A barium-containing L molecular sieve and its preparation method and application

By adjusting the feeding ratio of barium and aluminum and the hydrothermal crystallization conditions during the preparation of L molecular sieves, the problems of high barium dosage and low crystallinity were solved, and barium-containing L molecular sieves with high crystallinity and suitable morphology were prepared. By supporting the platinum catalyst, the selectivity and activity stability of the aromatization reaction are improved.

CN116328826BActive Publication Date: 2024-10-11CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111596363.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-24
Publication Date
2024-10-11
Estimated Expiration
2041-12-24

AI Technical Summary

Technical Problem

The preparation of barium-containing flake L molecular sieves in the prior art has the problems of high barium dosage, low crystallinity and waste of raw materials, which affects its application efficiency in catalytic reactions.

Method used

By mixing barium source, aluminum source, silicon source and inorganic alkali to form a gel, perform a hydrothermal crystallization reaction, supplement aluminum sol during the reaction process, adjust the feed ratio to reduce the silicon-aluminum ratio, and improve crystallinity and raw material utilization. , to prepare barium-containing L molecular sieves with suitable morphology index distribution.

Benefits of technology

The obtained barium-containing L molecular sieve has high relative crystallinity, low grain length/diameter ratio and good morphology index distribution. The platinum-loaded catalyst shows high selectivity and good activity stability in the aromatization reaction of n-alkanes. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003431329490000141
    Figure BDA0003431329490000141
  • Figure BDA0003431329490000151
    Figure BDA0003431329490000151
  • Figure BDA0003431329490000171
    Figure BDA0003431329490000171
Patent Text Reader

Abstract

A barium-containing L molecular sieve has a chemical composition of (0.03-0.1)BaO:(0.9-1.3)M2O:Al2O3:(5-8)SiO2, M is K or / and Na, the average crystal grain diameter of the molecular sieve is 0.10-0.35 μm, the average crystal grain length / diameter ratio is 0.20-0.50, and the crystal grains with a morphology index R of 0.1-0.5 account for more than 91% by mass of the total crystal grains. The catalyst prepared by loading platinum on the barium-containing L molecular sieve is used for the aromatization reaction of normal alkanes, and has high aromatization selectivity and good activity stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an L molecular sieve containing heteroatoms and a preparation method and application thereof, and specifically, to an L molecular sieve containing barium and a preparation method and application thereof. Background Art

[0002] L molecular sieve is a synthetic molecular sieve developed by Union Carbide in 1965. L molecular sieve belongs to the hexagonal crystal system. Its framework is composed of cancrystal cages (CAN cages) and double six-membered rings (D6R). CAN cages and D6R are alternately connected to form CAN-D6R-CAN cage columns, which are then connected to each other around the six-fold axis along the c-axis to form a three-dimensional framework structure with a one-dimensional twelve-ring pore system. The pore diameter is The chemical composition formula of a typical L molecular sieve framework is as follows:

[0003] (0.9~1.3)M 2 / n O:Al2O3:xSiO2:yH2O

[0004] Where M is a metal ion. For L molecular sieve, the most important metal ion is K + , can also be replaced by other alkali metals or alkaline earth metals, but generally L molecular sieve framework has more than 90% K + It is not easily exchanged. n is the valence of M, x=5~7, y=0~9.

[0005] Platinum-loaded L molecular sieve can be used as a good catalyst for the dehydrogenation and cyclization of normal alkanes. Compared with traditional reforming catalysts, platinum-loaded L molecular sieve catalyst (Pt / KL) is used to catalyze the aromatization reaction of n-hexane, which has higher activity and selectivity, so this catalyst has always received widespread attention. Companies such as Chevron and EXXON have conducted extensive research on the modification of Pt / KL catalysts for dehydrogenation and reforming reactions. Heteroatom incorporation is one of the important means of modifying L molecular sieve. After the heteroatoms are introduced into the molecular sieve framework, its structure, surface acidity and alkalinity, adsorption properties and other properties are affected, thereby changing its catalytic performance and expanding its application range.

[0006] The length / diameter ratio of L molecular sieve crystals can affect their catalytic performance. Trakarnroek et al. reported in the literature (Applied Catalysis A: General 2006, 313, 189) that for Pt / KL catalytic materials, Pt clusters in shorter molecular sieve channels have better dispersion and accessibility, which can prevent hydrocarbon molecules from being retained in the channels for a long time, thereby helping to improve the activity, selectivity and service life of the catalytic material. Therefore, a lower length / diameter ratio and shorter molecular sieve channels are conducive to improving the aromatization performance of Pt / KL catalysts.

[0007] CN106395851A discloses a LTL molecular sieve containing Ba heteroatom and a preparation method thereof, wherein the preparation method of the molecular sieve comprises: mixing a barium source, an inorganic base, an aluminum source, a silicon source, water and an alcohol in a molar ratio to obtain a sol, then aging and crystallizing in sequence, separating the obtained solid, washing, drying and then roasting to obtain the molecular sieve. The synthesis method is simple, the single-pot yield is high, and the synthesis and operation costs are low; the product obtained by the method has good crystallinity, purity and a more regular morphology. The product is used in the aromatization reaction of normal alkanes, and can significantly improve the yield of aromatics, especially the yield of C8 aromatics. The disadvantage of the preparation method is that the amount of barium used is high and alcohol needs to be dissolved.

[0008] US5491119 discloses a barium-containing L molecular sieve, the average length of the molecular sieve crystals is less than or equal to 0.6 microns, the average length / diameter ratio is less than 0.2, and it is in the form of flat sheets. The preparation method is: a certain number of moles of H2O, divalent cations, K2O, Si2O and Al2O3 are mixed, wherein the molar ratio of K2O to Si2O is 0.2-0.35, the molar ratio of Si2O to Al2O3 is 15-160, and the molar ratio of H2O to K2O is 45-70; then heated and crystallized to form a molecular sieve, wherein the divalent cations are preferably magnesium and barium. The preparation method has good repeatability, and the obtained L molecular sieve product has a flat disc-shaped appearance and a lower length / diameter ratio. However, the preparation of barium-containing thin-sheet L molecular sieves currently usually requires hydrothermal crystallization conditions with a high silicon-aluminum ratio to generate, so a large amount of silicon source in the initial feed remains in the mother liquor after the reaction, resulting in a waste of raw materials. At the same time, the introduction of barium often affects the crystallinity of the molecular sieve, thereby adversely affecting its use in catalytic reactions. Therefore, the current preparation method of flaky L molecular sieve has certain limitations in the field of industrial application. Summary of the invention

[0009] The purpose of the present invention is to provide a barium-containing L molecular sieve and a preparation method thereof. The catalyst prepared by loading platinum on the barium-containing L molecular sieve is used for the aromatization reaction of normal alkanes and has high aromatization selectivity and good activity stability.

[0010] The barium-containing L molecular sieve provided by the present invention has a chemical composition of (0.03-0.1)BaO:(0.9-1.3)M2O:Al2O3:(5-8)SiO2, wherein M is K and / or Na, the average grain diameter of the L molecular sieve is 0.10-0.35 μm, the average grain length / diameter ratio is 0.20-0.50, and the grains with a morphology index R of 0.1-0.5 account for more than 91% by mass of the total grains.

[0011] The barium-containing L molecular sieve provided by the present invention has high relative crystallinity, low average grain length / diameter ratio, flat sheet structure, and suitable morphology index distribution. The catalyst prepared by the molecular sieve loaded with platinum is used for the aromatization reaction of normal alkanes and has high aromatization selectivity and good activity stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is a schematic diagram of the parameters taken by the morphology index R and the grain length / diameter ratio λ of the barium-containing L molecular sieve synthesized by the present invention.

[0013] Figure 2 It is the X-ray diffraction spectrum of the barium-containing L molecular sieve synthesized in Examples 1 and 2 of the present invention and Comparative Examples 1 and 2.

[0014] Figure 3 This is a scanning electron microscope photograph of the barium-containing L molecular sieve synthesized in Example 1 of the present invention.

[0015] Figure 4 This is a scanning electron microscope photograph of the barium-containing L molecular sieve synthesized in Example 2 of the present invention.

[0016] Figure 5 This is a scanning electron microscope photograph of the barium-containing L molecular sieve synthesized in Comparative Example 2. DETAILED DESCRIPTION

[0017] The barium-containing L molecular sieve provided by the present invention has an appropriate barium content, and the molecular sieve crystal grain length / diameter ratio is low, presents a flat sheet structure, and has an appropriate morphology index distribution. The molecular sieve is prepared by mixing a barium source, an aluminum source, a silicon source, an inorganic base and water to form a first feed mixture gel, and then performing a hydrothermal crystallization reaction, and supplementing aluminum sol once or multiple times during the reaction to obtain a barium-containing L molecular sieve. The higher silicon-aluminum ratio in the first feed allows a flaky L molecular sieve with a low length / diameter ratio to be obtained, and the proportion of each substance in the total feed is adjusted by supplementing aluminum sol in the later stage of the reaction, and the silicon-aluminum ratio of the overall feed is reduced without changing the high silicon-aluminum ratio of the initial feed. While maintaining the morphology of the molecular sieve, a large amount of silicon source remaining in the crystallization reaction is further reacted, thereby improving the relative crystallinity of the molecular sieve and the utilization rate of the raw materials, and making the synthesized molecular sieve have an appropriate morphology index distribution. The catalyst prepared by loading platinum on the barium-containing L molecular sieve of the present invention is used for the aromatization reaction of normal alkanes, has high aromatization selectivity and good activity stability, and has a high aromatics yield.

[0018] In the present invention, the grain morphology index R is calculated by formula (1), and R represents the integrity of the L molecular sieve grains.

[0019] R=I 2 / (d·h) (1)

[0020] The length / diameter ratio λ of the grain is calculated by formula (2):

[0021] λ=I / d (2)

[0022] In formulas (1) and (2), I is the distance from the outermost top to the bottom of the molecular sieve crystal cylinder, d is the maximum diameter of the molecular sieve crystal cylinder, and h is the longest distance in the axial direction of the molecular sieve crystal cylinder. Figure 1 In the figure, I, d, and h of the grains are specifically marked.

[0023] In formula (1), the closer the morphology index R is to 1, the closer the grains are to a cylinder. In formula (2), the smaller the length / diameter ratio of the grains, the closer the molecular sieve grains are to a flake.

[0024] The L molecular sieve provided by the present invention has a chemical composition preferably of (0.03-0.09)BaO:(0.9-1.3)M2O:Al2O3:(5.5-7)SiO2. The average grain diameter of the L molecular sieve is preferably 0.20-0.30 μm, the average grain length / diameter ratio is preferably 0.22-0.40, in the grain integrity distribution, the grains with a morphology index R of 0.1-0.5 preferably account for 92-98% of the total grain amount, and the relative crystallinity is preferably greater than 95%.

[0025] The method for preparing barium-containing L molecular sieve provided by the present invention comprises the following steps:

[0026] (1) mixing a barium source, an aluminum source, a silicon source, an inorganic base and water to prepare a first-feed mixture gel, wherein the molar ratio of each substance in the first-feed mixture gel is (0.06-0.3)BaO:(2.5-8)M2O:Al2O3:(13-40)SiO2:(200-400)H2O, where M is K or / and Na, and subjecting the first-feed mixture gel to a hydrothermal crystallization reaction,

[0027] (2) Mixing an aluminum source, an inorganic base and water to prepare a feed aluminum sol, wherein the molar ratio of each substance in the feed aluminum sol is (0.5-2.0) M2O:Al2O3:(5-25)H2O, where M is K or / and Na, and adding the feed aluminum sol to the material obtained after hydrothermal crystallization of the first feed mixture gel described in step (1) to obtain a total gel of the reaction system, wherein the molar ratio of each substance in the total gel of the reaction system is (0.01-0.05) BaO:(1.5-3.0) M2O:Al2O3:(5-9) SiO2:(80-150) H2O, continuing the hydrothermal crystallization reaction, and performing solid-liquid separation on the product after hydrothermal crystallization to obtain a solid and a mother liquor, and washing and drying the obtained solid to obtain a barium-containing L molecular sieve.

[0028] In the preparation process of the first batch of mixed gel in step (1), there is no special requirement for the order of adding raw materials. The preferred order of adding raw materials is: dissolving the barium source in water to form a solution and adding it to the alkali-containing aluminum sol, and then mixing it with the silicon source evenly.

[0029] The molar ratio of aluminum in the aluminum sol in the step (2) to aluminum in the first feeding mixture gel in the step (1) is preferably 1 to 3.

[0030] The temperature for the hydrothermal crystallization reaction of the first feed mixture gel in step (1) is preferably 100-200° C., more preferably 120-180° C., and the time is preferably 15-60, more preferably 20-55 hours.

[0031] The temperature for the hydrothermal crystallization reaction after adding the aluminum sol in step (2) is preferably 100-200° C., more preferably 120-180° C., and the time is preferably 15-60 hours, more preferably 20-55 hours.

[0032] Preferably, in the step (2), the feed aluminum sol is added to the material obtained after the hydrothermal crystallization of the first feed mixture gel described in step (1) in multiple times, and a hydrothermal crystallization reaction is carried out after each addition of the feed aluminum sol. After the last addition of the feed aluminum sol, a total gel of the reaction system is obtained. The molar ratio of each substance in the total gel of the reaction system is preferably (0.01-0.05)BaO:(1.5-3.0)M2O:Al2O3:(5-9)SiO2:(80-150)H2O. The product after the last hydrothermal crystallization reaction is subjected to solid-liquid separation to obtain a solid and a mother liquor. The obtained solid is washed and dried to obtain a barium-containing L molecular sieve.

[0033] The number of times of adding the supplementary aluminum sol to the material after hydrothermal crystallization in step (1) is preferably 2 to 3 times, that is, the supplementary aluminum sol is added two to three times to the material obtained after hydrothermal crystallization of the first feed mixture gel in step (1).

[0034] Optionally, the supplementary aluminum sol is added twice to the material obtained after hydrothermal crystallization of the first feed mixture gel described in step (1), and a hydrothermal crystallization reaction is carried out after each addition of the supplementary aluminum sol. The molar ratio of aluminum in the second feed aluminum sol: aluminum in the first feed aluminum sol: aluminum in the first feed mixture gel is preferably 0.5-2.5:0.5-2.5:1.

[0035] Optionally, the supplementary aluminum sol is added three times to the material obtained after hydrothermal crystallization of the first feed mixture gel described in step (1), and a hydrothermal crystallization reaction is carried out after each addition of the supplementary aluminum sol. The molar ratio of aluminum in the third supplementary aluminum sol: aluminum in the second supplementary aluminum sol: aluminum in the first supplementary aluminum sol: aluminum in the first feed mixture gel is preferably 0.5-2:0.5-2:0.5-2:1.

[0036] In the above method of preparing barium-containing L molecular sieve by adding aluminum sol as feed material for multiple times, the temperature of the hydrothermal crystallization reaction after each addition of aluminum sol as feed material is preferably 100-200°C, more preferably 120-180°C, and the time is preferably 15-60 hours, more preferably 20-55 hours.

[0037] In the step (2), the molar ratio of each substance in the added aluminum sol is preferably (1.0-2.0) M2O:Al2O3:(5-22) H2O.

[0038] The drying temperature of the washed solid obtained after crystallization in step (2) is preferably 80 to 120° C., and the drying time is preferably 2 to 14 hours.

[0039] In the method of the present invention, the barium source is preferably selected from barium hydroxide and / or barium nitrate, the aluminum source is preferably selected from aluminum hydroxide and / or sodium aluminate, the silicon source is preferably selected from silica sol with a SiO2 content of 20 to 45% by mass, and the inorganic base is preferably selected from potassium hydroxide and / or sodium hydroxide.

[0040] The barium-containing L molecular sieve may also be calcined after drying, and the calcination temperature is preferably 300-650°C, more preferably 350-450°C.

[0041] The present invention also provides a normal alkane aromatization catalyst, comprising the barium-containing L molecular sieve of the present invention and platinum loaded thereon, wherein the platinum content is preferably 0.4-1.5% by mass calculated based on the barium-containing L molecular sieve, and the normal alkane is preferably C6-C8 normal alkane.

[0042] The method for loading platinum on the n-alkane aromatization catalyst preferably adopts an impregnation method, that is, the molecular sieve of the present invention is impregnated with a solution containing a platinum compound, and the liquid / solid mass ratio during impregnation is preferably 1.0 to 6:1, and the solid obtained after impregnation is dried and roasted to obtain the catalyst. The platinum-containing compound is preferably chloroplatinic acid, chloroplatinic acid amine, dichlorotetraammineplatinum or dinitrodiaminoplatinum. The drying temperature is preferably 80 to 130°C, the time is preferably 8 to 14 hours, and the roasting temperature is preferably 300 to 500°C, and the time is preferably 2 to 10 hours.

[0043] The present invention also provides an alkane aromatization method, comprising contacting normal alkane with the catalyst of the present invention under hydrogen conditions of 450-520°C and 0.3-1.0 MPa, wherein the normal alkane is preferably C6-C8 normal alkane, the hydrogen / hydrocarbon molar ratio is preferably 0.3-4, and the mass space velocity of the contact reaction between the normal alkane and the catalyst is preferably 0.1-20 h -1 , more preferably 0.5-5h -1 .

[0044] The catalyst needs to be reduced before contacting the crude oil. The reduction step preferably uses hydrogen as the reducing gas. The reduction temperature is preferably 350-550°C, more preferably 400-500°C. The volume ratio of hydrogen to catalyst during reduction is preferably 300-1000, more preferably 400-800. The reduction time is preferably 2-6 hours.

[0045] The present invention is further described below by way of examples, but the present invention is not limited thereto.

[0046] In the example, the crystal phase and relative crystallinity of the synthesized barium-containing L molecular sieve were analyzed by X-ray powder diffraction, and the analysis conditions were: Cu target, Kα radiation, Ni filter, tube voltage 45kV, tube current 250mA, scanning range 0.5°-50°, step width 0.02°.

[0047] The relative crystallinity calculation method is: calculate the sum of the peak areas of the characteristic peaks with 2θ angles of 14.7, 19.3, 22.6, 24.3, 25.5, 28.0, 29.0, and 30.6 in the XRD spectrum of the tested molecular sieve, recorded as A, and the sum of the areas of the above characteristic peaks in the XRD spectrum of the standard sample, recorded as B, and the ratio of A to B is the relative crystallinity of the tested L molecular sieve. The standard sample used is the L molecular sieve prepared in Comparative Example 1.

[0048] The chemical composition of the molecular sieves was determined by X-ray fluorescence spectroscopy.

[0049] The morphology index R was calculated based on the measurements of scanning electron microscopy and laser particle size analyzer.

[0050] SiO2 utilization rate = ((the mass of SiO2 in the synthetic molecular sieve feed - the mass of SiO2 in the mother liquor) ÷ the mass of SiO2 in the synthetic molecular sieve feed) × 100%.

[0051] KOH utilization rate = ((mass of KOH in the synthetic molecular sieve feed - mass of KOH in the mother liquor) ÷ mass of KOH in the synthetic molecular sieve feed) × 100%.

[0052] The concentrations of SiO2 and K2O in the mother liquor were tested by inductively coupled plasma optical emission spectrometry.

[0053] Example 1

[0054] 30gAl(OH)3 (purity of 97.55% by mass, the same below) and 120gKOH (produced by Changling Branch of Sinopec Catalyst Co., Ltd., purity of 93.30% by mass, the same below) were dissolved in 200mL of deionized water, and heated to dissolve to obtain aluminum sol. 2gBa(OH)2 (purity of 96.00% by mass, the same below) was dissolved in 160mL of deionized water, and then mixed with the aluminum sol to form a mixed solution. The mixed solution was added to 916g of silica sol (SiO2 concentration of 24.6% by mass, the same below) with stirring, and stirred for 0.5 hour to obtain a first feed mixture gel, wherein the molar ratio of each substance is 0.06BaO:5.3K2O:Al2O3:20SiO2:320H2O. Separately, 60 g of Al(OH) 3 and 60.9 g of KOH were dissolved in 63 mL of deionized water and heated to dissolve to obtain a feed aluminum sol, wherein the molar ratio of each substance was 1.35 K2O:Al2O3:12H2O.

[0055] The above-mentioned first batch mixture gel was transferred into a reactor for hydrothermal crystallization reaction at 170°C for 24 hours, and then the supplementary aluminum sol was added to the reactor to obtain the total gel of the reaction system, wherein the molar ratio of each substance was 0.02BaO:2.7K2O:Al2O3:7SiO2:115H2O, and the molar ratio of aluminum contained in the supplementary aluminum sol to aluminum contained in the first batch mixture gel (referred to as the supplementary aluminum: first aluminum molar ratio) was 2. After the supplementary feeding, the hydrothermal crystallization was continued at 170°C for 48 hours, and then cooled to 40°C. The product was separated from the solid to obtain a solid and a mother liquor. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 120°C for 10 hours to obtain a barium-containing L molecular sieve BaL-1, whose chemical composition (in terms of oxide molar ratio, the same below) was 0.05BaO:0.96K2O:Al2O3:5.90SiO2, and the X-ray powder diffraction spectrum was shown in Figure 2 , scanning electron microscope photos see Figure 3 The relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0056] Example 2

[0057] The barium-containing L molecular sieve was prepared according to the method of Example 1, except that the first feed mixture sol was subjected to hydrothermal crystallization reaction for 48 hours and then the feed aluminum sol was added to obtain the barium-containing L molecular sieve BaL-2, whose chemical composition was 0.05BaO:1.01K2O:Al2O3:5.82SiO2, and the X-ray powder diffraction spectrum was shown in Figure 2, scanning electron microscope photos see Figure 4 The relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0058] Example 3

[0059] The barium-containing L molecular sieve was prepared according to the method of Example 1, except that 3.05 g of Ba(NO3)2 was used instead of Ba(OH)2 to obtain the barium-containing L molecular sieve BaL-3, whose chemical composition is 0.06BaO:0.94K2O:Al2O3:5.86SiO2. Its relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0060] Example 4

[0061] The barium-containing L molecular sieve was prepared according to the method of Example 1, except that 54 g Al(OH)3 and 60.9 g KOH were dissolved in 100 mL deionized water and heated to dissolve to obtain a feed aluminum sol, wherein the molar ratio of each substance was 1.50 K2O:Al2O3:20H2O. After the first feed mixture gel was hydrothermally crystallized for 48 hours, the supplementary aluminum sol was added and the hydrothermal crystallization was continued for 48 hours. The molar ratio of supplementary aluminum: first aluminum was 1.8. The molar ratio of each substance in the total gel of the reaction system was 0.02BaO:2.9K2O:Al2O3:7SiO2:127H2O. The barium-containing L molecular sieve BaL-4 was obtained by reaction. Its chemical composition was 0.04BaO:0.93K2O:Al2O3:5.78SiO. Its relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grains are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0062] Example 5

[0063] The barium-containing L molecular sieve was prepared according to the method of Example 1, except that 60gAl(OH)3 and 50gKOH were dissolved in 25mL deionized water and heated to dissolve to obtain a feed aluminum sol, wherein the molar ratio of each substance was 1.11K2O:Al2O3:7H2O, the hydrothermal crystallization temperature of the first feed mixture gel was 150°C, the molar ratio of feed aluminum: first aluminum was 2, the molar ratio of each substance in the total gel of the reaction system was 0.02BaO:2.5K2O:Al2O3:7SiO2:111H2O, and hydrothermal crystallization was continued at 150°C for 24 hours after feeding. The barium-containing L molecular sieve BaL-5 was obtained, whose chemical composition was 0.04BaO:0.92K2O:Al2O3:5.75SiO2. The relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with a morphology index R of 0.1 to 0.5 to the total grains are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0064] Example 6

[0065] Dissolve 30gAl(OH)3 and 150gKOH in 100mL deionized water, heat and dissolve to obtain aluminum sol, dissolve 4gBa(OH)2 in 80mL deionized water, and mix with aluminum sol to form a mixed solution, add the mixed solution to 1.15kg silica sol under stirring, and stir for 0.5 hours to form the first feed mixture gel, wherein the molar ratio of each substance is 0.12BaO:6.6K2O:Al2O3:25SiO2:320H2O. Dissolve 45gAl(OH)3 and 50.8gKOH in 45mL deionized water, heat and dissolve to obtain a supplementary aluminum sol, wherein the molar ratio of each substance is 1.5K2O:Al2O3:12H2O.

[0066] The first feed mixture gel was transferred into the reactor for hydrothermal crystallization reaction at 170°C for 24 hours, and then the feed aluminum sol was added for the first feed. After the feed, the hydrothermal crystallization was continued at 170°C for 24 hours, and the feed aluminum sol was added again for the second feed, and then the hydrothermal crystallization was continued at 170°C for 48 hours. The molar ratio of aluminum in the second feed aluminum sol: aluminum in the first feed aluminum sol: aluminum in the first feed mixture gel is 1.5:1.5:1, and the molar ratio of each substance in the total gel of the reaction system is 0.03BaO:2.8K2O:Al2O3:6SiO2:90H2O. The product after hydrothermal crystallization after the second supplement of aluminum sol was cooled to 40°C, and the product was separated into solid and mother liquor by solid-liquid separation. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 110°C for 8 hours to obtain barium-containing L molecular sieve BaL-6, whose chemical composition was 0.08BaO:1.22K2O:Al2O3::5.52SiO2. Its relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with a morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0067] Example 7

[0068] Dissolve 30gAl(OH)3 and 67.7gKOH in 300mL deionized water, heat and dissolve to obtain aluminum sol, dissolve 3.3gBa(OH)2 in 243mL deionized water, mix with aluminum sol to form a mixed solution, add the mixed solution to 687g silica sol under stirring, stir for 0.5 hours to form the first feed mixture gel, wherein the molar ratio of each substance is 0.1BaO:3K2O:Al2O3:15SiO2:320H2O. Dissolve 22.5gAl(OH)3 and 22.8gKOH in 23mL water, heat and dissolve to obtain a supplementary aluminum sol, wherein the molar ratio of each substance is 1.35K2O:Al2O3:12H2O.

[0069] The above-mentioned first feed mixture gel was transferred into the reactor for hydrothermal crystallization reaction at 180°C for 24 hours, and then the feed aluminum sol was added for the first feed. After the feed, the hydrothermal crystallization was continued at 180°C for 24 hours, and the feed aluminum sol was added again for the second feed, and then the hydrothermal crystallization was continued at 180°C for 48 hours. The molar ratio of aluminum in the second feed aluminum sol: aluminum in the first feed aluminum sol: aluminum in the first feed aluminum sol is 0.75:0.75:1, and the molar ratio of each substance in the total gel of the reaction system is 0.04BaO:2.0K2O:Al2O3:6SiO2:136H2O. The product after hydrothermal crystallization after the second supplement of aluminum sol was cooled to 40°C, and the product was separated into solid and mother liquor by solid-liquid separation. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 80°C for 4 hours to obtain barium-containing L molecular sieve BaL-7, whose chemical composition was 0.09BaO:0.93K2O:Al2O3:5.88SiO2. Its relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with a morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0070] Example 8

[0071] 30gAl(OH)3 and 120gKOH were dissolved in 250mL deionized water, heated and dissolved to obtain aluminum sol, 2gBa(OH)2 was dissolved in 110mL deionized water, and then mixed with aluminum sol to form a mixed solution, and the mixed solution was added to 916kg silica sol under stirring, and stirred for 0.5 hours to form a first feed reaction mixture gel, wherein the molar ratio of each substance is: 0.06BaO:5.3K2O:Al2O3:20SiO2:320H2O. 21gAl(OH)3 and 21.3gKOH were dissolved in 22mL deionized water and heated to dissolve to obtain a supplementary aluminum sol, wherein the molar ratio of each substance is 1.35K2O:Al2O3:12H2O.

[0072] After the first batch of mixed gel was transferred into the reactor for hydrothermal crystallization reaction at 170°C for 24 hours, the aluminum sol was added for the first batch of feeding, and the hydrothermal crystallization was continued at 170°C for 24 hours. The aluminum sol was added again for the second batch of feeding, and then the hydrothermal crystallization was continued at 170°C for 24 hours. The aluminum sol was added again for the third batch of feeding, and then the hydrothermal crystallization was continued at 170°C for 48 hours. The molar ratio of aluminum in the aluminum sol of the third batch of feeding: aluminum in the aluminum sol of the second batch of feeding: aluminum in the aluminum sol of the first batch of feeding: aluminum in the aluminum sol of the first batch of feeding is 0.7:0.7:0.7:1, and the molar ratio of each substance in the total gel of the reaction system is 0.02BaO:2.6K2O:Al2O3:6SiO2:112H2O. The product after the hydrothermal crystallization after the second aluminum sol is supplemented is cooled to 40°C, and the product is separated into solid and mother liquor by solid-liquid separation. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 80°C for 4 hours to obtain barium-containing L molecular sieve BaL-8, whose chemical composition was 0.04BaO:1.07K2O:Al2O3:6.21SiO2. Its relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with a morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0073] Comparative Example 1

[0074] Preparation of Si-Al L Molecular Sieve

[0075] Dissolve 60gAl(OH)3 and 125gKOH in 365mL deionized water, heat and dissolve to obtain aluminum sol, add the aluminum sol to 916g silica sol with stirring, stir for 0.5 hours to obtain a mixture gel, wherein the molar ratio of each substance is 2.75K2O:Al2O3:10SiO2:162H2O. Move the above mixture gel into a reactor and perform hydrothermal crystallization reaction at 170°C for 72 hours, then cool to 40°C, and separate the product into solid and mother liquor through solid-liquid separation. Wash the solid with deionized water until the pH value of the washing liquid is 8, and then dry at 120°C for 10 hours to obtain silica-alumina L molecular sieve L-1, whose chemical composition is 1.03K2O:Al2O3:5.96SiO2, and the X-ray powder diffraction spectrum is shown in Figure 2 The relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0076] Comparative Example 2

[0077] According to the molar ratio of each substance in the first feed of the present invention, the barium-containing L molecular sieve is prepared

[0078] Dissolve 60gAl(OH)3 and 240gKOH in 500mL deionized water, heat and dissolve to obtain aluminum sol, dissolve 4gBa(OH)2 in 220mL deionized water, and mix with aluminum sol to form a mixed solution, add the mixed solution into 1.83kg silica sol with stirring, and stir for 0.5 hour to obtain a mixture gel, in which the molar ratio of each substance is 0.06BaO:5.3K2O:Al2O3:20SiO2:320H2O.

[0079] The mixture gel was transferred into a reactor, hydrothermally crystallized at 170°C for 72 hours, and then cooled to 40°C. The product was separated into solid and mother liquor by solid-liquid separation. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 120°C for 10 hours to obtain the barium-containing L molecular sieve BaL-A, whose chemical composition was 0.05BaO:0.93K2O:Al2O3:5.81SiO2, and the X-ray powder diffraction spectrum was shown in Figure 2 , scanning electron microscope photos see Figure 5 The relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1. The mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0080] Comparative Example 3

[0081] Preparation of L molecular sieve with low barium content according to the method of US5491119

[0082] Dissolve 60gAl(OH)3 and 240gKOH in 500mL deionized water, heat and dissolve to obtain aluminum sol, dissolve 0.4gBa(OH)2 in 220mL deionized water, and mix with aluminum sol to form a mixed solution, add the mixed solution into 1.83kg silica sol with stirring, and stir for 0.5 hour to obtain a mixture gel, in which the molar ratio of each substance is 0.006BaO:5.3K2O:Al2O3:20SiO2:320H2O.

[0083] The mixture gel was transferred into a reactor, hydrothermally crystallized at 170°C for 72 hours, and then cooled to 40°C. The product was separated into solid and mother liquor by solid-liquid separation. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 120°C for 10 hours to obtain the barium-containing L molecular sieve BaL-B, whose chemical composition was 0.01BaO:0.95K2O:Al2O3:5.76SiO2, relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1, and the mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0084] Comparative Example 4

[0085] Preparation of L molecular sieve with high barium content

[0086] Dissolve 45gAl(OH)3 and 40gKOH in 900mL deionized water, heat and dissolve to obtain aluminum sol, add the mixed solution to 360g silica sol under stirring, and stir for 0.5 hours to obtain a mixture sol. Dissolve 30gBa(OH)2 in a mixed solvent formed by 34g ethanol and 350mL deionized water to prepare a barium source solution. Slowly add the barium source solution dropwise into the sol and continue stirring until a barium-containing mixture gel is formed, wherein the molar ratio of each substance is 0.60BaO:1.2K2O:Al2O3:5SiO2:304H2O.

[0087] The barium-containing mixture gel was transferred into a reactor, hydrothermally crystallized at 130°C for 20 hours, and then cooled to 40°C. The product was separated into solid and mother liquor by solid-liquid separation. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 120°C for 10 hours to obtain a barium-containing L molecular sieve BaL-C, whose chemical composition was 0.35BaO:0.82K2O:Al2O3:5.02SiO2, relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1, and the mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0088] Comparative Example 5

[0089] Preparation of Barium-containing L Molecular Sieve by Multiple Crystallization

[0090] Dissolve 90gAl(OH)3 and 180gKOH in 200mL deionized water, heat and dissolve to obtain aluminum sol, dissolve 2gBa(OH)2 in 223mL deionized water, and mix with aluminum sol to form a mixed solution, add the mixed solution into 916g silica sol (silica sol concentration 24.6%) with stirring, and stir for 0.5 hour to form a mixture gel, in which the molar ratio of each substance is 0.02BaO:2.7K2O:Al2O3:7SiO2:115H2O.

[0091] The mixture gel was transferred into a reactor, and static hydrothermal crystallization was carried out at 170°C for 24 hours, stirred for 1 hour, and then static hydrothermal crystallization was carried out for 48 hours at this temperature, and then cooled to 40°C. The product was separated into solid and mother liquor by solid-liquid separation. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 120°C for 10 hours to obtain barium-containing L molecular sieve BaL-D-1, whose chemical composition was 0.02BaO:0.93K2O:Al2O3:5.35SiO2, relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total amount of grains are shown in Table 1, and the mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0092] Comparative Example 6

[0093] Preparation of Barium-containing L Molecular Sieve by Multiple Crystallization

[0094] Dissolve 90gAl(OH)3 and 127gKOH in 200mL deionized water, heat and dissolve to obtain aluminum sol, dissolve 2gBa(OH)2 in 255mL deionized water, and mix with aluminum sol to form a mixed solution, add the mixed solution into 916g silica sol with stirring, and stir for 0.5 hour to obtain a mixture gel, in which the molar ratio of each substance is 0.02BaO:1.9K2O:Al2O3:7SiO2:127H2O.

[0095] The mixture gel was transferred into a reactor, and hydrothermal crystallization was carried out at 120°C for 48 hours, stirred for 1 hour, and then static hydrothermal crystallization was carried out for 24 hours at the same temperature, stirred for 1 hour, and static hydrothermal crystallization was carried out for 3 times for 24 hours, and then cooled to 40°C. The product was separated into solid and mother liquor by solid-liquid separation. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 100°C for 12 hours to obtain barium-containing L molecular sieve BaL-D-8, whose chemical composition was 0.02BaO:0.90K2O:Al2O3:5.51SiO2, relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1, and the mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0096] Comparative Example 7

[0097] Preparation of barium-containing L molecular sieve according to the molar ratio of each substance in the total gel of the reaction system of the present invention

[0098] Dissolve 90gAl(OH)3 and 180gKOH in 300mL deionized water, heat and dissolve to obtain aluminum sol, dissolve 2gBa(OH)2 in 123mL deionized water, and mix with aluminum sol to form a mixed solution, add the mixed solution into 916g silica sol with stirring, and stir for 0.5 hour to obtain a mixture gel, in which the molar ratio of each substance is 0.02BaO:2.7K2O:Al2O3:7SiO2:115H2O.

[0099] The gel was transferred into a reactor, hydrothermally crystallized at 170°C for 72 hours, then cooled to 40°C, and the product was separated into solid and mother liquor by solid-liquid separation. The solid was washed with deionized water until the pH value of the washing liquid was 8, and then dried at 120°C for 10 hours to obtain barium-containing L molecular sieve BaL-E, whose chemical composition was 0.06BaO:0.91K2O:Al2O3:5.90SiO2, and its relative crystallinity, average grain diameter, average grain length / diameter ratio, and the ratio of grains with morphology index R of 0.1 to 0.5 to the total grain amount are shown in Table 1, and the mother liquor volume, mother liquor SiO2 concentration, mother liquor K2O concentration, raw material SiO2 utilization rate, and raw material KOH utilization rate are shown in Table 2. No residual Al element was detected in the mother liquor.

[0100] As can be seen from Table 1, the barium-free L molecular sieve prepared by the method of Comparative Example 1 has a larger average grain diameter and average grain length / diameter ratio than the barium-containing L molecular sieve prepared by the method of the present invention, and the percentage of grains with R of 0.1 to 0.5 in the total grain amount is lower, and the relative crystallinity is basically the same. The barium-containing L molecular sieves prepared by Comparative Examples 2 to 7 have a lower relative crystallinity and a percentage of grains with R of 0.1 to 0.5 in the total grain amount than the barium-containing L molecular sieve prepared by the method of the present invention.

[0101] As can be seen from Table 2, the utilization rates of the raw materials SiO2 and KOH for preparing the barium-containing L molecular sieve by the method of the present invention are higher than those of the comparative example.

[0102] Table 1

[0103]

[0104] Table 2

[0105]

[0106] Examples 9-16

[0107] Examples 9 to 16 are used to evaluate the aromatization selectivity and activity stability of the barium-containing L molecular sieve prepared by the method of the present invention.

[0108] 5 g of the barium-containing L molecular sieve prepared in Examples 1 to 8 were taken as carriers and impregnated with a Pt(NH3)2Cl2 solution with a concentration of 16 mg / mL, and the liquid / solid mass ratio during impregnation was 1.5. After impregnation, the solid was dried at 120°C for 12 hours and calcined at 350°C for 4 hours to prepare a catalyst with a Pt content of 1.0% by mass based on the carrier. The catalyst numbers prepared in each example and the molecular sieve carrier numbers used are shown in Table 3.

[0109] 2 mL of catalyst was loaded on the high-pressure microreactor, and aromatization reaction was carried out with n-hexane and n-octane as raw materials. The catalyst was reduced before the reaction, the reducing atmosphere was hydrogen, the reduction temperature was 480°C, the reduction time was 4 hours, and the volume ratio of hydrogen introduced per hour to the catalyst was 600:1. The aromatization reaction temperature was 480°C, the pressure was 0.7 MPa, and the feed mass space velocity was 3 h -1 , the hydrogen / hydrocarbon molar ratio is 0.86, the aromatization product of n-hexane is benzene, and the aromatization product of n-octane is C6-C8 aromatic hydrocarbons. The results of the reaction for 1h and 60h are shown in Table 3.

[0110] Comparative Examples 8 to 14

[0111] Comparative Examples 8 to 14 are used to evaluate the aromatization selectivity and activity stability of the molecular sieves prepared in the comparative examples.

[0112] Take 5g of L molecular sieve prepared in Comparative Examples 1 to 7 as carriers, and impregnate them with a Pt(NH3)2Cl2 solution with a concentration of 16mg / mL. The liquid / solid mass ratio during impregnation is 1.5. After impregnation, the solid is dried at 120°C for 12 hours and calcined at 350°C for 4 hours to prepare a catalyst with a Pt content of 1.0% by mass based on the carrier. The catalyst numbers prepared in each comparative example and the molecular sieve carrier numbers used are shown in Table 3.

[0113] 2 mL of catalyst was loaded on the high-pressure microreactor, and aromatization reaction was carried out with n-hexane and n-octane as raw materials. The catalyst was reduced before the reaction, the reducing atmosphere was hydrogen, the reduction temperature was 480°C, the reduction time was 4 hours, and the volume ratio of hydrogen introduced per hour to the catalyst was 600:1. The aromatization reaction temperature was 480°C, the pressure was 0.7 MPa, and the feed mass space velocity was 3 h -1 , hydrogen / hydrocarbon molar ratio 0.86, the product of n-hexane aromatization reaction is benzene, and the product of n-octane aromatization reaction is C6-C8 aromatic hydrocarbons. The results of reaction for 1h and 60h are shown in Table 3.

[0114] Table 3

[0115]

[0116] As can be seen from Table 3, the flaky barium-containing L molecular sieve prepared by the method of the present invention has a higher yield of benzene or C6-C8 aromatics than the L molecular sieve prepared in the comparative example, indicating that it has good aromatization selectivity, and after 60 hours of reaction, the yield of benzene or C6-C8 aromatics does not decrease much, indicating that the catalyst activity does not decrease much and has good activity stability.

Claims

1. A barium-containing L molecular sieve having a molar ratio of (0.03-0.1)BaO:(0.9-1.3)M 2 O:Al 2 O 3 :(5~8)SiO 2 The chemical composition of the L molecular sieve is as follows: wherein M is K or / and Na, the average crystal grain diameter of the L molecular sieve is 0.10-0.35 μm, the average crystal grain length / diameter ratio is 0.20-0.50, and the crystal grains with a morphology index R of 0.1-0.5 account for more than 91% by mass of the total crystal grains. The preparation method of the barium-containing L molecular sieve comprises the following steps: (1) mixing a barium source, an aluminum source, a silicon source, an inorganic base and water to prepare a first feed mixture gel, wherein the molar ratio of each substance in the first feed mixture gel is (0.06-0.3)BaO:(2.5-8)M 2 O:Al 2 O 3 :(13~40)SiO 2 :(200~400)H 2 O, M is K or / and Na, the first batch of mixed gel is subjected to hydrothermal crystallization reaction, (2) mixing an aluminum source, an inorganic base and water to prepare a feed aluminum sol, wherein the molar ratio of each substance in the feed aluminum sol is (0.5-2.0) M 2 O:Al 2 O 3 :(5~25)H 2 O, M is K or / and Na, and the supplementary aluminum sol is added to the material obtained after the hydrothermal crystallization of the first feed mixture gel described in step (1) to obtain a total gel of the reaction system, wherein the molar ratio of each substance in the total gel of the reaction system is (0.01-0.05)BaO:(1.5-3.0)M 2 O:Al 2 O 3 :(5~9)SiO 2 :(80~150)H 2 O, continue the hydrothermal crystallization reaction, separate the product after the hydrothermal crystallization into solid and liquid to obtain a solid and a mother liquor, and wash and dry the obtained solid to obtain a barium-containing L molecular sieve.

2. The barium-containing L molecular sieve according to claim 1, Features Its chemical composition is calculated by oxide molar ratio: (0.03-0.09)BaO: (0.9-1.3)M 2 O:Al 2 O 3 :(5.5~7)SiO 2 .

3. The barium-containing L molecular sieve according to claim 1, Features The average crystal diameter of the L molecular sieve is 0.20-0.30 μm.

4. The barium-containing L molecular sieve according to claim 1, Features The average grain length / diameter ratio is 0.22 to 0.

40.

5. The barium-containing L molecular sieve according to claim 1, Features The crystal grains having a morphology index R of 0.1 to 0.5 account for 92 to 98 mass % of the total crystal grains.

6. The barium-containing L molecular sieve according to claim 1, Features The relative crystallinity of the L molecular sieve is greater than 95%.

7. The barium-containing L molecular sieve according to claim 1, Features The molar ratio of the aluminum in the aluminum sol in the step (2) to the aluminum in the first feeding mixture gel in the step (1) is 1 to 3.

8. The barium-containing L molecular sieve according to claim 1, Features In the step (1), the temperature of the first feed mixture gel for hydrothermal crystallization reaction is 100-200° C. and the time is 15-60 hours.

9. The barium-containing L molecular sieve according to claim 1, Features In the step (2), after adding the aluminum sol as feed, the temperature for the hydrothermal crystallization reaction is 100 to 200° C. and the time is 15 to 60 hours.

10. The barium-containing L molecular sieve according to claim 1, Features In the step (2), the supplementary aluminum sol is added to the material obtained after the hydrothermal crystallization of the first feed mixture gel in the step (1) in multiple times, and the hydrothermal crystallization reaction is carried out after each addition of the supplementary aluminum sol. After the last addition of the supplementary aluminum sol, the total gel of the reaction system is obtained. The molar ratio of each substance in the total gel of the reaction system is (0.01-0.05)BaO:(1.5-3.0)M 2 O:Al 2 O 3 :(5~9)SiO 2 :(80~150)H 2 O, the product after the last hydrothermal crystallization reaction is subjected to solid-liquid separation to obtain a solid and a mother liquor, and the obtained solid is washed and dried to obtain a barium-containing L molecular sieve.

11. The barium-containing L molecular sieve according to claim 10, Features The supplementary aluminum sol is added two to three times into the material obtained after hydrothermal crystallization of the first feed mixture gel described in step (1).

12. The barium-containing L molecular sieve according to claim 11, Features The supplementary aluminum sol is added twice to the material obtained after hydrothermal crystallization of the first feed mixture gel described in step (1), and the molar ratio of aluminum in the second feed aluminum sol: aluminum in the first feed aluminum sol: aluminum in the first feed mixture gel is 0.5-2.5:0.5-2.5:

1.

13. The barium-containing L molecular sieve according to claim 11, Features The supplementary aluminum sol is added three times to the material obtained after hydrothermal crystallization of the first feed mixture gel described in step (1), and the molar ratio of aluminum in the third supplementary aluminum sol: aluminum in the second supplementary aluminum sol: aluminum in the first supplementary aluminum sol: aluminum in the first feed mixture gel is 0.5-2:0.5-2:0.5-2:

1.

14. The barium-containing L molecular sieve according to claim 10, Features The temperature of the hydrothermal crystallization reaction after adding the aluminum sol each time is 100 to 200° C. and the time is 15 to 60 hours.

15. The barium-containing L molecular sieve according to claim 1, Features The barium source is selected from barium hydroxide and / or barium nitrate, the aluminum source is selected from aluminum hydroxide and / or sodium metaaluminate, and the silicon source is selected from SiO 2 The silica sol has a content of 20 to 45% by mass, and the inorganic base is selected from potassium hydroxide and / or sodium hydroxide.

16. A catalyst for aromatization of normal alkanes, comprising the barium-containing L molecular sieve according to claim 1 and platinum supported thereon, wherein the platinum content is 0.4-1.5% by mass calculated based on the barium-containing L molecular sieve.

17. A method for aromatizing normal alkane, comprising contacting normal alkane with the catalyst according to claim 16 under hydrogen conditions of 450-520°C and 0.3-1.0 MPa.

18. The method according to claim 17, wherein the normal alkane is a C6-C8 normal alkane, the hydrogen / hydrocarbon molar ratio is 0.3-4, and the mass space velocity of the normal alkane and the catalyst in the contact reaction is 0.1-20h -1 .