Glass material

By optimizing the composition of glass materials, reducing high-temperature viscosity and improving chemical stability, the problems of high viscosity and high transmittance in the prior art black glass materials at high temperatures are solved, and low transmittance in the visible to near-infrared band are achieved and high-precision inspection requirements, suitable for bio-testing and platinum ware production.

CN116332503BActive Publication Date: 2024-11-26CDGM OPTICAL GLASS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310408037.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-11-26
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

The existing black glass materials are too viscous at high temperatures, making it difficult to obtain high uniformity, and have high transmittance in visible to near infrared bands, which cannot meet the needs of all black backgrounds, especially in biological detection, which is insufficient acid and water resistance, affecting fluorescence. Detection accuracy.

Method used

A glass material was designed, with the composition mainly composed of SiO2, B2O3, Al2O3, ZnO, Na2O, etc., containing transition metal oxides such as MnO2+V2O3+Fe2O3+CuO+CeO2+NiO+Co2O3+Cr2O3 and other transition metal oxides through reasonable components The proportional optimization reduces the high temperature viscosity of the glass and improves chemical stability, ensuring low transmittance in the visible to near infrared bands.

Benefits of technology

It achieves low transmittance in the visible light to near infrared band, has excellent chemical stability and low high temperature viscosity, and is suitable for high-precision biological detection and platinum vessel production, improving detection accuracy and the acid and water resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004182225970000131
    Figure BDA0004182225970000131
  • Figure BDA0004182225970000141
    Figure BDA0004182225970000141
  • Figure BDA0004182225970000142
    Figure BDA0004182225970000142
Patent Text Reader

Abstract

The present invention provides a glass material, wherein the components of the glass material are expressed in weight percentage and contain: SiO2: 40-68%; B2O3: 1-15%; Al2O3: 0.5-8%; ZnO: 5-20%; Na2O: 6-16%; MnO2+V2O3+Fe2O3+CuO+CeO2+NiO+Co2O3+Cr2O3: 1-18%. Through reasonable component design, the glass material obtained by the present invention has a low transmittance in the range of visible light to near infrared band, and has excellent chemical stability and low high temperature viscosity, and is suitable for the production of platinum utensils.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application for the invention patent application with application number 202111272115.2, application date October 29, 2021, and name “Glass Material”. Technical Field

[0002] The invention relates to a glass material, in particular to a high-uniformity glass material with relatively low transmittance in the range of visible light to near-infrared waveband. Background Art

[0003] Molecular diagnosis has the advantages of short detection time, high sensitivity, and strong specificity. In recent years, it has become an important development direction in the field of precision medicine and personalized treatment. Polymerase chain reaction technology (PCR) is a key technology in the field of molecular diagnosis. Its core technology lies in the precise quantitative analysis of the fluorescence generated during the reaction process. For example, in microfluidic gene detection chips, the more accurate the extraction of the fluorescence signal generated by the micro-unit, the higher the detection accuracy of PCR.

[0004] The accuracy of detecting fluorescent signals depends on a highly uniform black background. If the coating technology is used to form black, the light reflected by the film layer will strongly interfere with the fluorescent signal. Therefore, the black background material is required to evenly absorb the external light. In addition, the black background material is also required to have excellent acid and water resistance, especially with the development of array chips for biological detection in recent years. If the material has poor acid and water resistance, the substances in the material will be corroded and precipitated by the culture medium, especially the precipitation of alkali metal ions and transition metal ions will interfere with the fluorescence of the active substance, thereby reducing the accuracy of fluorescence detection.

[0005] In the prior art, black glass usually uses refractory materials as melting vessels. If the high-temperature viscosity is too large, a highly homogeneous product cannot be obtained and a highly uniform black background cannot be achieved. At the same time, the transmittance is high in certain bands and cannot meet the requirements of a completely black background. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a glass material with low high-temperature viscosity, excellent chemical stability and low transmittance in the visible light to near-infrared band.

[0007] The technical solution adopted by the present invention to solve the technical problem is:

[0008] (1) Glass material, whose components, expressed in weight percentage, contain: SiO2: 40-70%; B2O3: 1-15%; Al2O3: 0.5-8%; ZnO: 5-20%; Na2O: 6-16%; MnO2+V2O3+Fe2O3+CuO+CeO2+NiO+Co2O3+Cr2O3: 1-18%.

[0009] (2) The glass material according to (1), wherein the components, expressed in weight percentage, further contain: TiO2: 0-6%; and / or P2O5: 0-2%; and / or ZrO2: 0-8%; and / or Ln2O3: 0-10%; and / or Li2O: 0-5%; and / or K2O: 0-8%; and / or RO: 0-10%; and / or a clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3, and the clarifier is one or more of Sb2O3, SnO2, Na2SiF6, and K2SiF6.

[0010] (3) Glass material, whose components include SiO2, B2O3, ZnO and alkali metal oxides. The components, expressed in weight percentage, include MnO2+V2O3+Fe2O3+CuO+CeO2+NiO+Co2O3+Cr2O3: 1-18%. The light transmittance of glass material below 2 mm at 300-800 nm is less than 2%.

[0011] (4) The glass material according to (3), wherein the components thereof are expressed in weight percentage as follows: SiO2: 40-70%; and / or B2O3: 1-15%; and / or Al2O3: 0.5-8%; and / or ZnO: 5-20%; and / or Na2O: 6-16%; and / or TiO2: 0-6%; and / or P2O5: 0-2%; and / or ZrO2: 0-8%; and / or Ln2O3: 0 ~10%; and / or Li2O: 0~5%; and / or K2O: 0~8%; and / or RO: 0~10%; and / or clarifier: 0~1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3, and the clarifier is one or more of Sb2O3, SnO2, Na2SiF6, and K2SiF6.

[0012] (5) The glass material according to any one of (1) to (4), wherein the composition is expressed in weight percentage, wherein: (B2O3+Al2O3) / SiO2 is less than 0.3, preferably (B2O3+Al2O3) / SiO2 is less than 0.25, and more preferably (B2O3+Al2O3) / SiO2 is 0.05 to 0.2.

[0013] (6) The glass material according to any one of (1) to (4), wherein the composition is expressed in weight percentage, wherein: K2O / (Na2O+Li2O) is 0.03 to 1.0, preferably K2O / (Na2O+Li2O) is 0.05 to 0.8, and more preferably K2O / (Na2O+Li2O) is 0.1 to 0.5.

[0014] (7) The glass material according to any one of (1) to (4), wherein the composition is expressed in weight percentage, wherein: ZnO / SiO2 is 0.08 to 0.45, preferably ZnO / SiO2 is 0.1 to 0.4, and more preferably ZnO / SiO2 is 0.12 to 0.3.

[0015] (8) The glass material according to any one of (1) to (4), wherein the composition is expressed in weight percentage, wherein: TiO2 / (Fe2O3+CeO2) is 0.2 to 6.0, preferably TiO2 / (Fe2O3+CeO2) is 0.3 to 4.0, and more preferably TiO2 / (Fe2O3+CeO2) is 0.4 to 2.0.

[0016] (9) A glass material according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: Na2O+K2O+Li2O≤25%, preferably Na2O+K2O+Li2O≤23%, more preferably Na2O+K2O+Li2O≤20%; and / or Cr2O3 / (Fe2O3+CuO) is less than 3.0, preferably Cr2O3 / (Fe2O3+CuO) is less than 2.0, more preferably Cr2O3 / (Fe2O3+CuO) is less than 1.0.

[0017] (10) The glass material according to any one of (1) to (4), wherein the components thereof, expressed in weight percentage, comprise: SiO2: 45-68%, preferably SiO2: 47-65%; and / or B2O3: 1-12%, preferably B2O3: 2-10%; and / or MnO2+V2O3+Fe2O3+CuO+CeO2+NiO+Co2O3+Cr2O3: 2-15%, preferably MnO2+V2O3+Fe2O3+CuO+CeO2+NiO+Co2O3+Cr2O3: 3-10%; and / or Al2O3: 0.8-7%, preferably Al2O3: 1-5%; and / or ZnO: 7-16%, preferably ZnO: 8-15%; and / or Na2O: 7-14%, preferably Na2O: 8-13%; and / or TiO2: 0 ~5%, preferably TiO2: 0~4%; and / or P2O5: 0~1%; and / or ZrO2: 0~6%, preferably ZrO2: 0.5~5%; and / or Ln2O3: 0~8%, preferably Ln2O3: 0~4%; and / or Li2O: 0.5~4%, preferably Li2O: 0.7~3%; and / or K2O: 0.5~6%, preferably K2O: 1~6%; and / or RO: 0~8%, preferably RO: 0~6%; and / or clarifier: 0~0.8%, preferably clarifier: 0~0.5%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3, and the clarifier is one or more of Sb2O3, SnO2, Na2SiF6, and K2SiF6.

[0018] (11) The glass material according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: CuO: 0.5-6%, preferably CuO: 1-5%, more preferably CuO: 1.5-4%; and / or Fe2O3: 0-3%, preferably Fe2O3: 0.05-2%, more preferably Fe2O3: 0.1-1.5%; and / or MnO2: 0-3%, preferably MnO2: 0-2%, more preferably MnO2: 0-1%; and / or V2O3: 0-3%, preferably V2O3: 0-2% , more preferably V2O3: 0-1%; and / or CeO2: 0-2%, preferably CeO2: 0-1.5%, more preferably CeO2: 0-1%; and / or NiO: 0.1-5%, preferably NiO: 0.5-4%, more preferably NiO: 0.8-3%; and / or Co2O3: 0.1-5%, preferably Co2O3: 0.5-4%, more preferably Co2O3: 0.8-3%; and / or Cr2O3: 0-4%, preferably Cr2O3: 0-3.5%, more preferably Cr2O3: 0-3%.

[0019] (12) According to any one of the glass materials described in (1) to (4), the light transmittance of the glass material with a diameter of less than 2 mm at 300 to 800 nm is less than 2%, preferably less than 1.5%, more preferably less than 1%, and further preferably less than 0.8%.

[0020] (13) The glass material according to any one of (1) to (4) has an SCI value of 4.0 or less, preferably 3.5 or less, and more preferably 3.0 or less; and / or an SCE value of 5.0 or less, preferably 4.0 or less, and more preferably 3.0 or less; and / or a chromaticity uniformity of 0.7 to 1.3, preferably 0.75 to 1.25, and more preferably 0.8 to 1.2; and / or a water-resistant stability leaching percentage of 0.10% or less, preferably 0.06% or less, and more preferably 0.03% or less; and / or a acid-resistant stability leaching percentage of 0.5% or less, preferably 0.35% or less, and more preferably 0.19% or less; and / or a viscosity of the glass material at 1400° C. of 200 dPas or less, preferably 150 dPas or less, and more preferably 80 dPas or less; and / or a Cr 6+ The content is 1000 ppm or less, preferably 500 ppm or less, more preferably 100 ppm or less, further preferably 50 ppm or less, and further preferably 10 ppm or less.

[0021] (14) A glass preform made of the glass material described in any one of (1) to (13).

[0022] (15) A glass element made of the glass material described in any one of (1) to (13) or the glass preform described in (14).

[0023] (16) An instrument comprising the glass material described in any one of (1) to (13) and / or the glass element described in (15).

[0024] The beneficial effects of the present invention are as follows: through reasonable component design, the glass material obtained by the present invention has a low transmittance in the visible light to near-infrared band, and has excellent chemical stability and low high-temperature viscosity, and is suitable for the production of platinum utensils. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a spectral transmittance curve graph of the glass material of Example 19 of the present invention. DETAILED DESCRIPTION

[0026] The following is a detailed description of the embodiments of the glass material of the present invention. However, the present invention is not limited to the following embodiments and can be implemented with appropriate changes within the scope of the purpose of the present invention. In addition, although there are cases where the description of the repeated description is appropriately omitted, the main purpose of the invention is not limited thereto. In the following content, the glass material of the present invention is sometimes referred to as glass.

[0027] [Glass material]

[0028] The following is an explanation of the range of each component (ingredient) of the glass material of the present invention. In the present invention, unless otherwise specified, the content and total content of each component are all expressed in weight percentage (wt%), that is, the content and total content of each component are expressed in weight percentage relative to the total amount of glass material converted into oxide composition. Here, the "composition converted into oxide" means that when the oxides, composite salts and hydroxides used as raw materials for the glass material components of the present invention decompose and transform into oxides during melting, the total weight of the oxide material is taken as 100%.

[0029] Unless otherwise specified in specific circumstances, the numerical ranges listed in the present invention include upper and lower limits, "above" and "below" include endpoint values, and all integers and fractions included in the range, without being limited to the specific values ​​listed when the range is defined. "And / or" referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.

[0030] SiO2 is the main component of the glass network. If its content exceeds 70%, it is difficult to melt the glass, and it is difficult to eliminate bubbles, inclusions, stripes, etc. It is difficult to obtain a highly uniform black background, that is, excellent chromaticity uniformity. If its content is less than 40%, firstly, the water resistance and acid resistance of the glass are difficult to meet the design requirements, the glass network's confinement to the coloring ions is reduced, and the glass is easy to crystallize during the production process, resulting in white and gray precipitates in the glass, and the chromaticity uniformity is difficult to meet the design requirements. Therefore, the content of SiO2 is 40-70%, preferably 45-68%, and more preferably 47-65%.

[0031] An appropriate amount of B2O3 can strengthen the glass network mainly composed of SiO2, further improve the water resistance and acid resistance of the glass, and at the same time reduce the melting temperature and high temperature viscosity of the glass. For this type of borosilicate glass, the lower the high temperature viscosity, the easier it is to eliminate bubbles, inclusions, stripes, etc. in the glass. If the content of B2O3 is less than 1%, the above effect is not obvious. If the content of B2O3 is higher than 15%, due to the lack of oxygen in the glass system, B2O3 will instead transform into a loose structure, reducing the water resistance and acid resistance of the glass. Therefore, the content of B2O3 is limited to 1-15%, preferably 1-12%, and more preferably 2-10%.

[0032] An appropriate amount of Al2O3 can strengthen the glass network, improve the chemical stability of the glass, reduce the thermal expansion coefficient of the glass, and help reduce the precipitation of coloring ions in the glass. If its content is less than 0.5%, the above effects are not obvious. If the Al2O3 content exceeds 8%, the high-temperature viscosity of the glass rises rapidly, making it difficult to meet the design requirements. Therefore, the content of Al2O3 is limited to 0.5-8%, preferably 0.8-7%, and more preferably 1-5%.

[0033] A small amount of P2O5 in glass can significantly improve the chemical strengthening performance of glass, which is beneficial to improving the strength of glass. However, P2O5 in glass can promote the formation of glass microcrystals, especially when transition metal ions exist in glass. If its content is higher than 2%, the anti-crystallization performance of glass will decrease rapidly. In severe cases, the glass will be full of crystallization particles and crystallization bands, and a uniform black background cannot be formed. Therefore, the content of P2O5 is 0-2%, preferably 0-1%, and more preferably no P2O5.

[0034] An appropriate amount of ZnO can significantly enhance the tightness of the glass network, improve the water resistance and acid resistance of the glass, and reduce the thermal expansion coefficient and transition temperature of the glass. If its content is less than 5%, the above effects are not obvious. If its content is higher than 20%, the Abbe number of the glass decreases, and it is difficult to meet the design requirements. The surface tension of the glass increases during the melting process, bubbles are not easy to discharge, and the bubble degree is difficult to meet the design requirements. Therefore, the content of ZnO is controlled to be 5-20%, preferably 7-16%, and more preferably 8-15%.

[0035] An appropriate amount of TiO2 can form complex coloring with transition metal oxides in glass, enhance light absorption of 300-500nm, thereby reducing the amount of transition metal oxides used and further reducing the precipitation of transition metal oxides. On the other hand, an appropriate amount of TiO2 can enhance the network structure of glass and reduce the precipitation of alkali metal ions. If the content of TiO2 is higher than 6%, the reflectivity of the glass increases sharply, the SCI value is difficult to meet the design requirements, and the stability of the glass is reduced, and the risk of crystallization increases. Therefore, the content of TiO2 is limited to 0-6%, preferably 0-5%, and more preferably 0-4%.

[0036] ZrO2 can reduce the ability of glass solution to corrode the furnace body, increase the life of the furnace, and reduce the precipitation of alkali metal ions and transition metal ions. If its content exceeds 8%, insoluble matter is likely to appear in the glass, the glass's anti-crystallization ability decreases, and the high-temperature viscosity increases rapidly. Therefore, the content of ZrO2 is 0-8%, preferably 0-6%, and more preferably 0.5-5%.

[0037] Ln2O3 (Ln2O3 is one or more of La2O3, Gd2O3, and Y2O3) in glass can significantly improve the strength of glass, reduce the high temperature viscosity of glass, and more easily obtain highly uniform glass. If the content of Ln2O3 exceeds 10%, the SCI value of the glass exceeds the design requirements. Therefore, the content of Ln2O3 is 0 to 10%, preferably 0 to 8%, and more preferably 0 to 4%.

[0038] Li2O, Na2O, and K2O are alkali metal oxides. Their content and relative content have a significant influence on the light absorption curve, high-temperature viscosity, transition temperature, thermal expansion coefficient, water resistance, and weather resistance of the glass.

[0039] From the perspective of the effect of a single alkali metal oxide, Li2O has the strongest ability to reduce the transition temperature and high-temperature viscosity of glass. If its content exceeds 5%, the glass tends to be devitrified and the cost of raw materials rises rapidly. More importantly, if its content exceeds 5%, the acid resistance of the glass decreases rapidly. Therefore, the content of Li2O is limited to 0-5%. In some embodiments, if the content of Li2O is less than 0.5%, the high-temperature viscosity of the glass increases rapidly, and a higher temperature is required to remove bubbles during the melting process, which will cause a significant decrease in the coloring ability of CuO. Therefore, the content of Li2O is preferably 0.5-4%, and more preferably 0.7-3%.

[0040] An appropriate amount of Na2O can improve the melting performance of glass and reduce the high temperature viscosity of glass. If its content is less than 6%, the melting performance, high temperature viscosity and thermal expansion coefficient of glass are difficult to meet the design requirements, and the water resistance and weather resistance of glass decrease rapidly; if its content is higher than 16%, the thermal expansion coefficient of glass increases rapidly, and the water resistance and weather resistance of glass decrease, which is difficult to meet the design requirements. Therefore, the content of Na2O is limited to 6-16%, preferably 7-14%, and more preferably 8-13%.

[0041] An appropriate amount of K2O can form an "alkali neutralization" effect with Na ions and Li ions in the glass, further strengthening the glass network and reducing the precipitation of alkali metal ions and transition metal ions in the solution. If its content is higher than 8%, it will further aggravate the precipitation of alkali metal ions and transition metal ions. Therefore, the content of K2O is limited to 0-8%, preferably 0.5-6%, and more preferably 1-6%.

[0042] Co2O3 is a transition metal oxide, which can significantly reduce the light transmittance of 450-620nm in glass. If its content is less than 0.1%, the transmittance of the glass is higher than the design requirement. If its content is higher than 5%, the anti-crystallization ability of the glass decreases rapidly, the chemical stability of the glass decreases, and the precipitation amount of the glass in the solution increases rapidly. Therefore, the content of Co2O3 is limited to 0.1-5%, preferably 0.5-4%, and more preferably 0.8-3%.

[0043] The inventors have found through a large number of experimental studies that in some embodiments, the coloring ability of Co2O3 is closely related to the glass network former, and when the value of (B2O3+Al2O3) / SiO2 is greater than 0.3, the coloring ability of Co2O3 decreases significantly. Therefore, the value of (B2O3+Al2O3) / SiO2 is preferably 0.3 or less, more preferably 0.25 or less, and further preferably 0.05 to 0.2.

[0044] Alkaline earth metal oxide RO (RO is one or more of MgO, CaO, SrO, BaO) can enhance the stability of glass, reduce the risk of crystallization of glass during the production process, and can also reduce the high temperature viscosity of glass and improve the bubble degree of glass. If the content of RO exceeds 10%, the reflectivity of glass rises rapidly, and the alkaline earth metal oxide exceeding 10% will greatly reduce the acid resistance of glass, and it is easy to produce spots under the erosion of certain electrolyte solutions, thereby reducing the uniformity of black background. Therefore, the content of RO is limited to 0-10%, preferably 0-8%, and more preferably 0-6%. On the other hand, alkaline earth metal oxides will also cause changes in the coloring ability of Co2O3. If the content of RO exceeds 10%, the coloring ability of Co2O3 decreases. The inventors have found that CaO in alkaline earth metal oxides has the least damage to the coloring ability of Co2O3, so it is preferred that CaO is contained in the glass, followed by BaO, and if conditions permit, MgO and / or SrO are considered.

[0045] NiO in glass can significantly reduce the light transmittance of 450-750nm. If its content is less than 0.1%, the light transmittance of the glass is higher than the design requirement. If its content is higher than 5%, the anti-crystallization ability of the glass decreases rapidly, the chemical stability of the glass decreases, and the precipitation amount in the solution increases rapidly. Therefore, the content of NiO is 0.1-5%, preferably 0.5-4%, and more preferably 0.8-3%.

[0046] The inventors have found through a large number of experimental studies that, in some embodiments, when K2O exists in the glass and K2O / (Na2O+Li2O) is between 0.03 and 1.0, preferably between 0.05 and 0.8, and more preferably between 0.1 and 0.5, the absorption capacity of NiO at 450 to 750 nm is greatly enhanced, which can significantly reduce the use of transition metal oxides, thereby reducing the amount of precipitation of glass.

[0047] An appropriate amount of CuO can reduce the light transmittance at 200-450nm and 600-900nm. If its content is less than 0.5%, the light transmittance of the glass is higher than the design requirement. If its content is higher than 6%, the anti-crystallization ability of the glass decreases, and the water resistance and acid resistance decrease. Therefore, the content of CuO is limited to 0.5-6%, preferably 1-5%, and more preferably 1.5-4%.

[0048] The inventors have found through a large number of experimental studies that, in some embodiments, when the value of ZnO / SiO2 is greater than 0.45, the glass needs to be melted at a higher temperature to meet the requirements of bubble degree, and a higher temperature will weaken the coloring ability of CuO. If the value of ZnO / SiO2 is less than 0.08, the chemical stability of the glass decreases, and the ability to confine alkali metal ions and transition metal ions decreases. Therefore, the value of ZnO / SiO2 is preferably 0.08 to 0.45, more preferably 0.1 to 0.4, and further preferably 0.12 to 0.3.

[0049] An appropriate amount of Fe2O3 can reduce the light transmittance of 200-450nm. If its content is higher than 3%, the chemical stability of the glass decreases and the amount of precipitation in acid or aqueous solution increases sharply. Therefore, the content of Fe2O3 is 0-3%, preferably 0.05-2%, and more preferably 0.1-1.5%.

[0050] An appropriate amount of CeO2 can reduce the light transmittance of 200-450nm. If its content is higher than 2%, the glass's ability to resist crystallization decreases sharply, and even crystallization begins above the forming temperature. Therefore, the content of CeO2 is limited to 0-2%, preferably 0-1.5%, and more preferably 0-1%.

[0051] The inventors have found through a large number of experimental studies that when TiO2, CeO2 and Fe2O3 are simultaneously present in the glass, the coloring ability of Fe2O3 and CeO2 in the 200-450nm band is greatly enhanced; further, especially under the conditions of melting in an oxidizing atmosphere, it is preferred that TiO2 / (Fe2O3+CeO2) is between 0.2 and 6.0, more preferably TiO2 / (Fe2O3+CeO2) is between 0.3 and 4.0, and further preferably TiO2 / (Fe2O3+CeO2) is between 0.4 and 2.0, the coloring ability of 200-450nm is significantly enhanced, and under the condition that the light transmittance reaches the design standard, the usage of Fe2O3 and CeO2 can be reduced by more than 50%, which is beneficial to reduce the precipitation of transition metal oxides.

[0052] MnO2 and V2O3 can enhance the coloring of glass in the 200-800nm ​​band, but the coloring ability of MnO2 is sensitive to process conditions. When its content is greater than 3%, the spectrum changes greatly under different process conditions, affecting the consistency of the product. Therefore, the content of MnO2 is limited to less than 3%, preferably less than 2%, and more preferably less than 1%. V2O3 above 3% also has the above problems, and it will also cause the glass to become brittle and make subsequent processing more difficult. Therefore, the content of V2O3 is limited to less than 3%, preferably less than 2%, and more preferably less than 1%.

[0053] Adding an appropriate amount of Cr2O3 to glass can reduce the light transmittance of 300-500nm and 600-740nm. If its content exceeds 4%, Cr2O3 is likely to appear in the glass. 6+ ions, which are strong carcinogens and cannot meet the ROSH requirements. Therefore, the content of Cr2O3 is less than 4%, preferably less than 3.5%, and more preferably less than 3%. In some embodiments, it is further preferred that Cr2O3 is not contained.

[0054] The inventors found that Cr 6+ The probability of occurrence is lower in a reducing atmosphere, but a reducing atmosphere is fatal to metal vessels used in smelting. The inventors have found through a large number of experiments that when Cr2O3 exists in the components, an appropriate amount of alkali metal oxides, Fe2O3, and CuO can prevent the Cr2O3 component from being oxidized to Cr during high-temperature smelting in an oxidizing atmosphere. 6+Further, in some embodiments, when Na2O+K2O+Li2O≤25%, preferably Na2O+K2O+Li2O≤23%, more preferably Na2O+K2O+Li2O≤20%, and the value of Cr2O3 / (Fe2O3+CuO) is 3.0 or less, preferably Cr2O3 / (Fe2O3+CuO) is 2.0 or less, and more preferably Cr2O3 / (Fe2O3+CuO) is 1.0 or less, Cr is not likely to appear in the glass even under oxidizing atmosphere conditions. 6+ .

[0055] In order to obtain a black background, reduce the precipitation of transition metal oxides and improve the anti-crystallization performance of glass, the total content of transition metal oxides such as MnO2, V2O3, Fe2O3, CuO, CeO2, NiO, Co2O3, Cr2O3, etc. MnO2+V2O3+Fe2O3+CuO+CeO2+NiO+Co2O3+Cr2O3 is preferably 1-18%, more preferably MnO2+V2O3+Fe2O3+CuO+CeO2+NiO+Co2O3+Cr2O3 is 2-15%, and further preferably MnO2+V2O3+Fe2O3+CuO+CeO2+NiO+Co2O3+Cr2O3 is 3-10%.

[0056] Sb2O3, SnO2, Na2SiF6, K2SiF6 and the like can be used as clarifiers to improve the defoaming ability of glass. When the above clarifiers are present in total or individually, their content is less than 1%, preferably less than 0.8%, and more preferably less than 0.5%.

[0057] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the glass of the present invention; however, as raw materials and / or equipment for producing glass, there may be certain impurities or components that are not intentionally added, which may be contained in small amounts or trace amounts in the final glass. This situation is also within the scope of protection of the patent of this invention.

[0058] Next, the properties of the glass material of the present invention will be described.

[0059] <300~800nm ​​light transmittance>

[0060] The light transmittance of glass materials below 2mm shall be tested according to the method specified in GB / T 7962.12-2010.

[0061] In some embodiments, the light transmittance of the glass material with a thickness of 2 mm or less at 300 - 800 nm is 2% or less, preferably 1.5% or less, more preferably 1% or less, and further preferably 0.8% or less. The thickness of the above glass material is preferably 0.2 - 2 mm, more preferably 0.5 - 1.8 mm, further preferably 1 - 1.5 mm, and still further preferably 0.2 mm or 0.5 mm or 0.8 mm or 1 mm or 1.5 mm.

[0062] <SCI value>

[0063] The chromaticity is measured using a color difference meter according to the method specified by the International Commission on Illumination (Specular Component Include, abbreviated as SCI in this article).

[0064] In some embodiments, the SCI value of the glass material is 4.0 or less, preferably 3.5 or less, and more preferably 3.0 or less.

[0065] <SCE value>

[0066] The chromaticity is measured using a color difference meter according to the method specified by the International Commission on Illumination (Specular Component Enclude, abbreviated as SCE in this article).

[0067] In some embodiments, the SCE value of the glass material is 5.0 or less, preferably 4.0 or less, and more preferably 3.0 or less.

[0068] <Chromaticity uniformity>

[0069] The sample is processed into a specification of 40 mm × 30 mm × 1.5 mm, and after polishing, it is divided into 15 regions with a specification of 8 mm × 5 mm × 1.5 mm in the length and width directions. The SCE value is measured according to the standard method of SCE, and the SCE value with the largest absolute value is taken and divided by the average value of the SCE values measured 15 times.

[0070] In some embodiments, the chromaticity uniformity of the glass material is 0.7 - 1.3, preferably 0.75 - 1.25, and more preferably 0.8 - 1.2.

[0071] <Stability against water action>

[0072] The stability of the glass material against water action is tested according to the method specified in "GB / T 17129".

[0073] In some embodiments, the leaching percentage of the stability of the glass material against water action is ≤ 0.10%, preferably ≤ 0.06%, and more preferably ≤ 0.03%.

[0074] <Stability against acid action>

[0075] The acid resistance stability of glass materials is tested according to the method specified in GB / T 17129.

[0076] In some embodiments, the acid-resistant stability leaching percentage of the glass material is ≤0.5%, preferably ≤0.35%, and more preferably ≤0.19%.

[0077] <High temperature viscosity>

[0078] The high temperature viscosity of the glass material is tested using a THETA Rheotronic II high temperature viscometer using a rotation method. The value unit is dPaS (poise). The smaller the value, the lower the viscosity.

[0079] In some embodiments, the viscosity of the glass material at 1400° C. is 200 dPas or less, preferably 150 dPas or less, and more preferably 80 dPas or less.

[0080] <Cr 6+ Content>

[0081] Cr in glass materials 6+ The content is tested according to the method specified in IEC62321-7.

[0082] In some embodiments, the Cr of the glass material 6+ The content is 1000 ppm or less, preferably 500 ppm or less, more preferably 100 ppm or less, further preferably 50 ppm or less, and further preferably 10 ppm or less.

[0083] [Manufacturing method]

[0084] The manufacturing method of the glass material of the present invention is as follows: the glass of the present invention can be produced by conventional raw materials and processes, including but not limited to using carbonates, nitrates, phosphates, metaphosphates, pyrophosphates, hydroxides, oxides, etc. as raw materials, and after mixing according to conventional methods, the prepared furnace materials are put into a melting furnace (such as platinum or platinum alloy crucibles, gold or alloy crucibles containing gold) at 1200-1400° C. for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.

[0085] [Glass preforms and glass elements]

[0086] A glass preform can be made from the prepared glass material by means of direct drop molding, grinding, or compression molding such as hot press molding. That is, a glass preform can be made by directly precision drop molding molten glass into a glass precision preform, or by mechanical processing such as grinding and polishing, or by making a preform for compression molding from glass, re-hot press molding the preform, and then grinding the preform to make a glass preform. It should be noted that the means for preparing a glass preform are not limited to the above means.

[0087] As described above, the glass material of the present invention is useful for manufacturing various glass components, among which it is particularly preferred to form a preform from the glass material of the present invention and use the preform to perform re-hot pressing, precision stamping, etc. to make glass components such as lenses, prisms, and sheets.

[0088] In some embodiments, the glass materials described herein can be manufactured into glass elements, including but not limited to sheets, by various processes, including but not limited to slot drawing, float, roll pressing, and other sheet forming processes known in the art. Alternatively, the glass material can be formed by float or roll pressing as known in the art.

[0089] The glass material of the present invention can be used to manufacture glass elements of sheets by grinding or polishing, but the manufacturing of glass elements is not limited to these methods. The glass material of the present invention can be used to manufacture glass elements of various shapes by heat bending or pressing at a certain temperature, but it is not limited to these methods.

[0090] The glass elements of the present invention may have any thickness that is reasonably useful.

[0091] [instrument]

[0092] The glass material of the present invention and the glass element formed by the glass material can be used to make instruments such as photographic equipment, video equipment, projection equipment, display equipment, testing equipment, vehicle-mounted equipment and monitoring equipment.

[0093] The glass material of the present invention can also be applied to transmittance cutoff, black decorative materials, etc.

[0094] <Glass Material Example>

[0095] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided.

[0096] In this embodiment, the manufacturing method of the above-mentioned glass material is used to obtain a glass material having the composition shown in Tables 1 and 2. In addition, the properties of each glass are measured by the testing method described in the present invention, and the measurement results are shown in Tables 1 and 2. In the following Examples 1 to 20, the glass sample with the highest transmittance of 300 to 800 nm is 1.5 mm thick.

[0097] Table 1.

[0098]

[0099]

[0100] Table 2.

[0101]

[0102]

[0103]

[0104] The spectral transmittance curve of the glass material of Example 19 is as follows: Figure 1 shown.

Claims

1. Glass material, It is characterized in that Its components, expressed in weight percentage, contain: SiO 2 :40~68%; B 2 O 3 :1~15%;Al 2 O 3 :0.5~8%; ZnO: 5~20%; Na 2 O: 6~16%; MnO 2 +V 2 O 3 +Fe 2 O 3 +CuO+CeO 2 +NiO+Co 2 O 3 +Cr 2 O 3 :1~18%;TiO 2 :0.5~6%,TiO 2 / (Fe 2 O 3 +CeO 2 ) is 0.2~6.

0.

2. The glass material according to claim 1, It is characterized in that Its components, expressed in weight percentage, also contain: P 2 O 5 :0~2%;and / or ZrO 2 :0~8%;and / or Ln 2 O 3 :0~10%;and / or Li 2 O: 0-5%; and / or K 2 O: 0-8%; and / or RO: 0-10%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, BaO, Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 One or more of the following, the clarifier is Sb 2 O 3 SnO 2 、Na 2 SiF 6 , K 2 SiF 6 One or more of .

3. Glass material, It is characterized in that Its components contain SiO 2 , B 2 O 3 , ZnO and alkali metal oxides, the components of which are expressed in weight percentage, containing MnO 2 +V 2 O 3 +Fe 2 O 3 +CuO+CeO 2 +NiO+Co 2 O 3 +Cr 2 O 3 :1~18%;SiO 2 :40~68%; B 2 O 3 : 1~15%; ZnO: 5~20%; Na 2 O: 6-16%, TiO 2 / (Fe 2 O 3 +CeO 2 ) is 0.2 to 6.0, and the light transmittance of 300 to 800 nm of glass materials below 2 mm is less than 2%.

4. The glass material according to claim 3, It is characterized in that Its components, expressed in weight percentage, contain: Al 2 O 3 :0.5~8%; and / or TiO 2 :0.5~6%;and / or P 2 O 5 :0~2%;and / or ZrO 2 :0~8%;and / or Ln 2 O 3 :0~10%;and / or Li 2 O: 0-5%; and / or K 2 O: 0-8%; and / or RO: 0-10%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, BaO, Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 One or more of the following, the clarifier is Sb 2 O 3 SnO 2 、Na 2 SiF 6 , K 2 SiF 6 One or more of .

5. The glass material according to any one of claims 1 to 4, It is characterized in that Its components are expressed in weight percentage, where: (B 2 O 3 +Al 2 O 3 ) / SiO 2 is less than 0.3; and / or K 2 O / (Na 2 O+Li 2 O) is 0.03 to 1.0; and / or ZnO / SiO 2 0.08 to 0.45; and / or TiO 2 / (Fe 2 O 3 +CeO 2 ) is 0.3 to 4.0; and / or Na 2 O+K 2 O+Li 2 O≤25%; and / or Cr 2 O 3 / (Fe 2 O 3 +CuO) is 3.0 or less.

6. The glass material according to any one of claims 1 to 4, It is characterized in that Its components are expressed in weight percentage, where: (B 2 O 3 +Al 2 O 3 ) / SiO 2 is less than 0.25; and / or K 2 O / (Na 2 O+Li 2 O) is 0.05 to 0.8; and / or ZnO / SiO 2 0.1 to 0.4; and / or TiO 2 / (Fe 2 O 3 +CeO 2 ) is 0.4 to 2.0; and / or Na 2 O+K 2 O+Li 2 O≤23%; and / or Cr 2 O 3 / (Fe 2 O 3 +CuO) is 2.0 or less.

7. The glass material according to any one of claims 1 to 4, It is characterized in that Its components are expressed in weight percentage, where: (B 2 O 3 +Al 2 O 3 ) / SiO 2 0.05~0.2; and / or K 2 O / (Na 2 O+Li 2 O) is 0.1 to 0.5; and / or ZnO / SiO 2 0.12~0.3; and / or Na 2 O+K 2 O+Li 2 O≤20%; and / or Cr 2 O 3 / (Fe 2 O 3 +CuO) is less than 1.

0.

8. The glass material according to any one of claims 1 to 4, It is characterized in that Its components are expressed in weight percentages and contain: SiO 2 : 45 to 68%; and / or B 2 O 3 : 1 to 12%; and / or MnO 2 +V 2 O 3 +Fe 2 O 3 +CuO + CeO 2 +NiO + Co 2 O 3 +Cr 2 O 3 : 2 to 15%; and / or Al 2 O 3 : 0.8 to 7%; and / or ZnO: 7 to 16%; and / or Na 2 O: 7 to 14%; and / or TiO 2 : 0.5 to 5%; and / or P 2 O 5 : 0 to 1%; and / or ZrO 2 : 0 to 6%; and / or Ln 2 O 3 : 0 to 8%; and / or Li 2 O: 0.5 to 4%; and / or K 2 O: 0.5 to 6%; and / or RO: 0 to 8%; and / or clarifying agent: 0 to 0.8%, where RO is one or more of MgO, CaO, SrO, BaO, and Ln 2 O 3 is La 2 O 3 、Gd 2 O 3 、Y 2 O 3 One or more of them, and the clarifying agent is Sb 2 O 3 、SnO 2 、Na 2 SiF 6 、K 2 SiF 6 One or more of them.

9. The glass material according to any one of claims 1 to 4, It is characterized in that Its components, expressed in weight percentage, contain: SiO 2 : 47-65%; and / or B 2 O 3 :2~10%; and / or MnO 2 +V 2 O 3 +Fe 2 O 3 +CuO+CeO 2 +NiO+Co 2 O 3 +Cr 2 O 3 : 3-10%; and / or Al 2 O 3 : 1-5%; and / or ZnO: 8-15%; and / or Na 2 O: 8-13%; and / or TiO 2 :0.5~4%; and / or ZrO 2 :0.5~5%;and / or Ln 2 O 3 :0~4%;and / or Li 2 O: 0.7-3%; and / or K 2 O: 1-6%; and / or RO: 0-6%; and / or clarifier: 0-0.5%, wherein RO is one or more of MgO, CaO, SrO, BaO, Ln 2 O 3 For La 2 O 3 , Gd 2 O 3 , Y 2 O 3 One or more of the following, the clarifier is Sb 2 O 3 SnO 2 、Na 2 SiF 6 , K 2 SiF 6 One or more of .

10. The glass material according to any one of claims 1 to 4, It is characterized in that Its components are expressed in weight percentage, wherein: CuO: 0.5-6%; and / or Fe 2 O 3 :0~3%;and / or MnO 2 :0~3%;and / or V 2 O 3 :0~3%;and / or CeO 2 : 0-2%; and / or NiO: 0.1-5%; and / or Co 2 O 3 :0.1~5%;and / or Cr 2 O 3 :0~4%.

11. The glass material according to any one of claims 1 to 4, It is characterized in that Its components are expressed in weight percentages, where: CuO: 1 to 5%; and / or Fe 2 O 3 : 0.05 to 2%; and / or MnO 2 : 0 to 2%; and / or V 2 O 3 : 0 to 2%; and / or CeO 2 : 0 to 1.5%; and / or NiO: 0.5 to 4%; and / or Co 2 O 3 : 0.5 to 4%; and / or Cr 2 O 3 : 0 to 3.5%.

12. The glass material according to any one of claims 1 to 4, It is characterized in that Its components are expressed in weight percentage, wherein: CuO: 1.5-4%; and / or Fe 2 O 3 :0.1~1.5%; and / or MnO 2 :0~1%;and / or V 2 O 3 :0~1%;and / or CeO 2 : 0-1%; and / or NiO: 0.8-3%; and / or Co 2 O 3 :0.8~3%;and / or Cr 2 O 3 :0~3%.

13. The glass material according to any one of claims 1 to 2, It is characterized in that The light transmittance of glass materials less than 2 mm in the range of 300 to 800 nm is less than 2%.

14. The glass material according to any one of claims 1 to 4, It is characterized in that The light transmittance of glass materials with a diameter of less than 2 mm at 300 to 800 nm is less than 1.5%.

15. The glass material according to any one of claims 1 to 4, It is characterized in that The light transmittance of glass materials less than 2 mm in the range of 300 to 800 nm is less than 1%.

16. The glass material according to any one of claims 1 to 4, It is characterized in that The light transmittance of glass materials with a diameter of less than 2 mm at 300 to 800 nm is less than 0.8%.

17. The glass material according to any one of claims 1 to 4, It is characterized in that The SCI value of the glass material is 4.0 or less; and / or the SCE value of the glass material is 5.0 or less; and / or the chromaticity uniformity of the glass material is 0.7 to 1.3; and / or the water resistance stability leaching percentage of the glass material is ≤0.10%; and / or the acid resistance stability leaching percentage of the glass material is ≤0.5%; and / or the viscosity of the glass material at 1400°C is 200 dPas or less; and / or the Cr ... 6+ The content is less than 1000ppm.

18. The glass material according to any one of claims 1 to 4, It is characterized in that The SCI value of the glass material is 3.5 or less; and / or the SCE value of the glass material is 4.0 or less; and / or the chromaticity uniformity of the glass material is 0.75 to 1.25; and / or the water resistance stability leaching percentage of the glass material is ≤0.06%; and / or the acid resistance stability leaching percentage of the glass material is ≤0.35%; and / or the viscosity of the glass material at 1400°C is 150 dPas or less; and / or the Cr of the glass material is 6+ The content is less than 500ppm.

19. The glass material according to any one of claims 1 to 4, It is characterized in that The SCI value of the glass material is 3.0 or less; and / or the SCE value of the glass material is 3.0 or less; and / or the chromaticity uniformity of the glass material is 0.8 to 1.2; and / or the water resistance stability leaching percentage of the glass material is ≤0.03%; and / or the acid resistance stability leaching percentage of the glass material is ≤0.19%; and / or the viscosity of the glass material at 1400°C is 80 dPas or less; and / or the Cr of the glass material is 6+ The content is less than 100ppm.

20. The glass material according to any one of claims 1 to 4, It is characterized in that Cr in glass materials 6+ The content is less than 50ppm.

21. The glass material according to any one of claims 1 to 4, It is characterized in that Cr in glass materials 6+ The content is less than 10ppm.

22. Glass preforms, It is characterized in that Made of the glass material described in any one of claims 1 to 21.

23. Glass elements, It is characterized in that The glass preform is made of the glass material according to any one of claims 1 to 21 or the glass preform according to claim 22.

24. An instrument, It is characterized in that A glass material comprising the glass material according to any one of claims 1 to 21 and / or a glass element according to claim 23.