatic coating specifically includes the following steps: Oxygen was introduced into the plasma processor at a gas flow rate of 80 sccm, and a voltage of 310 V was turned on for test injection. After adjustment, the polystyrene butadiene copolymer was placed 23 mm below the nozzle of the plasma processor, and then oxygen plasma was injected for 90 seconds. After the treatment, the polystyrene butadiene copolymer was naturally cooled to obtain a hydroxylated polystyrene butadiene copolymer.

[0039] 1.5 parts by weight of hydroxylated polystyrene butadiene copolymer, 0.07 parts by weight of polyaniline and 3 parts by weight of 4,4'-diisocyanate dicyclohexylmethane were placed in 4.57 parts by weight of N-methylpyrrolidone and stirred and dispersed evenly to obtain a reaction solution, and then the reaction solution was stirred with 0.457 parts by weight of diethylamine alcoholamine and heated to 74°C for a timed reaction of 6 hours. After the reaction was completed, the solution was poured into ice ethanol and allowed to stand for precipitation, and then filtered and separated and naturally dried to obtain an adhesive antistatic coating.

[0040] Preparation Example 11: The preparation method of the adhesive antistatic coating specifically includes the following steps: Oxygen was introduced into the plasma processor at a gas flow rate of 90 sccm, and a voltage of 310 V was turned on for test injection. After adjustment, polystyrene-block-polyisoprene-block-polystyrene was placed 23 mm below the nozzle of the plasma processor, and then oxygen plasma was injected for 120 seconds. After the treatment, the mixture was naturally cooled to obtain hydroxylated polystyrene-block-polyisoprene-block-polystyrene.

[0041] 1.5 parts by weight of hydroxylated polystyrene-block-polyisoprene-block-polystyrene, 0.08 parts by weight of polypyrrole and 3.5 parts by weight of hexamethylene diisocyanate were placed in 10.16 parts by weight of N,N-dimethylformamide and stirred and dispersed uniformly to obtain a reaction solution, and then the reaction solution was stirred with 2.032 parts by weight of diethylamine and heated to 76°C for a timed reaction of 7 hours. After the reaction was completed, the solution was poured into ice ethanol and allowed to stand for precipitation, and then filtered and separated and naturally dried to obtain an adhesive antistatic coating.

[0042] Preparation Example 12: The preparation method of the adhesive antistatic coating specifically includes the following steps: Oxygen was introduced into the plasma processor at a gas flow rate of 100 sccm, and a voltage of 320 V was turned on for test injection. After adjustment, polystyrene-block-polyisoprene-block-polystyrene was placed 25 mm below the nozzle of the plasma processor, and then oxygen plasma was injected for 120 seconds. After the treatment, the mixture was naturally cooled to obtain hydroxylated polystyrene-block-polyisoprene-block-polystyrene.

[0043] 2 parts by weight of hydroxylated polystyrene-block-polyisoprene-block-polystyrene, 0.09 parts by weight of polypyrrole and 4 parts by weight of hexamethylene diisocyanate were placed in 12.18 parts by weight of N,N-dimethylformamide and stirred and dispersed uniformly to obtain a reaction solution, and then the reaction solution was stirred with 2.436 parts by weight of pyridine and heated to 78°C for a timed reaction of 8 hours. After the reaction was completed, the solution was poured into ice ethanol and allowed to stand for precipitation, and then filtered and separated and naturally dried to obtain an adhesive antistatic coating.

[0044] Preparation Example 13: The preparation method of the adhesive antistatic coating specifically includes the following steps: Oxygen was introduced into the plasma processor at a gas flow rate of 100 sccm, and a voltage of 320 V was turned on for test injection. After adjustment, polystyrene-block-polyisoprene-block-polystyrene was placed 25 mm below the nozzle of the plasma processor, and then oxygen plasma was injected for 150 seconds. After the treatment, the mixture was naturally cooled to obtain hydroxylated polystyrene-block-polyisoprene-block-polystyrene.

[0045] 2 parts by weight of hydroxylated polystyrene-block-polyisoprene-block-polystyrene, 0.1 parts by weight of polypyrrole and 4 parts by weight of trimethylhexamethylene diisocyanate were placed in 12.2 parts by weight of N,N-dimethylformamide and stirred and dispersed uniformly to obtain a reaction solution, and then the reaction solution was stirred with 2.44 parts by weight of pyridine and heated to 80°C for a timed reaction of 8 hours. After the reaction was completed, the solution was poured into ice ethanol and allowed to stand for precipitation, and then filtered and separated and naturally dried to obtain an adhesive antistatic coating.

[0046] Preparation Example 14: The preparation method of the adhesive antistatic coating specifically includes the following steps: The trimethylhexamethylene diisocyanate in Preparation Example 13 was replaced by toluene diisocyanate, and the other conditions remained the same as those in Preparation Example 13.

[0047] Preparation Example 15: The preparation method of the adhesive antistatic coating specifically includes the following steps: The trimethylhexamethylene diisocyanate in Preparation Example 13 was replaced with diphenylmethane-4,4'-diisocyanate, and the other conditions remained the same as those in Preparation Example 13.

[0048] Preparation Example 16: The preparation method of the adhesive antistatic coating specifically includes the following steps: The polypyrrole in Preparation Example 13 was replaced by carbon black, and the other conditions remained the same as those in Preparation Example 13.

[0049] Preparation Example 17: The preparation method of the adhesive antistatic coating specifically includes the following steps: The polypyrrole in Preparation Example 13 was replaced by conductive graphene, and the other conditions remained the same as those in Preparation Example 13.

[0050] Preparation Example 18: The preparation method of the adhesive antistatic coating specifically includes the following steps: 2 parts by weight of polystyrene-block-polyisoprene-block-polystyrene, 0.1 parts by weight of polypyrrole and 4 parts by weight of trimethylhexamethylene diisocyanate were placed in 12.2 parts by weight of N,N-dimethylformamide and stirred and dispersed uniformly to obtain a reaction solution, and then the reaction solution was stirred with 2.44 parts by weight of pyridine and heated to 80°C for a timed reaction of 8 hours. After the reaction was completed, the solution was poured into ice ethanol and allowed to stand for precipitation, and then filtered and separated and naturally dried to obtain an adhesive antistatic coating.

[0051] Embodiment 1: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The composite substrate layer obtained in Preparation Example 1 and the adhesive antistatic coating obtained in Preparation Example 8 were respectively controlled to have a thickness of 20 μm and 10 μm using a blade coater, and then the 20 μm thick composite substrate layer and the 10 μm thick adhesive antistatic coating were processed at a lamination pressure of 0.5 MPa.

[0052] Embodiment 2: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The composite substrate layer obtained in Preparation Example 2 and the adhesive antistatic coating obtained in Preparation Example 9 were respectively controlled to have a thickness of 22 μm and 12 μm using a blade coater, and then the 22 μm thick composite substrate layer and the 12 μm thick adhesive antistatic coating were obtained by lamination pressure processing at 0.5 MPa.

[0053] Embodiment 3: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The composite substrate layer obtained in Preparation Example 3 and the adhesive antistatic coating obtained in Preparation Example 10 were respectively controlled to have a thickness of 24 μm and 14 μm using a blade coater, and then the 24 μm thick composite substrate layer and the 14 μm thick adhesive antistatic coating were obtained by processing at a lamination pressure of 1 MPa.

[0054] Embodiment 4: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The composite substrate layer obtained in Preparation Example 4 and the adhesive antistatic coating obtained in Preparation Example 11 were respectively controlled to have a thickness of 26 μm and 16 μm using a blade coater, and then the 26 μm thick composite substrate layer and the 16 μm thick adhesive antistatic coating were obtained by lamination pressure processing at 1 MPa.

[0055] Embodiment 5: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The composite substrate layer obtained in Preparation Example 5 and the adhesive antistatic coating obtained in Preparation Example 12 were respectively controlled to have a thickness of 28 μm and 18 μm using a blade coater, and then the 28 μm thick composite substrate layer and the 18 μm thick adhesive antistatic coating were obtained by lamination pressure processing at 1.5 MPa.

[0056] Embodiment 6: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The composite substrate layer obtained in Preparation Example 5 and the adhesive antistatic coating obtained in Preparation Example 13 were respectively controlled to have a thickness of 28 μm and 20 μm using a blade coater, and then the 28 μm thick composite substrate layer and the 20 μm thick adhesive antistatic coating were obtained by lamination pressure processing at 2 MPa.

[0057] Comparative Example 1: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The adhesive antistatic coating in Example 6 was replaced by the adhesive antistatic coating obtained in Preparation Example 14, and the other conditions remained the same as in Example 6.

[0058] Comparative Example 2: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The adhesive antistatic coating in Example 6 was replaced by the adhesive antistatic coating obtained in Preparation Example 15, and the other conditions remained the same as in Example 6.

[0059] Comparative Example 3: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The adhesive antistatic coating in Example 6 was replaced by the adhesive antistatic coating obtained in Preparation Example 16, and the other conditions remained the same as in Example 6.

[0060] Comparative Example 4: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The adhesive antistatic coating in Example 6 was replaced by the adhesive antistatic coating obtained in Preparation Example 17, and the other conditions remained the same as in Example 6.

[0061] Comparative Example 5: A method for preparing an antistatic heat-sealing cover tape specifically comprises the following steps: The adhesive antistatic coating in Example 6 was replaced by the adhesive antistatic coating obtained in Preparation Example 18, and the other conditions remained the same as in Example 6.

[0062] Comparative Example 6: The thickness of the composite substrate layer and the adhesive antistatic coating in Example 6 were increased to 30 μm for the composite substrate layer and 22 μm for the adhesive antistatic coating, respectively, and the other conditions remained the same as in Example 6.

[0063] The surface resistance values ​​of the antistatic heat-sealing cover tapes obtained in Examples 1 to 6 and Comparative Examples 1 to 6 were measured using an AS982 surface resistance tester. Heat sealing was then performed at 50° C. and the peel strength was measured. The results are shown in the following table: From the data in the above table, we can see that: (1) The antistatic heat-sealing cover tapes of Examples 1 to 6 have low surface resistance, good electrical conductivity, are conducive to the release of static electricity, have good antistatic function, and can be heat-sealed at a relatively low temperature of 50°C, reducing the adverse effects of high-temperature sealing on electronic components. The peel strength after sealing is good, indicating that the heat sealing effect can be achieved.

[0064] (2) It can be seen from Comparative Examples 1 and 2 that although they have low surface resistance and good antistatic effect, due to the rigid benzene ring structure of toluene diisocyanate and diphenylmethane-4,4'-diisocyanate, the material has poor fluidity and cannot be heat-sealed at a relatively low temperature. It may be necessary to further increase the heat-sealing temperature. However, a higher heat-sealing temperature will have an adverse effect on electronic components.

[0065] (3) It can be seen from Comparative Examples 3 and 4 that although carbon black and conductive graphene have good conductive properties, conventional mixing easily produces agglomeration, resulting in uneven distribution of carbon black and conductive graphene, making it difficult to form a continuous and uniform conductive path, and thus the antistatic effect is poor.

[0066] (4) Comparative Example 5 shows that since polystyrene-block-polyisoprene-block-polystyrene does not have a functional group that can react with trimethylhexamethylene diisocyanate, it is difficult to improve the antistatic effect by simple mixing.

[0067] (5) It can be seen from Comparative Example 6 that a cover tape that is too thick may require a higher temperature to achieve heat sealing, and high temperature is not conducive to the protection of electronic components.

[0068] The above-described embodiments provide a detailed description of the technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected.

Claims

1. A heat-sealing cover tape capable of preventing static electricity, characterized in that: The heat-sealed bag cover is composed of a composite substrate layer and an adhesive antistatic coating.

2. The antistatic heat-sealing cover tape according to claim 1, characterized in that: The preparation method of the composite substrate layer comprises the following steps: Aramid material, polyurethane material and epoxy resin material are mixed in a weight ratio of 1:2-3:1-2, and then blended in a temperature environment of 170°C-200°C for 10min-15min to obtain a blend, and the blend is poured into a mold and naturally cooled to form the composite substrate layer.

3. The antistatic heat-sealing cover tape according to claim 2, characterized in that: The aramid material is aramid chopped fibers, the polyurethane material is polyester TPU2, and the epoxy resin material is HY604-810 solid epoxy resin, HY604-820 solid epoxy resin or HY604-850 solid epoxy resin.

4. The antistatic heat-sealing cover tape according to claim 1, characterized in that: The preparation method of the adhesive antistatic coating comprises the following steps: The thermoplastic elastomer is treated with oxygen plasma to obtain a hydroxylated thermoplastic elastomer; The hydroxylated thermoplastic elastomer, the conductive polymer containing a secondary amine structure and the diisocyanate coupling agent are dispersed in an organic solvent in a weight ratio of 1-2:0.05-0.1:2-4 to form a reaction liquid. The reaction liquid is mixed and stirred with an organic weak base catalyst in a weight ratio of 1:0.1-0.2, and then heated to 70°C-80°C for reaction for 4h-8h to obtain the adhesive antistatic coating.

5. The antistatic heat-sealing cover tape according to claim 4, characterized in that: The thermoplastic elastomer is polystyrene butadiene copolymer or polystyrene-block-polyisoprene-block-polystyrene.

6. The antistatic heat-sealing cover tape according to claim 4, characterized in that: The conditions of the oxygen plasma treatment include an oxygen flow rate of 60 sccm to 100 sccm, a voltage of 300 V to 320 V, a treatment distance of 20 mm to 25 mm, and a treatment time of 60 s to 150 s.

7. The antistatic heat-sealing cover tape according to claim 4, characterized in that: The conductive polymer containing a secondary amine structure is polyaniline or polypyrrole.

8. The antistatic heat-sealing cover tape according to claim 4, characterized in that: The diisocyanate coupling agent is isophorone diisocyanate, 4,4'-diisocyanate dicyclohexylmethane, hexamethylene diisocyanate or trimethylhexamethylene diisocyanate.

9. The antistatic heat-sealing cover tape according to claim 4, characterized in that: The organic weak base catalyst includes triethylamine, diethanolamine or pyridine.

10. A method for preparing an antistatic heat-sealing cover tape as claimed in any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: The composite substrate layer and the adhesive antistatic coating are processed by lamination pressure of 0.5MPa~2MPa.

Citation Information

Patent Citations

  • Cover belt and use method thereof

    CN107791638A

  • Environment-friendly composite cover tape and preparation process thereof

    CN115027115A

  • Antistatic pad and tray as well as manufacturing method thereof

    CN103552334A

  • Long aramid fiber-reinforced wear-resistant thermoplastic polyurethane (TPU) composite material and preparation method thereof

    CN103819892A

  • Heat-sealing type middle decapping tape and preparation method of heat-sealing type middle decapping tape

    CN113478931A

Cited By

  • Novel heat-sealing cover tape and preparation method thereof

    CN119773323A