Supported copper-bismuth catalyst for 1,4-butynediol synthesis and preparation method thereof
By using Al2O3 and SiO2 composite oxide carriers to support CuO and Bi2O3 catalysts in the synthesis of 1,4-butynediol, the problem of poor catalyst strength and loss is solved, the catalytic activity and stability are improved, and it is suitable for industrial production.
Patent Information
- Application Number
- CN202310292666.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-23
AI Technical Summary
The existing supported copper-bismuth catalyst used for the synthesis of 1,4-butynediol has poor strength, easy pulverization, short catalyst life, and serious loss of copper and silicon, which affects the continuous operation of industrial devices.
Al2O3 and SiO2 composite oxide carriers are used to support CuO and Bi2O3 catalysts, and through in-situ synthesis of the composite oxide carrier, additive modification, synthesis temperature and filtration speed modulation, the semi-coated state of the active metal is achieved, reducing copper and silicon of loss.
It improves the catalytic activity and stability of the catalyst, reduces the loss of copper and silicon, reduces environmental problems, reduces catalytic costs and operational risks, and is suitable for industrial mass production.
Smart Images

Figure BDA0004142160600000111 
Figure BDA0004142160600000121 
Figure BDA0004142160600000122
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic reaction, and specifically relates to a supported copper-bismuth catalyst for synthesizing 1,4-butynediol and a preparation method thereof. Background Art
[0002] 1,4-Butynediol (BYD) is an important raw material for fine chemicals and organic chemicals. Because it contains relatively active carbon-carbon triple bonds and two hydroxyl groups, it can be used to obtain a variety of high-value-added derivatives through chemical reactions. Its hydrogenation product 1,4-butanediol (BDO) is the basic raw material for the synthesis of γ-butyrolactone (GBL), tetrahydrofuran (THF), polybutylene terephthalate (PBT) and polyurethane (PU). As the country's requirements for the use of disposable biodegradable materials continue to increase, the demand for biodegradable materials PBAT and PBS is also growing, which leads to the growing demand for its upstream raw material BDO. The BDO production capacity will be close to 8 million tons in a few years. The Reppe method of synthesizing 1,4-butanediol through formaldehyde acetylation, also known as the acetylene aldehyde method, is one of the domestic methods for producing BYD with mature technology and significant economic benefits. It is also a relatively successful technical route for the production of fine chemicals in the new coal chemical industry. This process route can combine the raw material advantages of coal-based primary chemicals with the huge market demand for downstream high-value-added chemicals, and play a key role in opening up the industrial chain for efficient and comprehensive utilization of coal.
[0003] The core of the Reppe process is the Cu-Bi catalyst, which is divided into a micron-sized supported catalyst composed of copper oxide, bismuth oxide and siliceous materials and a non-supported catalyst with basic copper carbonate as the active component. For example: Patent application documents US4288641 and US3920759 disclose copper-bismuth catalysts with molecular sieves and magnesium silicate as carriers, respectively. Chinese patent application documents CN102950014, CN102950002 and CN103480382 disclose catalysts with basic copper-bismuth carbonate as the active substance. Chinese patent application document CN102658158 prepares the salts of copper, bismuth and magnesium into a solution, then adds organosilicon and organic solvent ethanol, hydrolyzes and precipitates under alkaline conditions, and then roasts in an inert atmosphere to obtain a Cu Bi / C MgOSiO2 catalyst. Existing industrial production practices show that the supported copper-bismuth catalyst in the Reppe process of synthesizing BYD has poor strength and is easy to pulverize, resulting in a short catalyst life. At the same time, there is a serious loss of copper and silicon, and a large amount of wastewater is generated by the need to remove copper and silicon through an ion exchange device, which seriously affects the continuous operation of the industrial device. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a supported copper-bismuth catalyst for 1,4-butynediol synthesis and a preparation method thereof in view of the above-mentioned deficiencies in the prior art. The supported copper-bismuth catalyst for 1,4-butynediol synthesis of the present invention can effectively promote the synthesis of 1,4-butynediol and has the characteristics of high catalytic activity, less loss of copper and silicon, and good stability.
[0005] To solve the above technical problems, the technical solution adopted by the present invention is: a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, characterized in that the catalyst comprises an Al2O3 and SiO2 composite oxide carrier, and CuO and Bi2O3 supported on the Al2O3 and SiO2 composite oxide carrier, in which the mass percentage of CuO in the catalyst is 25% to 35%, and the mass percentage of Bi2O3 is 1.5% to 4%.
[0006] The above-mentioned supported copper-bismuth catalyst for the synthesis of 1,4-butynediol is characterized in that the mass ratio of Si:Al in the Al2O3 and SiO2 composite oxide carrier is (1-8):1.
[0007] In addition, the present invention also provides a method for preparing the above-mentioned supported copper-bismuth catalyst for 1,4-butynediol synthesis, characterized in that it comprises:
[0008] Step 1, adding reagent I and deionized water to an aluminum source solution; the reagent I is citric acid, urea, glucose, oleylamine or ammonium bicarbonate;
[0009] Step 2: adding reagent II and deionized water to the silicon source solution to obtain solution A; the reagent II is sodium carbonate, potassium carbonate, sodium bicarbonate or ammonium bicarbonate;
[0010] Step 3: Mix the copper source solution with the dilute nitric acid solution containing the bismuth source, add reagent III and deionized water, control the pH of the system to 0.5 with nitric acid, mix well, and obtain solution B; the reagent III is a C2-C8 carboxylic acid compound;
[0011] Step 4: Heat the system of step 1 to 30-95°C, and drip solution A and solution B into the system simultaneously and in parallel under vigorous stirring for 30-360 min;
[0012] Step 5: Immediately after the dropwise addition is completed, the system after the dropwise addition in step 4 is filtered to obtain a filter cake, the filter cake is washed to a conductivity of 30 us / cm and then dried in a vacuum oven to obtain a dried solid phase, and the dried solid phase is calcined in an inert atmosphere at 350 to 750° C. in a tubular furnace to obtain a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol;
[0013] The step five can also be: filtering after aging for 15 to 60 minutes to obtain a filter cake, washing the filter cake until the conductivity is 30 us / cm and then drying it in a vacuum oven to obtain a dried solid phase, and calcining the dried solid phase in an inert atmosphere at 350 to 750° C. in a tubular furnace to obtain a supported copper bismuth catalyst for synthesizing 1,4-butynediol.
[0014] The above method is characterized in that, in step 1, the aluminum source is aluminum sulfate, aluminum nitrate, sodium aluminate or aluminum chloride.
[0015] The above method is characterized in that, in step 1, the mass of the reagent I is 0.1 to 2 times the mass of aluminum.
[0016] The above method is characterized in that in step 2, the silicon source solution is sodium silicate, sodium metasilicate, potassium silicate or ammonium silicate.
[0017] The above method is characterized in that, in step 2, the mass of reagent II is 3.5 to 5 times the mass of silicon.
[0018] The above method is characterized in that, in step three, the copper source is copper nitrate, copper acetate, copper chloride or copper sulfate; in step three, the bismuth source is bismuth nitrate, bismuth chloride, bismuth bromide or bismuth silicate.
[0019] The above method is characterized in that, in step three, the reagent III is benzoic acid, glutaric acid, oxalic acid or malonic acid; in step three, the mass of the reagent III is 0.1 to 0.5 times the mass of copper oxide.
[0020] The above method is characterized in that, in step 4, the system is heated to 50-85°C.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] 1. The supported copper-bismuth catalyst for 1,4-butynediol synthesis of the present invention can effectively promote the synthesis of 1,4-butynediol and has the characteristics of high catalytic activity, less loss of copper and silicon, and good stability.
[0023] 2. The preparation method of the supported copper-bismuth catalyst for 1,4-butynediol synthesis of the present invention utilizes in-situ synthesis of a composite oxide carrier, modification of auxiliary agents, modulation of synthesis temperature, speed and filtration speed to obtain an oxide carrier with suitable strength and particle size. The oxide carrier and active metal are simultaneously generated in-situ, and most of the active metal is embedded in the carrier in a semi-coated state, which can effectively reduce the loss of copper.
[0024] 3. In the preparation method of the supported copper-bismuth catalyst for 1,4-butynediol synthesis of the present invention, an aluminum oxide-silicon oxide composite oxide is used as a carrier, and the silicon oxide content is lower than that of the traditional copper-bismuth catalyst using a siliceous material as a carrier, which can effectively reduce the environmental problems caused by silicon loss.
[0025] 4. In the preparation method of the supported copper-bismuth catalyst for the synthesis of 1,4-butynediol of the present invention, the process of introducing copper and bismuth includes adding reagent III into the system. Reagent III mainly composed of dicarboxylic acid can effectively utilize its competitive adsorption ability for metal particles, reduce the clustering of active metal particles, and achieve a reduction in the copper oxide content under the same reaction effect, which can effectively reduce the catalytic cost and operation risk.
[0026] 5. The preparation method of the supported copper-bismuth catalyst for 1,4-butynediol synthesis of the present invention is easy to control, the raw materials are readily available, the process is simple, the cost is low, and it is easy to industrialize and mass produce.
[0027] The technical solution of the present invention is further described in detail below in conjunction with embodiments. DETAILED DESCRIPTION
[0028] In the supported copper-bismuth catalyst for 1,4-butynediol synthesis of the present invention and the preparation method thereof, the catalyst comprises 25% to 35% by mass of CuO, 1.5% to 4% by mass of Bi2O3, and a composite oxide carrier of Al2O3 and SiO2. The present invention utilizes in-situ synthesis of composite oxide carriers, and can effectively control the strength, particle size and filtration speed of the oxide carrier by modification of auxiliary agents, synthesis temperature and speed modulation. Moreover, the oxide carrier and the active metal are generated in-situ at the same time, and most of the active metal can be embedded in the carrier in a semi-coated state, which can reduce the loss of copper. The catalyst has good stability while maintaining good initial activity.
[0029] The catalyst of the present invention is described in detail below with reference to the examples, but the following description is not intended to limit the present invention.
[0030] A series of supported copper-bismuth catalysts for synthesizing 1,4-butynediol are prepared according to the method of the present invention, as follows.
[0031] Example 1
[0032] The present embodiment provides a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, wherein the catalyst is composed of a silicon oxide-alumina carrier with a Si:Al mass ratio of 5:1 and a supported mass percentage of 35% CuO and 1.5% Bi2O3. The preparation method of the catalyst comprises the following steps:
[0033] Step 1, adding 4.86g of citric acid and 300ml of deionized water to a precipitation container containing 486ml of aluminum sulfate solution; the aluminum concentration in the aluminum sulfate solution is 0.01g / ml; the precipitation container is a common container in the art for stirring and accommodating precipitates, such as a reaction tank;
[0034] Step 2: Add 100 g of sodium carbonate and 1000 ml of deionized water to 254 ml of a sodium silicate solution having a silicon concentration of 0.1 g / ml to obtain a solution A;
[0035] Step 3, 112 ml of a copper nitrate solution having a copper concentration of 0.25 g / ml and 5.38 ml of a dilute nitric acid solution containing bismuth nitrate having a bismuth concentration of 0.25 g / ml are mixed, 3.5 g of benzoic acid and 30 ml of deionized water are added, the pH of the system is controlled to be 0.5 with nitric acid, and the mixture is mixed evenly to obtain a solution B; the dilute nitric acid solution containing bismuth nitrate can be a dilute nitric acid solution containing bismuth nitrate obtained by dissolving bismuth nitrate in a dilute nitric acid solution having a concentration of 20%; the controlling the pH of the system to 0.5 with nitric acid is to add nitric acid to the system after adding benzoic acid and deionized water so that the pH of the system is 0.5;
[0036] Step 4: Heat the precipitation container described in step 1 to 60° C. and drip solution A and solution B into the precipitation container simultaneously and in parallel under vigorous stirring for 120 min.
[0037] Step 5: Immediately after the dropwise addition is completed, filter the system after the dropwise addition in step 4 to obtain a filter cake, wash the filter cake until the conductivity is 30 us / cm, and then bake it in a vacuum oven at 110° C. for 12 hours to obtain a dried solid phase, and calcine the dried solid phase in a tubular furnace at 350° C. under an inert atmosphere for 2 hours to obtain a supported copper bismuth catalyst for the synthesis of 1,4-butynediol.
[0038] Example 2
[0039] The present embodiment provides a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, wherein the catalyst is composed of a silicon oxide-alumina carrier with a Si:Al mass ratio of 1:1 and a supported mass percentage of 25% CuO and 2.0% Bi2O3, and the preparation method of the catalyst comprises the following steps:
[0040] Step 1: Add 35.56 g of urea and 600 ml of deionized water to a precipitation container containing 1778 ml of sodium aluminate solution; the aluminum concentration in the sodium aluminate solution is 0.01 g / ml;
[0041] Step 2: Add 80 g of potassium carbonate and 800 ml of deionized water to 184 ml of a sodium metasilicate solution having a silicon concentration of 0.1 g / ml to obtain a solution A;
[0042] Step 3, 79.9 ml of a copper acetate solution having a copper concentration of 0.25 g / ml and 7.17 ml of a dilute nitric acid solution containing bismuth chloride having a bismuth concentration of 0.25 g / ml are mixed, 6.25 g of glutaric acid and 30 ml of deionized water are added, the pH of the system is controlled to 0.5 with nitric acid, and the mixture is mixed evenly to obtain a solution B; the dilute nitric acid solution containing bismuth chloride can be a dilute nitric acid solution containing bismuth chloride obtained by dissolving bismuth chloride in a dilute nitric acid solution having a concentration of 20%;
[0043] Step 4: Heat the precipitation container described in step 1 to 95°C, and drip solution A and solution B into the precipitation container simultaneously and in parallel under vigorous stirring for 30 minutes;
[0044] Step 5: After aging for 60 minutes, filter to obtain a filter cake, wash the filter cake until the conductivity is 30 us / cm, and then bake it in a vacuum oven at 110° C. for 12 hours to obtain a dried solid phase, and calcine the dried solid phase in a tubular furnace at 550° C. under an inert atmosphere for 2 hours to obtain a supported copper bismuth catalyst for the synthesis of 1,4-butynediol.
[0045] Example 3
[0046] The present embodiment provides a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, wherein the catalyst is composed of a silicon oxide-alumina carrier with a Si:Al mass ratio of 8:1 and a supported mass percentage of 30% CuO and 4.0% Bi2O3, and the preparation method of the catalyst comprises the following steps:
[0047] Step 1: Add 5.02 g of glucose and 100 ml of deionized water to a precipitation container containing 335 ml of aluminum nitrate solution; the aluminum concentration in the aluminum nitrate solution is 0.01 g / ml.
[0048] Step 2: Add 120 g of sodium bicarbonate and 1200 ml of deionized water to 278.6 ml of a potassium silicate solution having a silicon concentration of 0.1 g / ml to obtain a solution A;
[0049] Step 3, 95.84 ml of a copper chloride solution having a copper concentration of 0.25 g / ml and 14.35 ml of a dilute nitric acid solution containing bismuth bromide having a bismuth concentration of 0.25 g / ml are mixed, 3 g of oxalic acid and 30 ml of deionized water are added, and the pH of the system is controlled to 0.5 with nitric acid, and mixed evenly to obtain a solution B; the dilute nitric acid solution containing bismuth bromide can be a dilute nitric acid solution containing bismuth bromide obtained by dissolving bismuth bromide in a dilute nitric acid solution having a concentration of 20%;
[0050] Step 4: Heat the precipitation container described in step 1 to 50° C. and drip solution A and solution B into the precipitation container simultaneously and in parallel under vigorous stirring for 360 min.
[0051] Step 5: After aging for 15 minutes, filter to obtain a filter cake, wash the filter cake until the conductivity is 30 us / cm, and then bake it in a vacuum oven at 110° C. for 12 hours to obtain a dried solid phase, and calcine the dried solid phase in a tubular furnace at 650° C. under an inert atmosphere for 2 hours to obtain a supported copper bismuth catalyst for the synthesis of 1,4-butynediol.
[0052] Example 4
[0053] The present embodiment provides a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, wherein the catalyst is composed of a silicon oxide-alumina carrier with a Si:Al mass ratio of 5:1 and a supported mass percentage of 30% CuO and 3.5% Bi2O3, and the preparation method of the catalyst comprises the following steps:
[0054] Step 1: Add 0.51 g of oleylamine and 300 ml of deionized water to a precipitation container containing 510 ml of aluminum chloride solution; the aluminum concentration in the aluminum chloride solution is 0.01 g / ml;
[0055] Step 2: Add 100 g of ammonium bicarbonate and 1000 ml of deionized water to 265.5 ml of ammonium silicate solution having a silicon concentration of 0.1 g / ml to obtain solution A;
[0056] Step 3, 95.86 ml of a copper sulfate solution having a copper concentration of 0.25 g / ml and 12.56 ml of a dilute nitric acid solution containing bismuth silicate having a bismuth concentration of 0.25 g / ml are mixed, 15 g of malonic acid and 30 ml of deionized water are added, the pH of the system is controlled to 0.5 with nitric acid, and the mixture is mixed evenly to obtain a solution B; the dilute nitric acid solution containing bismuth silicate can be a dilute nitric acid solution containing bismuth silicate obtained by dissolving bismuth silicate in a dilute nitric acid solution having a concentration of 20%;
[0057] Step 4: Heat the precipitation container described in step 1 to 30°C, and drip solution A and solution B into the precipitation container simultaneously and in parallel under vigorous stirring for 240 minutes;
[0058] Step 5: After aging for 60 minutes, filter to obtain a filter cake, wash the filter cake until the conductivity is 30 us / cm, and then bake it in a vacuum oven at 110° C. for 12 hours to obtain a dried solid phase, and calcine the dried solid phase in a tubular furnace at 750° C. under an inert atmosphere for 2 hours to obtain a supported copper bismuth catalyst for the synthesis of 1,4-butynediol.
[0059] Example 5
[0060] The present embodiment provides a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, wherein the catalyst is composed of a silicon oxide-alumina carrier with a Si:Al mass ratio of 5:1 and a supported mass percentage of 35% CuO and 3.0% Bi2O3, and the preparation method of the catalyst comprises the following steps:
[0061] Step 1: Add 2.38 g of ammonium bicarbonate and 300 ml of deionized water to a precipitation container containing 476 ml of sodium aluminate solution; the aluminum concentration in the sodium aluminate solution is 0.01 g / ml;
[0062] Step 2: Add 90 g of sodium bicarbonate and 900 ml of deionized water to 247 ml of a sodium silicate solution having a silicon concentration of 0.1 g / ml to obtain a solution A;
[0063] Step 3, 112 ml of a copper nitrate solution having a copper concentration of 0.25 g / ml and 10.76 ml of a dilute nitric acid solution containing bismuth nitrate having a bismuth concentration of 0.25 g / ml are mixed, 8.75 g of glutaric acid and 30 ml of deionized water are added, the pH of the system is controlled to 0.5 with nitric acid, and the mixture is mixed evenly to obtain a solution B; the dilute nitric acid solution containing bismuth nitrate can be a dilute nitric acid solution containing bismuth nitrate obtained by dissolving bismuth nitrate in a dilute nitric acid solution having a concentration of 20%;
[0064] Step 4: Heat the precipitation container described in step 1 to 70° C. and drip solution A and solution B into the precipitation container simultaneously and in parallel under vigorous stirring for 90 min.
[0065] Step 5: Immediately after the dropwise addition is completed, filter the system after the dropwise addition in step 4 to obtain a filter cake, wash the filter cake until the conductivity is 30 us / cm, and then bake it in a vacuum oven at 110° C. for 12 hours to obtain a dried solid phase, and calcine the dried solid phase in a tubular furnace at 500° C. under an inert atmosphere for 2 hours to obtain a supported copper bismuth catalyst for the synthesis of 1,4-butynediol.
[0066] Example 6
[0067] The present embodiment provides a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, wherein the catalyst is composed of a silicon oxide-alumina carrier with a Si:Al mass ratio of 5:1 and a supported mass percentage of 35% CuO and 3.0% Bi2O3, and the preparation method of the catalyst comprises the following steps:
[0068] Step 1: Add 4.76 g urea and 300 ml deionized water to a precipitation container containing 476 ml sodium aluminate solution; the aluminum concentration in the sodium aluminate solution is 0.01 g / ml
[0069] Step 2: Add 120 g of sodium bicarbonate and 1000 ml of deionized water to 247 ml of a sodium silicate solution having a silicon concentration of 0.1 g / ml to obtain a solution A;
[0070] Step 3, 112 ml of a copper nitrate solution having a copper concentration of 0.25 g / ml and 10.76 ml of a dilute nitric acid solution containing bismuth nitrate having a bismuth concentration of 0.25 g / ml are mixed, 17.5 g of glutaric acid and 30 ml of deionized water are added, the pH of the system is controlled to 0.5 with nitric acid, and the mixture is mixed evenly to obtain a solution B; the dilute nitric acid solution containing bismuth nitrate can be a dilute nitric acid solution containing bismuth nitrate obtained by dissolving bismuth nitrate in a dilute nitric acid solution having a concentration of 20%;
[0071] Step 4: Heat the precipitation container described in step 1 to 85°C, and drip solution A and solution B into the precipitation container simultaneously and in parallel under vigorous stirring for 45 minutes;
[0072] Step 5: Immediately after the dropwise addition is completed, filter the system after the dropwise addition in step 4 to obtain a filter cake, wash the filter cake until the conductivity is 30 us / cm, and then bake it in a vacuum oven at 110° C. for 12 hours to obtain a dried solid phase, and calcine the dried solid phase in a tubular furnace at 500° C. under an inert atmosphere for 2 hours to obtain a supported copper bismuth catalyst for the synthesis of 1,4-butynediol.
[0073] Example 7
[0074] The present embodiment provides a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, wherein the catalyst is composed of a silicon oxide-alumina carrier with a Si:Al mass ratio of 5:1 and a supported mass percentage of 35% CuO and 3.0% Bi2O3, and the catalyst preparation method comprises the following steps:
[0075] Step 1: Add 4.76 g of urea and 300 ml of deionized water to a precipitation container containing 476 ml of sodium aluminate solution; the aluminum concentration in the sodium aluminate solution is 0.01 g / ml;
[0076] Step 2: Add 120 g of sodium bicarbonate and 1000 ml of deionized water to 247 ml of a sodium silicate solution having a silicon concentration of 0.1 g / ml to obtain a solution A;
[0077] Step 3, 112 ml of a copper nitrate solution having a copper concentration of 0.25 g / ml and 10.76 ml of a dilute nitric acid solution containing bismuth nitrate having a bismuth concentration of 0.25 g / ml are mixed, 17.5 g of glutaric acid and 30 ml of deionized water are added, the pH of the system is controlled to 0.5 with nitric acid, and the mixture is mixed evenly to obtain a solution B; the dilute nitric acid solution containing bismuth nitrate can be a dilute nitric acid solution containing bismuth nitrate obtained by dissolving bismuth nitrate in a dilute nitric acid solution having a concentration of 20%;
[0078] Step 4: Heat the precipitation container described in step 1 to 50° C. and drip solution A and solution B into the precipitation container simultaneously and in parallel under vigorous stirring for 360 min.
[0079] Step 5: After aging for 30 minutes, filter to obtain a filter cake, wash the filter cake until the conductivity is 30 us / cm, and then bake it in a vacuum oven at 110° C. for 12 hours to obtain a dried solid phase, and calcine the dried solid phase in a tubular furnace at 500° C. under an inert atmosphere for 2 hours to obtain a supported copper bismuth catalyst for the synthesis of 1,4-butynediol.
[0080] Example 8
[0081] The present embodiment provides a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, wherein the catalyst is composed of a silicon oxide-alumina carrier with a Si:Al mass ratio of 5:1 and a supported mass percentage of 35% CuO and 3.0% Bi2O3, and the preparation method of the catalyst comprises the following steps:
[0082] Step 1: Add 4.76 g of oleylamine and 300 ml of deionized water to a precipitation container containing 476 ml of sodium aluminate solution; the aluminum concentration in the sodium aluminate solution is 0.01 g / ml;
[0083] Step 2: Add 100 g of sodium carbonate and 1000 ml of deionized water to 247 ml of a sodium silicate solution having a silicon concentration of 0.1 g / ml to obtain a solution A;
[0084] Step 3, 112 ml of a copper nitrate solution having a copper concentration of 0.25 g / ml and 10.76 ml of a dilute nitric acid solution containing bismuth nitrate having a bismuth concentration of 0.25 g / ml are mixed, 17.5 g of malonic acid and 30 ml of deionized water are added, the pH of the system is controlled to 0.5 with nitric acid, and the mixture is mixed evenly to obtain a solution B; the dilute nitric acid solution containing bismuth nitrate can be a dilute nitric acid solution containing bismuth nitrate obtained by dissolving bismuth nitrate in a dilute nitric acid solution having a concentration of 20%;
[0085] Step 4: Heat the precipitation container described in step 1 to 65°C, and drip solution A and solution B into the precipitation container simultaneously and in parallel under vigorous stirring for 150 minutes;
[0086] Step 5: After aging for 45 minutes, filter to obtain a filter cake, wash the filter cake until the conductivity is 30 us / cm, and then bake it in a vacuum oven at 110° C. for 12 hours to obtain a dried solid phase, and calcine the dried solid phase in a tubular furnace at 650° C. under an inert atmosphere for 2 hours to obtain a supported copper bismuth catalyst for the synthesis of 1,4-butynediol.
[0087] Performance evaluation:
[0088] Physical property test: Taking the catalyst used in industry as a comparison, the comparison catalyst and the catalyst of Examples 1 to 8 were tested under the following conditions: 20g of the catalyst was slurried with 400ml of deionized water, pH was adjusted to 5.5-6.0 with acetic acid, stirred at a speed of 900r / min for 30 days, filtered with a Buchner funnel with a diameter of 60mm, and a fixed negative pressure was maintained. When the original slurry was not completely drained and a dry filter cake was not formed, 1000ml of water was added to test the filterability of the catalyst, the filter cake was subjected to particle size analysis, and the filtrate was measured for copper residue. The specific results are shown in Table 1.
[0089] Chemical activity test: With the catalyst used in industry as a comparison, after activating the comparison catalyst and the catalyst of Examples 1 to 8, 1.0g of dry catalyst was taken and added to a stainless steel reactor with stirring containing 135ml of formaldehyde aqueous solution, the volume percentage of formaldehyde in the formaldehyde aqueous solution was 37%, and the pH was adjusted to 8 with a mass concentration of 20% NaOH solution, and the reactor was purged with nitrogen 3 times to completely replace the air in the reactor, and then purged with acetylene. After complete replacement, the acetylene pressure of the reactor was controlled at 1 atmosphere with a pressure regulating valve, and the temperature was raised to 80°C for reaction for 24h and then cooled, and then the acetylene was stopped, and the reactor was purged with nitrogen, and the reaction liquid was analyzed by GC, and the formaldehyde conversion rate was analyzed by sodium sulfite titration. The specific results are shown in Table 2.
[0090] It can be seen from Table 1 and Table 2 that the catalyst of the present invention has moderate particle size, good strength, good filterability and less copper loss, and exhibits good activity and selectivity in the acetylene-aldehyde reaction.
[0091] Table 1: Catalyst physical property test results
[0092]
[0093]
[0094] Table 2 Catalyst chemical activity test results
[0095]
[0096]
[0097] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol, characterized in that: The catalyst comprises an Al2O3 and SiO2 composite oxide carrier, and CuO and Bi2O3 supported on the Al2O3 and SiO2 composite oxide carrier, wherein the mass percentage of CuO in the catalyst is 25% to 35%, and the mass percentage of Bi2O3 is 1.5% to 4%; the method comprises: Step 1, adding reagent I and deionized water to an aluminum source solution; the reagent I is citric acid, urea, glucose or oleylamine; the aluminum source is aluminum sulfate, aluminum nitrate, sodium aluminate or aluminum chloride; Step 2: Add reagent II and deionized water to the silicon source solution to obtain solution A; the reagent II is sodium carbonate, potassium carbonate, sodium bicarbonate or ammonium bicarbonate; the silicon source solution is sodium silicate, sodium metasilicate, potassium silicate or ammonium silicate; Step 3: Mix the copper source solution and the dilute nitric acid solution containing a bismuth source, add reagent III and deionized water, control the pH of the system to 0.5 with nitric acid, mix well, and obtain solution B; the reagent III is a C2~C8 carboxylic acid compound; Step 4: Heat the system of step 1 to 30-95°C, and drip solution A and solution B into the system simultaneously and in parallel under vigorous stirring for 30-360 min; Step 5: Immediately after the dropwise addition is completed, the system after the dropwise addition in step 4 is filtered to obtain a filter cake, the filter cake is washed to a conductivity of 30 us / cm and then dried in a vacuum oven to obtain a dried solid phase, and the dried solid phase is calcined in an inert atmosphere in a tubular furnace at 350-750° C. to obtain a supported copper-bismuth catalyst for the synthesis of 1,4-butynediol; The step five can also be: filtering after aging for 15 to 60 minutes to obtain a filter cake, washing the filter cake until the conductivity is 30 us / cm and then drying it in a vacuum oven to obtain a dried solid phase, and calcining the dried solid phase in an inert atmosphere at 350 to 750° C. in a tubular furnace to obtain a supported copper bismuth catalyst for the synthesis of 1,4-butynediol.
2. The method according to claim 1, characterized in that The mass ratio of Si:Al in the Al2O3 and SiO2 composite oxide carrier is (1-8):
1.
3. The method according to claim 1, characterized in that In step 1, the mass of the reagent I is 0.1 to 2 times the mass of aluminum.
4. The method according to claim 1, characterized in that: In step 2, the mass of the reagent II is 3.5 to 5 times the mass of silicon.
5. The method according to claim 1, characterized in that In step three, the copper source is copper nitrate, copper acetate, copper chloride or copper sulfate; in step three, the bismuth source is bismuth nitrate, bismuth chloride, bismuth bromide or bismuth silicate.
6. The method according to claim 1, characterized in that In step 3, the reagent III is benzoic acid, glutaric acid, oxalic acid or malonic acid; in step 3, the mass of the reagent III is 0.1 to 0.5 times the mass of copper oxide.
7. The method according to claim 1, characterized in that In step 4, the system is heated to 50-85°C.
Citation Information
Cited By
Preparation method of composite catalyst for synthesizing 1, 4-butynediol
CN119500147A
A method for preparing a composite catalyst for synthesizing 1,4-butynediol
CN119500147B