Fiber manufacturing method

By setting up a rectifying filter in the cooling section and adjusting the cooling conditions, the index M derived from the Nusselt number is used to control the change in fiber outer diameter, which solves the problem of fiber outer diameter change in the melt spinning method and achieves consistent outer diameter. improve.

CN116324057BActive Publication Date: 2024-10-29NITTO DENKO CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202180069650.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-06-04
Publication Date
2024-10-29
Estimated Expiration
2041-06-04

AI Technical Summary

Technical Problem

In the melt spinning method, the change in the outer diameter of the fiber is difficult to suppress, affecting the quality and consistency of the product.

Method used

By installing a rectifying filter in the cooling section, the temperature of the cooling fluid is ensured to be constant, and the index M derived from the Nusselt number is 1.52 or less. The flow rate of the cooling fluid, the moving distance of the linear body, and the coiling speed are adjusted to control Changes in the outer diameter of the fiber.

Benefits of technology

It effectively suppresses changes in the outer diameter of the fiber, improves the consistency of the outer diameter of the fiber, and ensures stable product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116324057B_ABST
    Figure CN116324057B_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing a fiber suitable for suppressing outer diameter variation. The manufacturing method of this embodiment includes: a step of ejecting a softened linear body (1) from a nozzle (10); and a step of winding the linear body (1) through a cooling section (20) to which a cooling fluid (50) is supplied to obtain a fiber (5). The cooling section (20) has a filter (40) for rectifying the cooling fluid (50). In the cooling section (20), the temperature of the cooling fluid (50) is substantially constant in the direction in which the linear body (1) moves. In the manufacturing method of this embodiment, the index M determined by the following formula (I) is less than 1.52. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a fiber, for example, a method for producing a plastic optical fiber. Background Art

[0002] As an example of a method for manufacturing fibers such as plastic optical fiber (POF), a melt spinning method is known. In the melt spinning method, for example, a heated resin composition is delivered to a nozzle, and a softened linear body is ejected from the nozzle. The linear body is cooled and solidified to thereby produce a fiber.

[0003] In the melt spinning method, the cooling of the linear body is performed, for example, by bringing the linear body into contact with a cooling fluid. As the cooling fluid, for example, cooling air or cooling water is used (Patent Documents 1 and 2). By bringing the linear body into contact with the cooling fluid while winding, the linear body is, for example, stretched while solidifying. Thus, a fiber having a target outer diameter can be obtained.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-186772

[0007] Patent Document 2: Japanese Patent Application Publication No. 2006-163007 Summary of the invention

[0008] Problems to be solved by the invention

[0009] In the melt spinning method, it is required to suppress the variation in the outer diameter of the formed fiber. Therefore, an object of the present invention is to provide a method for producing a fiber suitable for suppressing the variation in the outer diameter.

[0010] Means for solving problems

[0011] The present inventors have conducted intensive research and have newly discovered that heat transfer between the linear body and the cooling fluid generated when cooling the linear body affects the change in the outer diameter of the fiber. Based on this finding, the present inventors have conducted research and derived a new index M consisting of only measurable parameters from the Nusselt number, which is an index of heat transfer, to complete the present invention.

[0012] The present invention provides a method for producing a fiber, comprising:

[0013] The step of ejecting the softened linear body from the nozzle; and

[0014] The step of winding the linear body so as to pass through a cooling portion to which a cooling fluid is supplied to obtain a fiber,

[0015] The cooling unit includes a filter for rectifying the cooling fluid.

[0016] In the cooling unit, the temperature of the cooling fluid is substantially constant in the direction in which the linear body moves.

[0017] The index M determined by the following formula (I) is 1.52 or less.

[0018]

Mathematical formula l

[0019]

[0020] In the above formula (I), Q a is the flow rate (m 3 / s),

[0021] L is the moving distance of the linear body in the cooling section (m),

[0022] T w is the temperature of the linear body just after being ejected from the nozzle (°C),

[0023] T a is the temperature of the cooling fluid (°C),

[0024] D f is the outer diameter of the above fiber (m),

[0025] D n is the outer diameter of the linear body just after being ejected from the nozzle (m),

[0026] U is the winding speed of the linear body (m / s),

[0027] K is 1.0×10 8 (℃·s 2 / m 3 ).

[0028] Effects of the Invention

[0029] According to the present invention, a method for producing a fiber suitable for suppressing outer diameter fluctuation can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a diagram for explaining an example of a spinning device for carrying out the production method of the present invention.

[0031] Figure 2 This is a diagram for explaining an example of a nozzle and a cooling unit included in a spinning device.

[0032] Figure 3This is a graph showing the relationship between the index M in Production Examples 1 to 15 and the ratio of the triple value of the standard deviation of the outer diameter of the fiber to the average value of the outer diameter of the fiber (3σ / Ave.). DETAILED DESCRIPTION

[0033] Another aspect of the present invention provides a method for producing a fiber, comprising:

[0034] The step of ejecting the softened linear body from the nozzle; and

[0035] The step of winding the linear body so as to pass through a cooling portion to which a cooling fluid is supplied to obtain a fiber,

[0036] The index M determined by the following formula (I) is 1.6 or less.

[0037]

Mathematical formula 2

[0038]

[0039] In the above formula (I), Q a is the flow rate (m 3 / s),

[0040] L is the moving distance of the linear body in the cooling section (m),

[0041] T w is the temperature of the linear body just after being ejected from the nozzle (°C),

[0042] T a is the temperature of the cooling fluid (°C),

[0043] D f is the outer diameter of the above fiber (m),

[0044] D n is the outer diameter of the linear body just after being ejected from the nozzle (m),

[0045] U is the winding speed of the above-mentioned linear body (m / s),

[0046] K is 1.0×10 8 (℃·s 2 / m 3 ).

[0047] Hereinafter, embodiments of the present invention will be described, but the following description is not intended to limit the present invention to the specific embodiments.

[0048] like Figure 1 and 2As shown, the manufacturing method of this embodiment includes: a step of ejecting a softened linear body 1 from a nozzle 10; and a step of winding the linear body 1 in a manner of passing through a cooling section 20 to which a cooling fluid 50 is supplied to obtain a fiber 5. The cooling section 20 has a filter 40 for rectifying the cooling fluid 50. In the cooling section 20, the temperature of the cooling fluid 50 is substantially constant in the direction in which the linear body 1 moves. In addition, in the manufacturing method of this embodiment, the index M determined by the following formula (I) is 1.52 or less.

[0049]

Mathematical formula 3

[0050]

[0051] In formula (I), Q a is the flow rate (m 3 / s). L is the moving distance (m) of the linear body 1 in the cooling unit 20. w T is the temperature (°C) of the linear body 1 immediately after being ejected from the nozzle 10. a is the temperature of the cooling fluid 50 (°C). f is the outer diameter of fiber 5 (m). n is the outer diameter (m) of the linear body 1 immediately after being ejected from the nozzle 10. U is the winding speed (m / s) of the linear body 1. K is a proportionality constant related to temperature for deriving the index M from the Nusselt number and is 1.0×10 8 (℃·s 2 / m 3 ).

[0052] In the manufacturing method of this embodiment, the index M is preferably 1.2 or less, more preferably 1.0 or less, further preferably 0.8 or less, and particularly preferably 0.5 or less. The index M is 0 or more, and may be greater than 0, for example, 0.01 or more.

[0053] As described above, the index M is derived from the Nusselt number as an index of heat transfer. According to the research of the present inventors, by adjusting the manufacturing conditions in a manner such that the index M is less than 1.52, there is a tendency to suppress the variation in the outer diameter of the fiber 5. The variation in the outer diameter of the fiber 5 can be evaluated by the ratio (3σ / Ave.) of three times the standard deviation of the outer diameter of the fiber 5 (3σ) to the average value (Ave.) of the outer diameter of the fiber 5. Regarding the fiber 5 obtained by the manufacturing method of the present embodiment, the ratio 3σ / Ave. is not particularly limited, for example, it is less than 2.0%, preferably less than 1.5%, more preferably less than 1.0%, and further preferably less than 0.8%. The lower limit of the ratio 3σ / Ave. is not particularly limited, for example, it is 0.2%. It should be noted that the outer diameter of the fiber 5 can be measured using a commercially available displacement meter. The average value and standard deviation of the outer diameter of the fiber 5 are values ​​calculated based on the measured values ​​of the outer diameter of the fiber 5 at least 50 locations.

[0054] Furthermore, the index M and 3σ / Ave. may satisfy at least one selected from the following formulas (II) and (III).

[0055] 3σ / Ave.≥M-0.5 (II)

[0056] 3σ / Ave.≤M+1 (III)

[0057] When the index M is 1.52 or less, the flow rate Q of the cooling fluid 50 supplied to the cooling unit 20 is a There is no special limit, for example, 0m 3 / s~1.0×10 -2 m 3 / s, preferably more than 0m 3 / s and 1.0×10 -2 m 3 / s or less, more preferably 0.5×10 -4 m 3 / s~1.0×10 -3 m 3 / s.

[0058] Likewise, the moving distance L of the linear bodies 1 in the cooling unit 20 is not particularly limited, and is, for example, 0.1 m to 2.0 m.

[0059] The temperature T of the linear body 1 immediately after being ejected from the nozzle 10 w The temperature T of the cooling fluid 50 is not particularly limited, but is, for example, 100° C. or higher, preferably 150° C. to 300° C. a The temperature is not particularly limited, but is, for example, 50°C or lower, and preferably 5°C to 40°C.

[0060] The outer diameter D of the fiber 5 fThere is no particular limitation, but for example, 1.0×10 -5 m~1.0×10 -3 m. Outer diameter D of fiber 5 f Specifically, it refers to an average value calculated from the measured values ​​of the outer diameters of the fibers 5 at least at 50 locations. n There is no particular limitation, but for example, 1.0×10 -4 m~1.0×10 -2 m, preferably 1.0×10 -3 m~1.0×10 -2 m.

[0061] The winding speed U of the linear object 1 is not particularly limited, and is, for example, 0.05 m / s to 10 m / s, and preferably 0.1 m / s to 5 m / s.

[0062] Next, refer to Figure 1 and 2 An example of a spinning device 100 for implementing the production method of this embodiment will be described. Figure 2 In the figure, for the convenience of explanation, the shadow of the linear body 1 is omitted.

[0063] The nozzle 10 and the cooling part 20 are components of the spinning device 100. The nozzle 10 is, for example, a cylindrical component whose internal space is connected to the outside at the upper first opening 11 and the lower second opening 12. Typically, the first opening 11 and the second opening 12 each have a circular shape when viewed from above. The diameter of the second opening 12 may be the same as the diameter of the first opening 11, may be smaller than the diameter of the first opening 11, or may be larger than the diameter of the first opening 11. The second opening 12 corresponds to the opening of the nozzle 10 for ejecting the linear body 1. In the embodiment in which the diameter of the second opening 12 is less than the diameter of the first opening 11, the outer diameter D of the above formula (I) n For example, the diameter is the same as that of the second opening 12 .

[0064] The nozzle 10 includes, for example, a reduced diameter portion 13 and a cylindrical portion 14. The cylindrical portion 14 is connected to the reduced diameter portion 13 below the reduced diameter portion 13. In the nozzle 10, for example, the first opening 11 is formed at the end of the reduced diameter portion 13, and the second opening 12 is formed at the end of the cylindrical portion 14. The reduced diameter portion 13 has, for example, a truncated cone shape that decreases in diameter from the first opening 11 toward the cylindrical portion 14. The shape of the cylindrical portion 14 is, for example, cylindrical.

[0065] The material of the nozzle 10 is not particularly limited, and examples thereof include metals and resins.

[0066] In the manufacturing method of the present embodiment, for example, the softened linear body 1 is supplied to the first opening 11 of the nozzle 10. The linear body 1 is ejected from the second opening 12 through the reduced diameter portion 13 and the cylindrical portion 14. In this specification, the linear body supplied to the first opening 11 is sometimes referred to as "linear body 1a", and the linear body ejected from the second opening 12 is sometimes referred to as "linear body 1b". However, instead of supplying the linear body 1a to the first opening 11, molten resin and / or viscous liquid may be supplied to the first opening 11. Even in this case, since the molten resin and viscous liquid are formed into fibers by the nozzle 10, the linear body 1b is ejected from the second opening 12.

[0067] The linear body 1a supplied to the first opening 11 passes through the diameter-reducing portion 13, for example, so that its outer diameter is reduced. That is, the outer diameter of the linear body 1b ejected from the nozzle 10 is smaller than that of the linear body 1a before being supplied to the nozzle 10. The outer diameter of the linear body 1b immediately after being ejected from the second opening 12 is usually equal to the diameter of the second opening 12. It should be noted that, typically, the linear body 1 is ejected from the nozzle 10 while being in contact with the peripheral edge of the second opening 12. Therefore, the temperature of the nozzle 10 near the second opening 12 can be regarded as the temperature T in the above formula (I). w .

[0068] The cooling unit 20 includes, for example, a cylindrical cooling pipe 30. The cooling pipe 30 is, for example, cylindrical in shape. The cooling pipe 30 has an internal space 35 (particularly, an internal space 45 of a filter 40 described later, which corresponds to a part of the internal space 35) connected to the outside at the upper first opening 34a and the lower second opening 34b. The cooling pipe 30 is connected to, for example, the nozzle 10 and extends downward from the nozzle 10. The first opening 34a of the cooling pipe 30 surrounds, for example, the second opening 12 of the nozzle 10.

[0069] The cooling pipe 30 has, for example, a main body 31 and a cylindrical portion 37. The main body 31 includes an inner wall 32, an outer wall 33, and a storage space 36 formed between the inner wall 32 and the outer wall 33. The inner wall 32 and the outer wall 33 are each shaped like a cylinder, preferably a cylindrical shape. The inner wall 32 and the outer wall 33 are each shaped not necessarily like a cylindrical shape, and may be, for example, a square cylinder. The inner wall 32 and the outer wall 33 extend from the first opening 34a to the second opening 34b, respectively. The space surrounded by the inner wall 32 corresponds to the internal space 35 of the cooling pipe 30.

[0070] In the storage space 36, for example, a refrigerant 51 for cooling the cooling fluid 50 supplied to the internal space 35 of the cooling pipe 30 is introduced. In detail, on the outer wall 33, for example, a first opening portion 38a is formed near the second opening portion 34b of the cooling pipe 30. The first opening portion 38a is connected to, for example, a refrigerant supply path 56 for supplying the refrigerant 51 to the storage space 36, and functions as a refrigerant inlet. The refrigerant 51 can be introduced into the storage space 36 through the first opening portion 38a. In addition, on the outer wall 33, a second opening portion 38b can also be formed near the first opening portion 34a of the cooling pipe 30. The second opening portion 38b is connected to, for example, a refrigerant discharge path 57 for discharging the refrigerant 51 from the storage space 36, and functions as a refrigerant outlet. In this embodiment, the refrigerant discharge path 57 may be connected to the refrigerant supply path 56 via the storage space 36, and the refrigerant 51 circulates in the refrigerant supply path 56, the storage space 36, and the refrigerant discharge path 57. Figure 2 , the cooling medium 51 is shown to move from the bottom to the top in the storage space 36. However, the cooling pipe 30 may also be configured so that the cooling medium 51 moves from the top to the bottom in the storage space 36. That is, the second opening 38b formed in the outer wall 33 functions as a cooling medium inlet, and the first opening 38a functions as a cooling medium outlet.

[0071] The cylindrical portion 37 is a cylindrical member that passes through the main body 31 in the direction from the inner wall 32 toward the outer wall 33. The cylindrical portion 37 extends, for example, in a direction perpendicular to the direction in which the inner wall 32 extends. A first opening portion 39a is formed at the end of the cylindrical portion 37 on the outer wall 33 side. A second opening portion 39b is formed at the end of the cylindrical portion 37 on the inner wall 32 side. The first opening portion 39a is connected to, for example, a cooling fluid supply path 55 for supplying the cooling fluid 50 into the cylindrical portion 37, and functions as a cooling fluid inlet. The cooling fluid 50 transported into the cylindrical portion 37 is supplied to the internal space 35 of the cooling pipe 30 through the second opening portion 39b. It should be noted that, for example, a flow rate Q of the cooling fluid 50 supplied to the internal space 35 is provided in the cylindrical portion 37. a Flow meter.

[0072] The position of the cylindrical portion 37 is not particularly limited as long as the cooling fluid 50 can be sufficiently supplied to the internal space 35 of the cooling pipe 30. For example, the distance between the cylindrical portion 37 and the first opening 34a of the cooling pipe 30 may be equal to the distance between the cylindrical portion 37 and the second opening 34b of the cooling pipe 30, or may not be equal to the distance between the cylindrical portion 37 and the second opening 34b of the cooling pipe 30. Figure 2In the embodiment, the cylindrical portion 37 is located near the center of the cooling pipe 30 in the longitudinal direction. However, the cylindrical portion 37 may also be located near the end (upper or lower portion) of the cooling pipe 30. Figure 2 In the embodiment, one cooling fluid supply path 55 is connected to one cylindrical portion 37. However, in the present embodiment, the cooling pipe 30 may include a plurality of cylindrical portions 37, and the plurality of cooling fluid supply paths 55 may be connected to the plurality of cylindrical portions 37, respectively.

[0073] As described above, the cooling unit 20 has a filter 40 for rectifying the cooling fluid 50. The shape of the filter 40 is, for example, cylindrical, preferably cylindrical. The filter 40 is, for example, made of nonwoven fabric, woven fabric, net, etc., and the cooling fluid 50 can pass through. The filter 40 is, for example, located in the internal space 35 of the cooling pipe 30 and extends in the same direction as the cooling pipe 30. The length of the filter 40 may be the same as or different from that of the cooling pipe 30. The internal space 45 of the filter 40 is connected to the outside at the first opening 41 at the top and the second opening 42 at the bottom. The internal space 45 of the filter 40 can be regarded as a part of the internal space 35 of the cooling pipe 30. Similarly, the openings 41 and 42 of the filter 40 can also be regarded as parts of the openings 34a and 34b of the cooling pipe 30, respectively. The filter 40 is connected to the nozzle 10, for example. The first opening 41 of the filter 40 surrounds the second opening 12 of the nozzle 10, for example. The diameter of the second opening 42 of the filter 40 may be the same as or different from the inner diameter of the filter 40.

[0074] It should be noted that the cooling portion 20 may also include a cylindrical wall portion that is impermeable to the cooling fluid 50 instead of the filter 40. The shape of the cylindrical wall portion is, for example, the same as the shape illustrated in the filter 40. In the case where the cooling portion 20 has a cylindrical wall portion, the linear body 1 is not in direct contact with the cooling fluid 50. Even in such a manner, external interference caused by the air present outside can be suppressed by the cooling pipe 30. Through the cylindrical wall portion, the cooling fluid 50 can also exchange heat with the air present in the internal space surrounded by the wall portion. Even in the case where the linear body 1 is not in direct contact with the cooling fluid 50, the indicator M can be used as an indicator for suppressing the change in the outer diameter of the fiber 5.

[0075] The cooling unit 20 further includes, for example, a cover 43, and the cover 43 partially closes the second opening 34b of the cooling pipe 30 except for the second opening 42 of the filter 40. The cover 43 is connected to, for example, the end of the cooling pipe 30 and the end of the filter 40, respectively. As long as the cover 43 does not contact the linear body 1, it may further close a part of the second opening 42 of the filter 40. The cover 43 may be integrated with the cooling pipe 30. By means of the cover 43, for example, it is possible to suppress the cooling fluid 50 from being released to the outside of the cooling pipe 30 without contacting the linear body 1.

[0076] In this embodiment, the cooling fluid 50 is, for example, a gas. Examples of the gaseous cooling fluid 50 include air, inert gases such as helium, etc., and air is preferred. As the refrigerant 51, for example, a liquid such as water can be used. The temperature of the refrigerant 51 is not particularly limited, and is, for example, 20° C. or less.

[0077] The material of the main body 31 and the cylindrical portion 37 of the cooling pipe 30 is not particularly limited, and examples thereof include glass, metal, etc. The material of the filter 40 is not particularly limited, and examples thereof include metal and resin.

[0078] In the manufacturing method of the present embodiment, the cooling fluid 50 is transported to the internal space 35 of the cooling pipe 30 through the cylindrical portion 37. The cooling fluid 50 transported to the internal space 35 fills the internal space 35. In the case where the cooling unit 20 has a cover 43, the cooling fluid 50 is released to the outside from the portion of the second opening 34b of the cooling pipe 30 that is not closed by the cover 43. However, the cooling unit 20 may not have a cover 43, and the entire second opening 34b of the cooling pipe 30 may be exposed to the outside of the cooling unit 20. In this case, the cooling fluid 50 is released to the outside from the entire second opening 34b. In addition, there may be a gap between the nozzle 10 and the cooling pipe 30 so that the cooling fluid 50 is also released from the first opening 34a of the cooling pipe 30. In the case where the cooling unit 20 has a filter 40, the cooling fluid 50 passes through the filter 40 and also fills the internal space 45. The cooling fluid 50 is rectified by passing through the filter 40.

[0079] The linear body 1 ejected from the second opening 12 of the nozzle 10 is introduced into the internal space 35 of the cooling pipe 30 (or the internal space 45 of the filter 40) through the first opening 34a of the cooling pipe 30 (or the first opening 41 of the filter 40). The linear body 1 introduced into the internal space 35 or 45 contacts the cooling fluid 50. In this way, in the manufacturing method of the present embodiment, the linear body 1 is cooled by contacting the cooling fluid 50 in the cooling section 20. The linear body 1 gradually solidifies as it is cooled by the cooling fluid 50. When the cooling fluid 50 is rectified by the filter 40, the linear body 1 can contact the cooling fluid 50 uniformly. If the linear body 1 contacts the cooling fluid 50 uniformly, there is a tendency to further suppress the variation in the outer diameter of the obtained fiber 5. By the filter 40, it is possible to suppress the cooling fluid 50 transported to the internal space 35 of the cooling pipe 30 from being directly sprayed onto the linear body 1 without being rectified.

[0080] The linear body 1 passes through the internal space 35 or 45 while being cooled, and is transported to the second opening 34b of the cooling pipe 30 (or the second opening 42 of the filter 40). Figure 2In this embodiment, the linear body 1 moves in the internal space 35 along the direction in which the cooling pipe 30 extends. In this embodiment, the moving distance L of the linear body 1 in the cooling unit 20 is equal to the length of the cooling pipe 30.

[0081] It should be noted that the linear body 1 is slowly stretched in the cooling unit 20 . Thus, the outer diameter of the linear body 1 gradually decreases as the linear body 1 passes through the cooling unit 20 , for example.

[0082] The cooling fluid 50 supplied to the internal space 35 exchanges heat with the refrigerant 51 via the inner wall 32 of the cooling tube 30, and also exchanges heat with the linear body 1 passing through the internal space 35. Therefore, a temperature gradient is generated in the cooling fluid 50 near the inner wall 32 and near the linear body 1. However, at a position of the internal space 35 away from the inner wall 32 and the linear body 1, the cooling fluid 50 hardly generates a temperature gradient. The temperature T of the above formula (I) is a It refers to the temperature of the cooling fluid 50 at a position in the inner space 35 where the cooling fluid 50 hardly generates a temperature gradient. As an example, the temperature T of formula (I) a It may be the temperature of the cooling fluid 50 near the filter 40. The temperature of the cooling fluid 50 near the filter 40 is substantially constant, for example, in the direction in which the filter 40 extends (ie, the direction in which the linear body 1 moves). In other words, the temperature of the cooling fluid 50 passing through the filter 40 is substantially uniform.

[0083] The cooling unit 20 is not limited to the above structure, and for example, may have a storage tank capable of storing a liquid cooling fluid instead of the cooling pipe 30. As the liquid cooling fluid, water can be cited, for example. In this case, the storage tank of the cooling unit 20 has, for example, a cooling fluid inlet for introducing the cooling fluid into the storage tank and a cooling fluid outlet for discharging the cooling fluid to the outside. The linear body 1 ejected from the nozzle 10 is wound up, for example, in a manner passing through the storage tank.

[0084] like Figure 1 As shown, the spinning device 100 is provided with a first extrusion device 90a, a second extrusion device 90b, a third extrusion device 90c, a first chamber 95, a second chamber 96 and a third chamber 97, for example, in order to produce a linear body 1a supplied to the nozzle 10. The first chamber 95, the second chamber 96 and the third chamber 97 are arranged in sequence in the vertical direction downward. The third chamber 97 is connected to the nozzle 10.

[0085] The first extrusion device 90a has a housing 91a for housing the first resin composition 80a, and the first resin composition 80a can be extruded from the housing 91a by introducing gas into the housing 91a. The first extrusion device 90a, for example, has a heater (not shown) for heating the first resin composition 80a housed in the housing 91a. The first resin composition 80a, for example, softens by being heated and becomes flowable. The softened first resin composition 80a is pressed on its upper surface by the gas introduced into the housing 91a and extruded from the first extrusion device 90a. It should be noted that the gas sent to the housing 91a is preferably an inert gas such as nitrogen. The heating temperature of the first resin composition 80a can be appropriately set according to the composition of the first resin composition 80a, for example, 100°C to 300°C. The viscosity μ of the first resin composition 80a extruded from the first extrusion device 90a is not particularly limited, for example, 1 to 7000 Pa·s.

[0086] The first resin composition 80a extruded from the first extrusion device 90a moves downward in the vertical direction, for example, to be formed into a fibrous molded body (core 2). That is, the manufacturing method of this embodiment further includes, for example, a step of extruding the first resin composition 80a using the first extrusion device 90a to form the core 2. The core 2 is transported from the first extrusion device 90a to the first chamber 95.

[0087] The first resin composition 80a is preferably a composition suitable for the core of POF. The first resin composition 80a, for example, contains a fluorine-containing polymer (polymer (P)). From the viewpoint of suppressing light absorption caused by the stretching energy of the CH bond, the polymer (P) preferably does not substantially contain hydrogen atoms, and it is particularly preferred that all hydrogen atoms bonded to carbon atoms are replaced by fluorine atoms. In this specification, the polymer (P) does not substantially contain hydrogen atoms means that the content of hydrogen atoms in the polymer (P) is less than 1 mol%.

[0088] The polymer (P) preferably has a fluorinated aliphatic ring structure. The fluorinated aliphatic ring structure may be contained in the main chain of the polymer (P) or in the side chain of the polymer (P). The polymer (P) has, for example, a structural unit (A) represented by the following formula (1).

[0089]

Chemical formula 1

[0090]

[0091] In formula (1), R ff 1 ~R ff 4 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 7 carbon atoms, or a perfluoroalkyl ether group having 1 to 7 carbon atoms. ff 1 With Rff 2 Can be connected to form a ring. "Perfluoro" means that all hydrogen atoms bonded to carbon atoms are replaced by fluorine atoms. In formula (1), the carbon number of the perfluoroalkyl group is preferably 1 to 5, more preferably 1 to 3, and further preferably 1. The perfluoroalkyl group may be linear or branched. Examples of the perfluoroalkyl group include trifluoromethyl, pentafluoroethyl, heptafluoropropyl, and the like.

[0092] In formula (1), the carbon number of the perfluoroalkyl ether group is preferably 1 to 5, and more preferably 1 to 3. The perfluoroalkyl ether group may be linear or branched. Examples of the perfluoroalkyl ether group include perfluoromethoxymethyl and the like.

[0093] In R ff 1 With R ff 2 When the rings are connected to form a ring, the ring may be a five-membered ring or a six-membered ring. Examples of the ring include a perfluorotetrahydrofuran ring, a perfluorocyclopentane ring, and a perfluorocyclohexane ring.

[0094] Specific examples of the structural unit (A) include structural units represented by the following formulae (A1) to (A8).

[0095]

Chemical formula 2

[0096]

[0097] The structural unit (A) is preferably a structural unit (A2) among the structural units represented by the above formulae (A1) to (A8), that is, a structural unit represented by the following formula (2).

[0098]

Chemical formula 3

[0099]

[0100] Polymer (P) can include one or more structural units (A). In polymer (P), the content of structural unit (A) is preferably 20 mol% or more relative to the total of all structural units, and more preferably 40 mol% or more. By including more than 20 mol% of structural units (A), polymer (P) has a tendency to have higher heat resistance. In the case of including more than 40 mol% of structural units (A), polymer (P) has a tendency to have higher transparency and high mechanical strength in addition to high heat resistance. In polymer (P), the content of structural unit (A) is preferably less than 95 mol% relative to the total of all structural units, and more preferably less than 70 mol%.

[0101] The structural unit (A) is derived from, for example, a compound represented by the following formula (3). ff1 ~R ff 4 The same as formula (1). The compound represented by formula (3) can be obtained by a known production method represented by the production method disclosed in Japanese Patent Publication No. 2007-504125.

[0102]

Chemical formula 4

[0103]

[0104] Specific examples of the compound represented by the above formula (3) include compounds represented by the following formulas (M1) to (M8).

[0105]

Chemical formula 5

[0106]

[0107] The polymer (P) may contain other structural units in addition to the structural unit (A). Examples of the other structural units include the following structural units (B) to (D).

[0108] The structural unit (B) is represented by the following formula (4).

[0109]

Chemical formula 6

[0110]

[0111] In formula (4), R 1 ~R 3 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. 4 It represents a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A part of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A part of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom.

[0112] The polymer (P) may contain one or more structural units (B). In the polymer (P), the content of the structural unit (B) is preferably 5 to 10 mol% relative to the total of all structural units. The content of the structural unit (B) may be 9 mol% or less, or 8 mol% or less.

[0113] The structural unit (B) is derived from, for example, a compound represented by the following formula (5). 1 ~R 4 The same as formula (4). The compound represented by formula (5) is a fluorine-containing vinyl ether such as perfluorovinyl ether.

[0114]

Chemical formula 7

[0115]

[0116] The structural unit (C) is represented by the following formula (6).

[0117]

Chemical formula 8

[0118]

[0119] In formula (6), R 5 ~R 8 Each independently represents a fluorine atom or a perfluoroalkyl group having 1 to 7 carbon atoms. The perfluoroalkyl group may have a ring structure. A portion of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom.

[0120] The polymer (P) may contain one or more structural units (C). In the polymer (P), the content of the structural unit (C) is preferably 5 to 10 mol% relative to the total of all structural units. The content of the structural unit (C) may be 9 mol% or less, or 8 mol% or less.

[0121] The structural unit (C) is derived from, for example, a compound represented by the following formula (7). 5 ~R 8 The same as formula (6). The compound represented by formula (7) is a fluorine-containing olefin such as tetrafluoroethylene and chlorotrifluoroethylene.

[0122]

Chemical formula 9

[0123]

[0124] The structural unit (D) is represented by the following formula (8).

[0125]

Chemical formula 10

[0126]

[0127] In formula (8), Z represents an oxygen atom, a single bond or -OC(R 19 R 20 )O-,R 9 ~R 20 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. A portion of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkoxy group may be substituted by a halogen atom other than a fluorine atom. s and t each independently represent an integer from 0 to 5, and s+t is an integer from 1 to 6 (wherein Z is -OC(R 19 R 20)O-, s+t can be 0).

[0128] The structural unit (D) is preferably represented by the following formula (9). The structural unit represented by the following formula (9) is the case where Z is an oxygen atom, s is 0, and t is 2 in the above formula (8).

[0129]

Chemical formula 11

[0130]

[0131] In formula (9), R 141 , R 142 , R 151 and R 152 Each independently represents a fluorine atom, a perfluoroalkyl group having 1 to 5 carbon atoms, or a perfluoroalkoxy group having 1 to 5 carbon atoms. A portion of the fluorine atoms may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkyl group may be substituted by a halogen atom other than a fluorine atom. A portion of the fluorine atoms in the perfluoroalkoxy group may be substituted by a halogen atom other than a fluorine atom.

[0132] The polymer (P) may contain one or more structural units (D). In the polymer (P), the content of the structural unit (D) is preferably 30 to 67 mol% relative to the total of all structural units. The content of the structural unit (D) is, for example, 35 mol% or more, 60 mol% or less, or 55 mol% or less.

[0133] The structural unit (D) is derived from, for example, a compound represented by the following formula (10). 9 ~R 18 , s and t are the same as those in formula (8). The compound represented by formula (10) is a fluorine-containing compound having two or more polymerizable double bonds and capable of cyclopolymerization.

[0134]

Chemical formula 12

[0135]

[0136] The structural unit (D) is preferably derived from a compound represented by the following formula (11). In formula (11), R 141 , R 142 , R 151 and R 152 Same as formula (9).

[0137]

Chemical formula 13

[0138]

[0139] Specific examples of the compound represented by formula (10) or formula (11) include the following compounds.

[0140] CF2=CFOCF2CF=CF2

[0141] CF2=CFOCF(CF3)CF=CF2

[0142] CF2=CFOCF2CF2CF=CF2

[0143] CF2=CFOCF2CF(CF3)CF=CF2

[0144] CF2=CFOCF(CF3)CF2CF=CF2

[0145] CF2=CFOCFClCF2CF=CF2

[0146] CF2=CFOCCl2CF2CF=CF2

[0147] CF2=CFOCF2OCF=CF2

[0148] CF2=CFOC(CF3)2OCF=CF2

[0149] CF2=CFOCF2CF(OCF3)CF=CF2

[0150] CF2=CFCF2CF=CF2

[0151] CF2=CFCF2CF2CF=CF2

[0152] CF2=CFCF2OCF2CF=CF2

[0153] CF2=CFOCF2CFClCF=CF2

[0154] CF2=CFOCF2CF2CCl=CF2

[0155] CF2=CFOCF2CF2CF=CFCl

[0156] CF2=CFOCF2CF(CF3)CCl=CF2

[0157] CF2=CFOCF2OCF=CF2

[0158] CF2=CFOCCl2OCF=CF2

[0159] CF2=CClOCF2OCCl=CF2

[0160] The polymer (P) may further contain other structural units other than the structural units (A) to (D), but preferably does not substantially contain other structural units other than the structural units (A) to (D). It should be noted that the polymer (P) does not substantially contain other structural units other than the structural units (A) to (D) means that the total amount of the structural units (A) to (D) is 95 mol% or more, preferably 98 mol% or more, relative to the total amount of all structural units in the polymer (P).

[0161] The polymerization method of the polymer (P) is not particularly limited, and for example, a common polymerization method such as radical polymerization can be used. The polymerization initiator used for polymerizing the polymer (P) may be a perfluorinated compound.

[0162] The glass transition temperature (Tg) of the polymer (P) is not particularly limited, and is, for example, 100°C to 140°C, may be 105°C or higher, or may be 120°C or higher. In this specification, Tg refers to the midpoint glass transition temperature (Tg) determined in accordance with the provisions of JIS K7121:1987. mg ).

[0163] The first resin composition 80a may contain a polymer (P) as a main component, and is preferably substantially composed of the polymer (P). The first resin composition 80a may further contain additives such as a refractive index adjuster. The first resin composition 80a is solid at room temperature (25° C.), for example.

[0164] The second extrusion device 90b is provided with a housing 91b for housing the second resin composition 80b having a composition suitable for the cladding layer of POF. As the second extrusion device 90b, the device described above for the first extrusion device 90a can be used. In the second extrusion device 90b, by introducing gas into the housing 91b, the second resin composition 80b can be extruded from the housing 91b.

[0165] The second resin composition 80b extruded from the second extrusion device 90b is supplied to the first chamber 95. In the first chamber 95, by coating the core 2 with the second resin composition 80b, the cladding 3 arranged on the outer periphery of the core 2 and covering the outer periphery can be formed. The core 2 coated with the cladding 3 moves from the first chamber 95 to the second chamber 96. In this way, the manufacturing method of the present embodiment further includes, for example, a step of coating the side surface of the core 2 with the second resin composition 80b different from the first resin composition 80a constituting the core 2.

[0166] When the fiber 5 is used as a POF, the refractive index of the second resin composition 80b forming the cladding 3 is preferably lower than the refractive index of the first resin composition 80a forming the core 2. Examples of the resin material contained in the second resin composition 80b include fluorine-containing resins, acrylic resins such as methyl methacrylate, styrene resins, and carbonate resins.

[0167] The third extrusion device 90c, for example, includes a housing portion 91c for housing a third resin composition 80c having a composition suitable for a coating layer (upper cladding layer) of POF, a screw 92 disposed in the housing portion 91c, and a hopper 93 connected to the housing portion 91c. The third extrusion device 90c, for example, includes a heater (not shown) for heating the third resin composition 80c. In the third extrusion device 90c, a granular third resin composition 80c is supplied to the housing portion 91c through the hopper 93. The granular third resin composition 80c supplied to the housing portion 91c is softened by being kneaded by the screw 92 while being heated so as to flow. The softened third resin composition 80c is extruded from the housing portion 91c by the screw 92.

[0168] The third resin composition 80c extruded from the third extruder 90c is supplied to the second chamber 96. In the second chamber 96, the cladding 3 is coated with the third resin composition 80c, so that the coating layer 4 covering the outer periphery of the cladding 3 can be formed. Thus, the linear body 1a having the core 2, the cladding 3, and the coating layer 4 can be obtained. The linear body 1a moves from the second chamber 96 to the third chamber 97.

[0169] Examples of the resin material contained in the third resin composition 80c forming the covering layer 4 include polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyethersulfone, polycarbonate, various engineering plastics, cycloolefin polymers, PTFE, modified PTFE, and PFA.

[0170] The linear body 1a is transported to the first opening 11 of the nozzle 10 through the third chamber 97. A heater (not shown) for heating the linear body 1a may also be provided in the third chamber 97. In the third chamber 97, for example, the temperature and viscosity of the linear body 1a are appropriately adjusted. In the third chamber 97, by heating the linear body 1a, the refractive index adjusting agent contained in the first resin composition 80a can be diffused in the linear body 1a.

[0171] It should be noted that in this embodiment, a molded body having a three-layer structure including a core 2, a cladding 3, and a coating 4 is used as the linear body 1a. However, the structure of the linear body 1a is not limited to a three-layer structure. The structure of the linear body 1a may be a double-layer structure consisting of the core 2 and the cladding 3, or a single-layer structure consisting of the core 2.

[0172] like Figure 1 As shown, the spinning device 100 further includes a nip roller 60, guide rollers 63, 64, 65, and a winding roller 66, for example, in order to convey and wind up the linear body 1b ejected from the nozzle 10. The nip roller 60 is, for example, located below the cooling unit 20. The linear body 1 that has passed through the cooling unit 20 passes between two rollers 61 and 62 of the nip roller 60, for example.

[0173] The guide rollers 63, 64 and 65 are arranged in sequence in the conveying direction of the linear body 1. The linear body 1 that has passed through the clamping roller 60 passes through the guide rollers 63, 64 and 65 and is wound up on the winding roller 66 as the fiber 5. The winding speed U of the above formula (I) can be calculated from the rotation speed of the winding roller 66 and the clamping roller 60, etc.

[0174] The spinning device 100 may also include a displacement meter 70 for measuring the outer diameter of the linear body 1 near the winding roller 66, for example, between the guide roller 65 and the winding roller 66. The outer diameter of the linear body 1 measured by the displacement meter 70 may also be regarded as the outer diameter of the fiber 5. It should be noted that in the manufacturing method of the present embodiment, the linear body 1 is sufficiently cooled in the cooling section 20. Therefore, from the time when the linear body 1 passes through the cooling section 20 to the time when it is wound up by the winding roller 66, there is a tendency that the temperature of the linear body 1 hardly changes and the outer diameter of the linear body 1 hardly changes. In other words, in the manufacturing method of the present embodiment, the outer diameter of the fiber 5 is substantially the same as the outer diameter of the linear body 1 just after passing through the cooling section 20.

[0175] The spinning device 100 may further include a controller (not shown) storing a program for appropriately operating the spinning device 100. The controller may control the driving of each roller, or may control a heater provided in each extruder, for example.

[0176] The fiber 5 made by the manufacturing method of this embodiment is preferably POF. However, the fiber 5 can also be used for other purposes other than POF. For example, as a line woven into a film or a nonwoven fabric, the fiber 5 can be used. The manufacturing method of this embodiment can also be used as a manufacturing method for fibers containing materials other than resin compositions (e.g., glass).

[0177] Example

[0178] Hereinafter, the present invention will be described in further detail with reference to Examples and Comparative Examples, but the present invention is not limited thereto.

[0179] (Production Examples 1 to 15)

[0180] In Manufacturing Examples 1 to 15, fibers are manufactured under the conditions described in Table 1 using a nozzle and a cooling unit. Specifically, a resin composition composed of polycarbonate is extruded from an extrusion device to form a core. The core is introduced into the nozzle as a linear body. The cooling unit has a cooling pipe connected to the nozzle and extending downward from the nozzle, and a cylindrical filter located in the inner space of the cooling pipe and rectifying the cooling fluid. In the inner space of the cooling pipe, the linear body ejected from the nozzle is brought into contact with the cooling fluid and cooled. Air as a cooling fluid is supplied to the inner space of the cooling pipe. Water as a refrigerant is supplied to the storage space of the cooling pipe. The outer diameter of the linear body just after being ejected from the nozzle is the same as the diameter of the opening of the nozzle for ejecting the linear body.

[0181] The outer diameter of the linear body was measured near the winding roll using a displacement meter (LS-9006M manufactured by KEYENCE), and the obtained measured value was regarded as the outer diameter of the fiber. The outer diameter was measured at a cycle of 0.1 seconds and 500 locations. The ratio 3σ / Ave. was calculated based on the obtained results. The relationship between the index M and the ratio 3σ / Ave. is shown in Tables 1 and Figure 3 .

[0182]

Table 1

[0183]

[0184] From Table 1 and Figure 3 It is found that in Production Examples 1, 2, 4 to 6, and 9 to 15 where the index M is 1.52 or less, the value of the ratio (3σ / Ave.) is smaller than that in Production Examples 3, 7, and 8, and the change in the outer diameter of the fiber is suppressed.

[0185] Industrial Applicability

[0186] The manufacturing method of this embodiment is suitable for manufacturing POF.

Claims

1. A method for producing a fiber, comprising: The step of ejecting the softened linear body from a nozzle; as well as The step of winding the linear body so as to pass through a cooling portion to which a cooling fluid is supplied to obtain a fiber, The cooling unit includes a filter for rectifying the cooling fluid. In the cooling unit, the temperature of the cooling fluid is substantially constant in the direction in which the linear body moves. The index M determined by the following formula (I) is 1.52 or less, In the formula (I), Q a is the flow rate of the cooling fluid supplied to the cooling unit, and Q a The unit is m 3 / s, L is the moving distance of the linear body in the cooling unit, and the unit of L is m. T w is the temperature of the linear body just after being ejected from the nozzle, and the T w The unit is ℃, T a is the temperature of the cooling fluid, the T a The unit is ℃, D f is the outer diameter of the fiber, the D f The unit is m, D n is the outer diameter of the linear body just after being ejected from the nozzle, and D n The unit is m, U is the winding speed of the linear body, and the unit of U is m / s. K is 1.0×10 8 ℃·s 2 / m 3 .

2. The manufacturing method according to claim 1, wherein: The index M is 1.0 or less.

3. The manufacturing method according to claim 1, wherein: The temperature T of the linear body immediately after being ejected from the nozzle w It is above 100°C.

4. The manufacturing method according to claim 1, wherein: In the cooling unit, the linear body is cooled by being brought into contact with the cooling fluid.

5. The manufacturing method according to claim 1, wherein: The cooling unit has a cylindrical cooling pipe. The cooling fluid is supplied to an inner space of the cooling pipe, and the linear body passes through the inner space of the cooling pipe.

6. The manufacturing method according to claim 5, wherein: The cooling pipe is connected to the nozzle and extends downward from the nozzle.

7. The manufacturing method according to claim 5, wherein: The cooling pipe has a main body, and the main body includes an inner wall, an outer wall, and a receiving space formed between the inner wall and the outer wall. A refrigerant medium for cooling the cooling fluid is introduced into the accommodation space.

8. The manufacturing method according to claim 5, wherein: The filter is cylindrical and is located in the inner space of the cooling pipe. The linear body passes through the inner space of the filter.

9. The manufacturing method according to claim 1, wherein: The cooling fluid is a gas.

10. The manufacturing method according to claim 1, wherein: The cooling fluid is air.

11. The manufacturing method according to claim 1, wherein: The linear body has a core and a cladding arranged on the periphery of the core, The manufacturing method further includes the step of extruding the resin composition using an extrusion device to form the fiber core.

12. The manufacturing method according to claim 1, wherein: A ratio of a value three times the standard deviation of the outer diameter of the fibers to an average value of the outer diameter of the fibers is 2.0% or less.

13. The manufacturing method according to claim 1, wherein: The fiber is a plastic optical fiber.

Citation Information

Patent Citations

  • Manufacturing method of plastic optical fiber and manufacturing equipment thereof

    JP2006163007A

  • Method for producing fluorine-containing 1,3-dioxolane compound, fluorine-containing 1,3-dioxolane compound, fluorine-containing polymer of fluorine-containing 1,3-dioxolane compound, and optical or electrical material using said polymer

    JP2007504125A

  • Manufacturing device of plastic optical fiber, and manufacturing method thereof

    JP2009186772A

  • Method for manufacturing optical fiber strand