Flexible polyurethane foam and its formulation
By using a combination of surface-treated low-surface area silica and tertiary amine catalysts in flexible polyurethane foam, the problem of difficulty in incorporating gas phase silica in in situ method is solved, and the mechanical properties and polymerization stability of the foam are improved, achieving the realization of the process. High resilience and low dry compression permanent deformation effect.
Patent Information
- Application Number
- CN202180067912.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-09-29
Smart Images

Figure CN116323736B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to formulations for flexible polyurethane foams and polymer foams made therefrom. Background Art
[0002] The term "polyurethane" describes a wide variety of polymer compositions. Each of these polymer compositions contains a polymer whose repeating units include -N-CO-O- bonds. In addition, polyurethanes may also include urea (-N-CO-N-) bonds. However, the composition of the molecular chains between these polyurethanes and the urea bonds and the method of making the polymer also affect the final properties. Therefore, polyurethanes with different compositions and / or made by different methods are used in various applications, ranging from adhesives to coatings to elastomers to different types of foams. Typically, polyurethanes are produced by reacting polyisocyanates with polyols (or polyamines to produce polyureas). Two different polyols can be used to produce block copolymers. For example, low molecular weight diols and diamines lead to the formation of short chains that associate to form crystalline domains by hydrogen bonds. A second "softer" block can be formed by using polyether or polyester polyols, which leads to amorphous domains. Such block copolymer compositions are typically used to form thermoplastic polyurethanes (TPUs). The tensile properties of the polymer depend on how the tensile force interferes with the hydrogen bonds in the crystalline domains.
[0003] Alternatively, polyurethane foam is typically formed by the reaction of diisocyanates with polyols and polyamines in the presence of a blowing agent. Mechanical properties depend in part on the contrast between rigid urea bonds and more flexible polyurethane bonds, rather than utilizing crystalline domains. The blowing agent may be an adjuvant, such as a volatile organic compound, or may be generated in situ. Adding water to the reaction mixture results in two competing reactions, polycondensation and generation of carbon dioxide by the reaction between isocyanate and water. Increasing the functionality of polyols and isocyanates increases the crosslinking density earlier during polymerization, strengthens the cell walls, and prevents the increased carbon dioxide pressure from destroying the cell walls to a great extent, thereby increasing the rigidity of the foam. Rigid (closed cell) polyurethane foam is typically used for thermal insulation, while flexible (open cell) polyurethane foam is used for cushioning and sound insulation.
[0004] Various fillers are commonly used in polyurethanes to modify their mechanical, electrical and other properties. These fillers can be combined with polymeric materials, such as by melt mixing, or incorporated into the prepolymer composition prior to polycondensation in an in-situ process. Fillers used in an in-situ process must fulfill two functions. Not only do they need to provide the desired properties to the final product, but they must also not interfere with the polymerization and foaming process to produce the product.
[0005] Fumed silica is often used to control the thixotropy and pore size of polyurethane foams. In JP04850574, fumed silica is melt-mixed into a polymerized polyurethane composition, and then carbon dioxide is injected to create pores. Similarly, fumed silica is used as a foam stabilizer in US20080153935. Nevertheless, it is still desirable to incorporate fumed silica into flexible polyurethane foams (wherein fumed silica is combined with precursor materials before polycondensation) in an in-situ method, and to allow silica to contribute to the mechanical properties of the final material. Summary of the invention
[0006] The use of low surface area silica having trimethylsilyl groups at the surface in combination with a tertiary amine catalyst enables an in situ polymerization process to produce flexible polyurethane foams with beneficial properties.
[0007] In one embodiment, a method of producing a flexible polyurethane foam comprises providing a polyol comprising at least a first polyol and up to 10 wt % of a polyol having a molecular weight of 50 to 150 m 2 / g surface area of fumed silica, the first polyol having a weight average molecular weight of 3000 to 6000 and a functionality of 2.5 to 3.5, wherein the fumed silica has a C1-C3 alkylsilyl group at its surface, the polyol composition, a polyisocyanate having a functionality of 1.8 to 2.5, water and a tertiary amine catalyst are combined to form a prepolymer composition, and the prepolymer composition is allowed to polymerize to form an open-cell foam structure having a density of 1.8 to 4 pcf and a) at least 40%, such as 40% to 70% resilience, b) no more than 15%, such as 3% to 15% dry compression permanent deformation, or both. The flexible polyurethane foam can exhibit a density of 1.8 to 3 pcf or a density of 2 to 4 pcf.
[0008] The polyisocyanate may include hexamethylene diisocyanate (HDI), phenylene diisocyanate (PDI), 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), 4,4'-diphenylmethane diisocyanate (MDI), an isomer mixture of diphenylmethane diisocyanate, or a mixture of two or more of these. The first polyol may include a polyether polyol or a polyester polyol. The polyol composition may further include a second polyol having a weight average molecular weight of 2000 to 10000. The fumed silica may have a molecular weight of 50 to 150 m 2 / g or 50 to 100m 2The C1-C3 alkylsilyl group may be a trimethylsilyl group or a dimethylsilyl group.
[0009] The method may include loading the prepolymer composition into a mold having one side open to the atmosphere, and the resulting flexible polyurethane foam may have a density of 1.8 to 3 pcf. Alternatively, the method may include loading the prepolymer composition into a mold and closing the mold, and the resulting flexible polyurethane foam may have a density of 2 to 4 pcf.
[0010] The flexible polyurethane foam can have a compression force deflection (compression force deflection) at 50% as measured by ASTM D3574 that is increased by at least 30%, e.g., at least 50%, at least 70%, or from 30% to 155%, relative to a flexible polyurethane foam produced by the same process but replacing the silica with an equal mass portion of the first polyol.
[0011] In another embodiment, the flexible polyurethane foam comprises up to 10 wt % of a polyurethane having a molecular weight of 50 to 150 m 2 / g of surface area of fumed silica, wherein the fumed silica has C1-C3 alkyl silane groups on its surface, and the flexible polyurethane foam exhibits a resilience of at least 40%, such as 40% to 70%, a dry compression set of no more than 15%, such as 3% to 15%, or both. The fumed silica may have a surface area of 50 to 150 m 2 / g or 50 to 100m 2 The flexible polyurethane foam may be a molded foam or a free-rise foam. The polyurethane foam may comprise a polyether polyurethane or a polyester polyurethane. The flexible polyurethane foam may have a density of 1.8 to 4 pcf, such as a density of 1.8 to 3 pcf or a density of 2 to 4 pcf.
[0012] The flexible polyurethane foam can have a deflection at 50% compressive force as measured by ASTM D3574 that is at least 30%, e.g., at least 50%, at least 70%, or 30% to 155% greater than a flexible polyurethane foam of the same composition but replacing silica with a polyol.
[0013] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory only and are intended to provide further explanation of the invention as claimed. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] The present invention is described with reference to the several figures of the accompanying drawings, in which:
[0015] Figure 1 The viscosities of polyol dispersions prepared with fumed silica having different surface chemistries are shown.
[0016] Figure 2 The viscosities of polyol dispersions prepared with fumed silica having different surface areas are shown.
[0017] Figure 3 The viscosities of polyol dispersions prepared with hydrophobic and hydrophilic (untreated) fumed silica are shown. DETAILED DESCRIPTION
[0018] In one embodiment, a method of producing a flexible polyurethane foam comprises providing a polyol comprising at least a first polyol and up to 10 wt % of a polyol having a molecular weight of 50 to 150 m 2 / g of surface area of fumed silica, the first polyol having a weight average molecular weight of 3000 to 6000 and a functionality of 2.5 to 3.5, wherein the fumed silica has a C1-C3 alkylsilane group at its surface, combining the polyol composition, a polyisocyanate having a functionality of 1.8 to 2.5 (e.g., 1.8 to 2.25), water, and a tertiary amine catalyst to form a prepolymer composition, and allowing the prepolymer composition to polymerize under conditions forming an open-cell foam structure having a density of 1.8 to 4 pcf.
[0019] Flexible polyurethane foams are typically formed by the reaction of a diisocyanate with a polyol and a polyamine in the presence of a blowing agent. For flexible open-cell foams, the polyol typically has a functionality of 2.5-3.5, but polyols of higher functionality can be used in some cases. This results in less crosslinking than rigid foams with significantly higher polyol functionalities (e.g., 4.5 to 5). Likewise, the use of polyisocyanates with a functionality of up to 2.5, such as diisocyanates or polyisocyanates with a functionality of 1.8 to 2.25, also reduces the crosslink density compared to rigid foams with an isocyanate functionality typically of about 2.7 or more.
[0020] Suitable isocyanates for the formulations and methods provided herein include any organic isocyanates for polyurethane foams. Aromatic isocyanates are preferred, but aliphatic, alicyclic and araliphatic isocyanates may also be used. Exemplary isocyanates include m-phenylene diisocyanate, 2,4- and / or 2,6-toluene diisocyanate (TDI), various isomers of diphenylmethane diisocyanate (MDI), hexamethylene-1,6-diisocyanate, tetramethylene-1,4-diisocyanate, cyclohexane-1,4-diisocyanate, hexahydrotoluene diisocyanate, hydrogenated MDI (H12MDI), naphthalene-1,5-diisocyanate, methoxyphenyl-2,4-diisocyanate, 4,4′-biphenylene diisocyanate, 3,3′-dimethoxy-4, 4′-biphenyl diisocyanate, 3,3′-dimethyldiphenylmethane-4,4′-diisocyanate, 4,4′,4″-triphenylmethane triisocyanate, polymethylene polyphenyl isocyanate or a mixture thereof with MDI, hydrogenated polymethylene polyphenyl isocyanate, toluene-2,4,6-triisocyanate, and 4,4′-dimethyldiphenylmethane-2,2′,5,5′-tetraisocyanate, or mixtures of these. The triisocyanates are preferably used in admixture with sufficient diisocyanate to give an overall functionality of 2 to 2.25.
[0021] Suitable polymer polyols for formulations and methods provided herein include both polyether polyols and polyester polyols and other polymer polyols known to those skilled in the art. Suitable polyols typically have a molecular weight of 3000 to 6000, preferably a weight average molecular weight. Suitable polymer polyols for open-cell foams have a hydroxyl number of 2.5 to 3.5, for example, 2.5 to 3. Polyol mixtures may also be used. For example, polyols with lower or higher molecular weights may be combined to provide an average polyol molecular weight desired. Therefore, one or more other polyols with a weight average molecular weight of 2000 to 10000 may be combined with the first polyol.
[0022] Polyether polyols can be obtained by reacting small molecule polyols with alkylene oxides to form polyether polyols. Exemplary small molecule polyols include, but are not limited to, ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, trimethylene glycol, tetramethylene glycol, hexamethylene glycol, glycerol, diglycerol, sorbitol, pentaerythritol, sucrose, and bisphenol A. Exemplary polyethers include polyalkylene oxides such as polyethylene oxide, polypropylene oxide, and polytetramethylene oxide. Alternatively or in addition, polymer polyols can be produced by copolymerizing vinyl monomers such as styrene or acrylonitrile with polyols.
[0023] Polyester polyols can be obtained by reacting small molecule polyols (such as those described above) with polyesters. Exemplary polyesters include any polyester known to those skilled in the art for use in flexible polyurethane foams, and can be produced from organic dicarboxylic acids (such as C2-C12 unbranched aliphatic chains terminated with carboxylic acid groups) and difunctional or trifunctional alcohols (such as C2-C12 alkylene glycols or polyether alcohols).
[0024] Mixtures of polymer polyols may also be employed. Exemplary polymer polyols include those disclosed in US201800223030, US9034936, and US10119002 (the entire contents of which are incorporated herein by reference), provided that the polyol formulation (one or more polyols) should have an overall functionality (i.e., the number of hydroxyl groups per molecule) of 2.5 to 3.
[0025] Tertiary amine catalysts are preferred over metal and low-order amine catalysts to reduce competition between fumed silica and polyols for the catalyst. Exemplary tertiary amine catalysts include any tertiary amine catalyst known to those skilled in the art to be suitable for use in the production of polyurethane foams, including but not limited to dimethylethanolamine, triethylenediamine, tetramethylpropylenediamine, tetramethylhexamethylenediamine, and dimethylcyclohexylamine.
[0026] Other components known to those skilled in the art for open-cell polyurethane foams may also be used. Examples include surfactants, viscosity modifiers, crosslinking agents, chain extenders, pigments, flame retardants, auxiliary gelling catalysts, auxiliary blowing catalysts, and any combination of these. Other polyols may also be used to introduce different copolymers or functional groups into polyurethane, such as to promote pore formation or pore opening. Other fillers such as styrene acrylonitrile beads, barium sulfate or calcium carbonate may be used in combination with the fumed silica provided herein.
[0027] Fumed silica is typically produced by a pyrogenic process in which a gaseous feedstock containing a fuel (e.g., methane or hydrogen), oxygen, and a volatile silicon compound is fed into a burner. Water formed by the combustion of the fuel in oxygen reacts in liquid or gaseous form with the volatile silicon compound to produce silica particles. These particles coalesce and aggregate to form fumed silica.
[0028] During the formation of polyurethane foam, it is desirable to balance the properties of the formulation to coordinate the growth of carbon dioxide bubbles with the crosslinking of the polyol component. If the formulation is too viscous, the diffusion of carbon dioxide formed by the reaction of water and isocyanate will be slowed down. In addition, the expansion gas will not apply enough pressure to displace the liquid formulation and form bubbles of appropriate size. The silica dispersed in the liquid system affects its rheological properties through two different interactions. The first is the attraction between individual silica particles. The aggregated structure of fumed silica allows it to form a chain network that can be interrupted under agitation or shearing, making fumed silica an effective thixotropic adhesive. The formation of these networks is conducive to systems with high surface area (small primary particles) silica. Therefore, in a preferred embodiment, the fumed silica used herein has a surface area of not more than 150 m 2 / g, for example, not more than 130m 2 / g or not more than 100m 2 The second interaction is the interaction between the liquid matrix and the silica surface. In hydrophilic polyol systems, highly hydrophobic and surface-treated silica with low affinity for polyols is expected to have strong particle-particle interactions and promote high yield stress. In contrast, silica without surface treatment is well dispersed in liquids (e.g., water or methanol) and does not significantly change viscosity. Therefore, in complex formulations, careful modification of the silica surface can have a huge impact on system rheology.
[0029] The prepared fumed silica is hydrophilic and has multiple Si-OH groups on the surface. These silanol groups can interact with alcohol through hydrogen bonds, and interact with the oxyalkylene groups of polyethers through acid-base interactions. Therefore, untreated silica is expected to have a small impact on the viscosity of polyols. However, the hydroxyl groups of silica can compete with the hydroxyl groups of polyols in polymerization. The hydrophobization of silica has capped a certain proportion of silanol groups. However, hydrophobization also changes the interfacial interaction between silica and the prepolymer formulation and the final polymer, potentially changing the viscosity behavior of the prepolymer formulation and / or the mechanical properties of the flexible polyurethane foam. In addition, the hydrophobization treatment preferably does not interfere with the polymerization reaction.
[0030] It has been unexpectedly found that hydrophobization of fumed silica with agents that leave short alkylsilane groups on the surface reduces competition between silica and polymer polyols without undesirably increasing viscosity. In contrast, surface treatments with larger alkyl or siloxane chains on the surface are too hydrophobic and will adversely affect foam development. Preferred surface treatments leave C1-C3 alkylsilane groups on the surface, such as trimethylsilyl, dimethylsilyl, ethylsilane or methylethylsilane groups. The silane groups may be connected to the surface of the fumed silica by one, two or three siloxane bonds, or may be connected to one or two adjacent alkylsilane groups by siloxane bonds.
[0031] Thus, fumed silica can be hydrophobized with silazanes such as hexamethyldisilazane or alkylsilanes such as dimethyldichlorosilane, methyltrimethoxysilane, methyltrichlorosilane, methyltrimethoxysilane, methyltriethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, trimethylchlorosilane, trimethylmethoxysilane, trimethylethoxysilane, ethyltriethoxysilane, ethyltrichlorosilane, ethyltrimethoxysilane, propyltrichlorosilane, propyltrimethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, ethylmethyldichlorosilane and other C1-C3 linear and branched alkylsilanes.
[0032] The high surface area and branched structure of fumed silica also enhances its surface interaction with the surrounding polymer matrix. This interaction allows silica to reinforce polymer foams more effectively than sol-gel or precipitated silica. Therefore, it is desirable that the silica have sufficient surface area, for example, at least 50 or 60 m 2 / g to provide enhancement.
[0033] The components of the polyurethane can be combined and polymerized using any method known to those skilled in the art. Preferably, the fumed silica is dispersed in a polyol according to methods known to those skilled in the art, and can then be combined with one or more remaining non-isocyanate components of the polyurethane before being combined with a polyisocyanate and polymerized. The polyurethane foam can be a free-rise foam, wherein polymerization occurs in a container open to atmospheric pressure, or a molded foam, wherein polymerization occurs in a closed mold. The closed mold creates a limited space for the expansion of the polyurethane foam after the unpolymerized material is loaded into the mold. Therefore, the density of the foam can be partially controlled by changing the amount of material in the closed mold, and the density of the free-rise foam can be controlled by adjusting the formulation to control the generation of carbon dioxide and the relative rate of polymerization and carbon dioxide formation. The density of a typical free-rise foam is 1.8 to 3 pcf, while the density of a typical molded foam is 2 to 4 pcf.
[0034] For free rise or molded foam, the use of silica as described herein provides enhancement to the foam without significantly reducing the flexibility imparted by the open cell structure of the foam. Preferably, the polyurethane foam has a resilience of at least 40%, such as 40% to 70%. Alternatively or in addition, the polyurethane foam has a dry compression permanent deformation of not more than 15%, such as 3% to 15%. Alternatively or in addition, the addition of fumed silica as described herein improves the compressive force deflection. For example, relative to a silica-free formulation, the CFD at 50% measured by ASTM D3574, Test C can be increased by at least 30%, such as at least 50%, at least 70%, or 30% to 155%.
[0035] The present invention will be further illustrated by the following examples, which are intended to be merely exemplary in nature.
[0036] Example
[0037] Example 1
[0038] CAB-O-SIL TG-6110 hydrophobic fumed silica (with 85 m 2 / g BET surface area and trimethylsilyl groups at the surface) (Cabot Corporation) was dispersed in Pluracol 2090 polyether polyol triol (BASF) to form a 15wt% dispersion. The silica dispersion was produced in 350g batches using a SpeedMixer (Flackteck, Landrum, Sc) followed by a plenary mixer (PC Laborsystem Labotop). The polyol was weighed into a 600g plastic container and the silica was added in stages until all the material was added. The material was then mixed at 2350rpm for 5 minutes and cooled to room temperature. This mixing sequence was repeated three more times for a total of 20 minutes to ensure complete mixing. The two batches were combined and degassed in a plenary mixer at 1 bar vacuum for 15 minutes. Appropriate amounts of the dispersion and additional Pluracol 2090 polyol were charged to a 400 mL polyethylene beaker as shown in Table 1-1, along with the additional components in the amounts listed in Table 1-2, to prepare polyol component formulations having 0%, 2%, 4%, 6%, 8% and 10% fumed silica based on the total weight of the polyol component. The silica-polyol dispersion can be used as a drop-in replacement for an equivalent amount of pure polyol on a mass basis to achieve the desired fumed silica concentration in the polyol component. A no-silica control polyol component was prepared with 97 g of Pluracol 2090 polyol and the additional raw materials in the amounts listed in Table 1-2. The polyol components were combined with polyisocyanate (Suprasec 7007 polyisocyanate; Huntsman) in the amounts shown in Tables 1-3 (isocyanate index = 90) in a 400 mL tri-pour polyethylene cup using a high torque mixer (CRAFSTMAN 10-Inch Drill Press, Model No. 137.219000) at 3,100 rpm for 7 s at ambient temperature and then transferred to a polyethylene lined box (6"x6"x3"; 15.24x15.24x7.62 cm). After the foam rise was complete, all foams were placed in an air circulating oven preheated to 70°C for 30 min to complete the cure. Three samples were prepared for each formulation.
[0039] Table 1-1
[0040] Example 1C (silicon dioxide free) 1-1 1-2 1-3 1-4 1-5 Fumed silica % in polyol component 0 2 4 6 8 10 Amount of dispersion (g) 0 14.2 28.36 42.54 56.71 70.89 Additional Pluracol 2090(g) 97 82.8 68.64 54.46 40.29 26.11 Added water (g) 3.45 3.44 3.44 3.44 3.44 3.44
[0041] Table 1-2
[0042]
[0043] Table 1-3
[0044] Example 1C (silicon dioxide free) 1-1 1-2 1-3 1-4 1-5 Total mass of polyol components (g) 106.35 106.34 106.34 106.34 106.34 106.34 Isocyanate content (g) 61.74 61.60 61.45 61.31 61.16 61.01
[0045] The rectangular foams were characterized by: foam density (ASTM D3574, Test A), resilience by ball rebound (ASTM D3574, Test H), tensile strength at break (ASTM D3574, Test E), elongation at break (ASTM D3574, Test E), deflection at 25%, 50%, and 65% of compression force (ASTM D3574, Test C), tear strength (ASTM D-624, Die C), and average pore size (ASTM D3576).
[0046] The apparent cell structure of the foams with 2% and 4% fumed silica based on the total polyol component (1.3% and 2.5% based on the total foam weight, respectively) was uniform, and the fumed silica had no significant effect on the cell size compared to the reference foam (Tables 1-4). However, the foam with 6% fumed silica based on the total polyol component (3.8% based on the total foam weight) exhibited a slightly coarse cell structure. As the amount of fumed silica in the formulation was further increased, the cell structure became coarser.
[0047] Table 1-4
[0048]
[0049] The introduction of 1.3% and 2.5% fumed silica based on the total foam weight had no significant effect on density, resilience, tensile strength and elongation (Tables 1-4). However, with the introduction of such small amounts of fumed silica, the tear strength and compression force deflection (CFD) values increased significantly (Tables 1-4).
[0050] Outgassing was observed during foam rise of foams produced with 3.8%, 5.1% and 6.4% fumed silica based on total foam weight (using polyol components with 6%, 8% and 10% fumed silica). The cell structure was also coarser. It is speculated that this is caused by the cell-opening effect of the fumed silica. However, these samples exhibited CFD at 50% of 3.29 ± 0.21, 3.86 ± 0.20 and 4.21 ± 0.46, respectively, indicating that the silica still provides reinforcement to the foam.
[0051] Example 2
[0052] To optimize the cell structure, additional foams were prepared using the above method and the formulations listed in Table 2-1 below using a polyol component with 10% fumed silica, wherein the surfactant (Tegostab B 4690 surfactant) and open-cell polyol (Lumulse POE 26 polyol) concentrations were adjusted, as well as propylene carbonate (1,2 propylene glycol cyclic carbonate 99.7%, Sigma-Aldrich) to the polyol component of some formulations to reduce viscosity. About half of the polyol component (amount as shown in Table 2-1) was combined with sufficient isocyanate (isocyanate index of 90) in a 400 mL three-inverted polyethylene cup (the exact amount in Table 2-1), mixed as described in Example 1 for 7 seconds, poured into a 1000 mL polyethylene three-inverted beaker, and allowed to rise freely.
[0053] Table 2-1
[0054]
[0055] *Added water plus residual water = 3.6g
[0056] As shown in Table 2-1, when the surfactant concentration was increased, the pore structure did not improve (Examples 2-1 and 2-2). However, when the amount of cell-opening polyol was reduced, the pore structure improved significantly (Examples 2-3 and 2-4). Viscosity can also affect the foaming process - the addition of propylene carbonate also reduced the roughness of the pore structure, especially when combined with a reduced amount of cell-opening polyol (Examples 2-5, 2-6, 2-7).
[0057] Example 3
[0058] Open cell polyurethane foams were produced as follows: using polyol components (similar to Examples 2-6) with 0% (comparative), 6%, 8% and 10% CAB-O-SIL TG-6110 fumed silica in the polyol component formulations as shown in Table 3-1 below, combined with the amounts of isocyanate shown below using the method described in Example 1 (isocyanate index of 90), and dispensed into 6"x6"x3" polyethylene lined boxes as described in Example 1 and allowed to rise freely. The resulting foams had 0%, 3.8%, 5.1% and 6.4% fumed silica. The cell structure of all foams was uniform. Three samples were prepared for each formulation.
[0059] Table 3-1
[0060]
[0061] The results of the cell size measurements and mechanical testing (performed as described in Example 1) are provided in Table 3-2. The cell size of the foam with 3.8% fumed silica is significantly smaller than that of the comparative foam. The cell size increases with fumed silica loading but is always smaller than that of the comparative foam. With increasing amounts of FS in the formulation, the resilience and elongation at break decrease. The tensile strength, tear strength, and CFD values of the foams prepared with FS are all significantly higher than those of the reference foam at the same density.
[0062] Table 3-2
[0063] nature Example 3 - Comp Example 3-1 Example 3-2 Example 3-3 Density, pcf 2.44±0.03 2.41±0.03 2.38±0.02 2.43±0.04 The rebound of the ball, % 60±1 49±1 <![CDATA[49 ± 1]]> 47±1 Tensile strength at break, psi 15.8±1.3 18.8±1.4 21.0±1.4 17.0±0.8 Elongation at break, % 123±8 120±8 113±7 98±7 Tear strength, lbf / in 3.06±0.26 4.24±0.25 3.92±0.25 4.04±0.13 CFD@25%, kPa 1.19±0.06 2.20±0.12 2.56±0.16 2.95±0.23 CFD@50%, kPa 2.36±0.12 4.13±0.29 4.70±0.30 5.53±0.45 CFD@65%, kPa 5.18±0.45 8.10±0.58 8.40±0.76 9.97±0.56 Hole size, mm 1.06±0.08 0.78±0.07 0.94±0.06 0.92±0.08
[0064] Example 4
[0065] The silica-free (comparative) polyol component and the polyol components containing 2%, 4%, 6%, 8% and 10% fumed silica according to the formulation in Example 1 were sealed and aged in a closed cabinet at ambient temperature. After two weeks, the polyol component with 2% fumed silica was a thick liquid and flowed only slowly, while the remaining samples with higher fumed silica concentrations had a pasty appearance and did not flow when inverted. In contrast, the reference composition remained flowable (fluid).
[0066] Additional polyol component formulations were prepared with 10% fumed silica, as shown in Table 4-1 below; the viscosities of these formulations after aging for various times at ambient temperature are also shown (arrows indicate that the viscosity was still rising when the measurement was made). Viscosity was measured in a Brookfield Viscometer, Model LVF according to ASTM D-4878.
[0067] Table 4-1
[0068] Component (g) Example 4-1 Example 4-2 Example 4-3 Example 4-4 Embodiment 4-5 Embodiment 4-6 Fumed silica-polyol dispersion 70.89 70.89 70.89 70.89 70.89 70.89 Pluracol 2090 26.11 26.11 26.11 26.11 26.11 26.11 Lumulse POE26 3 3 3 3 3 3 Tegostab B 4690 1 1 1 1 1 1 Dabco 33LV 0.8 0.8 0 0 0.8 0 Diethanolamine LF 85% 1 0 0 1 0 0 Triethanolamine 0 0 0 0 1 1 Toyocat ET 0.1 0.1 0 0 0.1 0 Added water 3.44 3.44 3.44 3.44 3.44 3.44 Viscosity (mPa-s) initial 5,530 5,750 5,580 6,620 6,340 6,200 1 day 9,960 7,800 5,570 9,000 8,400 6,480 2 days 25,500 7,840 5,500 27,350 10,180 6,480 3 days paste 9,440 5,490 paste 12,120 - 5 days paste - - paste - 6,730 6 days paste 19,500↑ 5,400 paste 21,700↑ 6,740
[0069] The viscosity of the polyol component prepared without the use of Dabco 33LV catalyst and without any diethanolamine (DEA) does not change over time (Example 4-3). The viscosity of the polyol component containing one of these two products (Dabco 33LV or DEA) increases over time (Examples 4-2 and 4-4). The polyol component prepared with DEA and without Dabco 33LV has the consistency of a paste after only three days. The polyol component prepared with Dabco 33LV and without DEA becomes a very viscous liquid after 6 days.
[0070] The viscosity of the polyol component prepared with triethanolamine (TEOA) instead of DEA and without Dabco 33LV changed only slightly, if at all, after 6 days of storage (Example 4-6). The change in viscosity of the polyol component prepared with TEOA and Dabco 33LV was comparable to the change in viscosity of the polyol component prepared with Dabco 33LV without any amine chain extender (Examples 4-2 and 4-5). These results clearly show that fumed silica interacts more with secondary amines than with tertiary amines. In addition, it may not be necessary to use amine chain extenders or crosslinkers in open-cell PU systems employing fumed silica.
[0071] Example 5
[0072] As described above, CAB-O-SIL TG-6110 hydrophobic fumed silica (Cabot Corporation) was dispersed in Pluracol 2090 polyether triol (BASF) to form a 15 wt% dispersion. The dispersion was combined with additional components (including poly-G 85-29 ethylene oxide-terminated polyether polyol triol (Monument Chemical)) in the proportions listed in Table 5-1 below to form a polyol component. Similar to Example 1, the silica-polyol dispersion can be used as a direct replacement for an equivalent amount of pure polyol on a mass basis to prepare polyol components having silica concentrations of 0%, 2%, 4%, 6%, 8%, and 10%. A total of 223.34 g of the polyol components were combined with 131.52 g of Suprasec 7007 polyisocyanate (to achieve an isocyanate index of 90) in a 1000 mL three-inverted polyethylene cup using a high torque mixer (CRAFSTMAN 10-Inch Drill Press, Model No. 137.219000) at 3,100 rpm for 7 s at ambient temperature and then poured into a 12"x12"x2" (30 cmx30 cmx5 cm) aluminum mold preheated to 70°C before the liquid mixture became cloudy and began to expand. After pouring, the mold was closed and the foam was allowed to cure for 260 s before the mold was opened and the foam demolded. All molded foams were aged in an ambient atmosphere for at least one week before testing. The foam pad was manually impacted (i.e., compressed by hand to open the cell window) immediately after demolding. In addition to the tests described in Example 1, the foams were also characterized by the following tests under ASTM D-3574: Dry Constant Deflection Compression Set (Test D), humid aging compression set (Test D and Test L humid heat aging), humid aging load (CFD) loss (Test C and Test L-humid heat aging; 22h @ 50°C and 95% relative humidity, and Test C and Test J2-steam autoclave aging; 5h @ 120°C). The molded foams were also evaluated for CFD at 25%, 50% and 65% deflection (deflection) as described in Example 1, but with a 60s dwell time. Two foam samples were measured using each formulation.
[0073] Table 5-1
[0074]
[0075] The molded foams prepared with 0%, 1.3%, 2.5%, 3.8% FS based on the total foam weight (0%, 2%, 4% and 6% FS based on the total polyol component, respectively) showed a uniform surface (skin) and a uniform apparent pore structure. Some defects on the skin were observed in the foams prepared with 5.1% and 6.3% fumed silica based on the total foam weight (8% and 10% FS based on the total polyol component, respectively). However, regardless of the slight skin defects, the pore structure of these foams is uniform. The mechanical properties of the resulting foams are listed in Table 5-2. The resilience of the molded foams decreases with increasing concentrations of fumed silica.
[0076] Table 5-2
[0077]
[0078] Example 6
[0079] CAB-O-SIL TG-6110 (Example 6-x) and CT1221 (Example 6-Cx) silicas (Cabot Corporation; CT1221 silica has a 180-250 m 2 / g BET surface area and trimethylsilyl groups at the surface) as described in Example 1. The polyol component as described in Example 1 was prepared using the formulation listed in Table 6-1 (including Voranol-Voractiv 6340 polyether polyol (Dow), Dabco NE300 blowing catalyst (Evonik), Dabco NE1091 gelling catalyst (Evonik), Dabco DC193 surfactant (Evonik), propylene carbonate (see Example 2) and diethanolamine LF 85% (Webb Chemical). The polyol component was combined with Lupranate T80 isocyanate (a mixture of 2,4- and 2,6-toluene diisocyanates, Huntsman) in the amounts specified in Table 6-2 (isocyanate index of 90) and cast in polyethylene lined boxes as described in Example 1 ("free rise foam"). Free rise foams were prepared in duplicate. The polyurethane formulations specified in Table 6-2 were scaled up by 250% for Example 6-C1 and 257% for Examples 6-1 and 6-2 to prepare molded foams according to the method described in Example 5. The molded foams were prepared in duplicate. The foams were evaluated as described above.
[0080] Table 6-1a
[0081]
[0082] *Added water = total water in formulation
[0083] Table 6-1b
[0084]
[0085] *Added water = total water in formulation
[0086] Table 6-2
[0087] Example No. Amount of polyol component (g) Lupranate T80 isocyanate amount Free rise foam appearance 6-C1 106.1 30.63 Uniform, fine 6-1 106.1 30.43 Uniform, fine 6-2 106.1 30.36 Uniform, fine 6-C2 106.1 30.47 Collapsed in 71-74s 6-C3 106.6 30.50 Collapse in 75s 6-C4 106.1 30.49 Horizontal split in the center 6-C5 106.1 30.48 Collapse in the 81s 6-C6 108.1 30.47 Collapse in 75s 6-C7 106.1 30.55 Slow descent after full ascent
[0088] Table 6-2 demonstrates that stable foams were prepared with the lower surface area TG-6110 silica. Presumably, the open cell nature of the silica compensated for the absence of an open cell polyol in the formulation. However, the foam with the higher surface area CT-1221 silica collapsed even in the absence of an open cell polyol. Foam stability did not improve with changes in surfactant concentration, partial replacement of Tegostab dispersant with an alternative dispersant, Dabco DC 193 surfactant, addition of propylene carbonate, or reduction in silica concentration.
[0089] In addition to the above tests, the hysteresis loss of the foam was characterized according to ASTM D-3574 (Procedure B-CFD Hysteresis loss). Table 6-3 shows the mechanical and other properties of molded foams containing TG-6110 silica relative to the silica-free control. The introduction of TG-6110 silica increases CFD and does not significantly affect the resilience of the free-rise foam. In the molded foam, the introduction of TG-6110 silica increases CFD and tear strength, but does not significantly affect tensile strength.
[0090] Table 6-3
[0091]
[0092] Example 7
[0093] A 15% dispersion of CAB-O-SIL TG-6110 and CT 1221 silica was prepared in Jeffol G 31-28 glyceryl ethylene oxide tip triol (Huntsman) as described above. A polyol component with 6 wt% silica (including Lumulse POE 26 ethoxylated glycerol, Tegostab B 4690 surfactant, diethanolamine LF 85% crosslinker, Dabco 33LV triethylenediamine, and Toyocat ET bis(2-dimethylaminoethyl) ether) was prepared as described in Example 1 using the formulation listed in Table 7-1. The polyol component was combined with Suprasec 7007 isocyanate in the amounts listed in Table 7-1 as described in Example 1 and cast in a polyethylene lined box ("free rise foam") as described in Example 1 to form a foam with 3.8 wt% silica. The foam appearance was visually evaluated.
[0094] Table 7-1
[0095]
[0096] Both foams produced without silica and with the lower surface area TG-6110 silica exhibited uniform and fine pore structure. Foams produced with the higher surface area CT-1221 silica and Lumulse POE open cell polyol exhibited partial foam collapse, while foams produced with CT-1221 silica without open cell polyol exhibited coarse pores in the core of the foam.
[0097] Example 8
[0098] Fumed silica (see Table 8-1 below, all silicas from Cabot Corporation) was combined with Voranol 220-046 polyether polyol (Dow) in a Hauschild Speedmixer DAC-150 at 6 wt% loading until a Hegman grind of 5 was achieved. Dispersion was evaluated in a TA Instruments AR2000 Rheometer using 4 cm parallel plate geometry and a 500 micron gap at 25°C. Viscosity data are shown in Figure 1 The data show that fumed silica treated with octylsilane groups or siloxane polymers significantly increases viscosity compared to fumed silica treated with alkylsilane groups having three or fewer carbons.
[0099] Table 8-1
[0100]
[0101] Example 9
[0102] CAB-O-SIL TG-6110 (circles) and CT-1221 (triangles) silicas were combined with Voranol 6340 (closed symbols) and Jeffol G 31-28f (open symbols) polyols at 15% loading as described in Example 1. Viscosity was measured as described in Example 8 and plotted against shear rate. The results are shown in Figure 2 The CT-1221 silica, which exhibits a higher surface area, also resulted in a significant increase in viscosity.
[0103] Example 10
[0104] CAB-O-SIL TG-6110 (circles) and L90 (triangles) silicas were combined with Voranol 232-034 (closed symbols) polyol at 10% loading as described in Example 1. Viscosity was measured as described in Example 8 and plotted against shear rate. The interaction of hydrophobic TG-6110 silica and untreated hydrophilic L90 silica with amine catalysts was evaluated by adding 1 wt % triethanolamine to the sample, mixing for 30 s in a SpeedMixer (Flackteck, Landrum, SC), allowing the sample to incubate for 30 min at ambient temperature, and then measuring the viscosity again (open symbols). The results are shown in Figure 3 The results also show that untreated L90 silica causes a significant increase in the viscosity of the polyol. In a polymeric system, this increase in viscosity can prevent the proper development of bubbles in the foam.
[0105] The above description of the preferred embodiments of the present invention has been presented for the purpose of illustration and description. It is not intended to be exhaustive or to limit the present invention to the precise form disclosed. Modifications and variations are possible in light of the above teachings or may be obtained from the practice of the present invention. The embodiments are selected and described in order to explain the principles of the present invention and their practical application, so that those skilled in the art can utilize the present invention in various embodiments and make various modifications according to the specific use contemplated. It is intended that the scope of the present invention be defined by the claims appended hereto and their equivalents.
Claims
1. A method for producing a flexible polyurethane foam, comprising: Provided is a method comprising at least a first polyol and up to 10 wt % of a polyol having a molecular weight of 50 to 150 m 2 / g of surface area of fumed silica, the first polyol having a weight average molecular weight of 3000 to 6000 and a functionality of 2.5 to 3.5, wherein the fumed silica has a C1-C3 alkyl silane group at its surface; combining the polyol composition, a polyisocyanate having a functionality of 1.8 to 2.5, water, and a tertiary amine catalyst to form a prepolymer composition; and The prepolymer composition is allowed to polymerize to form an open cell foam structure having a density of 1.8 to 4 pcf and one or more of: a) a resilience of at least 40% and b) a dry compression set of no greater than 15%.
2. The method of claim 1, wherein the resilience is from 40% to 70%.
3. The method of claim 1, wherein the dry compression set is from 3% to 15%.
4. The method of claim 1, wherein the flexible polyurethane foam exhibits a density of 1.8 to 3 pcf.
5. The method of claim 1, wherein the flexible polyurethane foam exhibits a density of 2 to 4 pcf.
6. The process of any one of claims 1 to 5, wherein the polyisocyanate comprises hexamethylene diisocyanate (HDI), phenylene diisocyanate, 2,4-toluene diisocyanate (2,4-TDI), 2,6-toluene diisocyanate (2,6-TDI), 4,4'-diphenylmethane diisocyanate, an isomeric mixture of diphenylmethane diisocyanate, or a mixture of two or more of these.
7. The method of any one of claims 1-5, wherein the first polyol comprises a polyether polyol or a polyester polyol.
8. The method of any one of claims 1-5, wherein the polyol composition further comprises a second polyol having a weight average molecular weight of 2,000 to 10,000.
9. The method of any one of claims 1 to 5, wherein the fumed silica has a carbon content of 50 to 150 m 2 / g of BET surface area.
10. The method of any one of claims 1 to 5, wherein the fumed silica has a carbon content of 50 to 100 m 2 / g of BET surface area.
11. The method of any one of claims 1 to 5, wherein allowing comprises loading the prepolymer composition into a mold having one side open to atmosphere.
12. The method of claim 11, wherein the flexible polyurethane foam has a density of 1.8 to 3 pcf.
13. The method of any one of claims 1-5, wherein allowing comprises loading the prepolymer composition into a mold and closing the mold.
14. The method of claim 13, wherein the flexible polyurethane foam has a density of 2 to 4 pcf.
15. The method according to any one of claims 1 to 5, wherein the C1-C3 alkylsilyl group is a trimethylsilyl group or a dimethylsilyl group.
16. The method of any one of claims 1-5, wherein the flexible polyurethane foam has a deflection at 50% compressive force as measured by ASTM D3574 that is improved by at least 30% relative to a flexible polyurethane foam produced by the same method but in which the silica is replaced with an equal mass portion of the first polyol.
17. The method of claim 16, wherein the flexible polyurethane foam has a deflection at 50% compressive force as measured by ASTM D3574 that is improved by at least 50% relative to a flexible polyurethane foam produced by the same method but in which the silica is replaced with an equal mass portion of the first polyol.
18. The method of claim 16, wherein the flexible polyurethane foam has a deflection at 50% compressive force as measured by ASTM D3574 that is improved by at least 70% relative to a flexible polyurethane foam produced by the same method but in which the silica is replaced with an equal mass portion of the first polyol.
19. The method of claim 16, wherein the flexible polyurethane foam has a deflection at 50% compressive force as measured by ASTM D3574 that is improved by 30% to 155% relative to a flexible polyurethane foam produced by the same method but wherein the silica is replaced with an equal mass portion of the first polyol.
20. A flexible polyurethane foam produced by the process of any one of claims 1 to 19.
21. The flexible polyurethane foam of claim 20, wherein the foam is a molded foam or a free rise foam.
22. The flexible polyurethane foam of any one of claims 20-21, wherein the polyurethane comprises a polyether polyurethane or a polyester polyurethane.
23. The flexible polyurethane foam of any of claims 20-21, having a deflection at 50% compressive force as measured by ASTM D3574 that is at least 30% greater than a flexible polyurethane foam of the same composition but with a polyol substituted for silica.
24. The flexible polyurethane foam of claim 23 having a deflection at 50% compressive force as measured by ASTM D3574 that is at least 50% greater than a flexible polyurethane foam having the same composition but with a polyol substituted for silica.
25. The flexible polyurethane foam of claim 23 having a deflection at 50% compressive force as measured by ASTM D3574 that is at least 70% greater than a flexible polyurethane foam having the same composition but substituting a polyol for silica.
26. The flexible polyurethane foam of claim 23 having a deflection at 50% compressive force as measured by ASTM D3574 that is 30% to 155% greater than a flexible polyurethane foam having the same composition but substituting a polyol for silica.
Citation Information
Patent Citations
Additives for improving polyurethane foam performance
US10119002B2
Polyester Polyurethane Foam Containing Fumed Silica
US20080153935A1
Method for producing flexible polyester urethane foams with increased compressive strength
US20180223030A1
Flame retardant polyurethane foams containing biuret linkages
US9034936B2
Dispersible silica particles
WO2006128793A1